A method for improving steel nitriding effect by high temperature ball milling
Patent Information
- Application Number
- CN202310563480.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-18
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2043-05-18
Smart Images

Figure CN116590651B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of nitriding treatment, and in particular relates to a method for improving the nitriding effect of steel by utilizing high-temperature ball milling. Background Art
[0002] Nitriding of steel is also called nitriding. It is a chemical heat treatment process that allows nitrogen atoms to penetrate into the surface of steel to form a hardened layer, which makes steel parts have high hardness, fatigue strength and good wear resistance. At the same time, the hardening layer can still maintain high hardness when heated to a very high temperature, which can give parts working at high temperatures good wear resistance. Therefore, nitriding technology is widely used in various mechanical industries.
[0003] At present, the existing gas nitriding process is time-consuming. For example, it often takes more than 20 hours to obtain a 0.2-0.3 mm thick nitriding layer, and it often takes 20-80 hours to obtain a 0.3-0.5 mm thick nitriding layer. It has low efficiency, high energy consumption, high cost, and serious environmental pollution. Summary of the invention
[0004] The purpose of this section is to summarize some aspects of embodiments of the present invention and briefly introduce some preferred embodiments. Some simplifications or omissions may be made in this section and the specification abstract and the invention title of this application to avoid blurring the purpose of this section, the specification abstract and the invention title, and such simplifications or omissions cannot be used to limit the scope of the present invention.
[0005] In view of the above problems and / or the problems existing in the prior art, the present invention is proposed.
[0006] Therefore, the purpose of the present invention is to overcome the deficiencies in the prior art and provide a method for improving the nitriding effect of steel by utilizing high temperature ball milling.
[0007] In order to solve the above technical problems, the present invention provides the following technical solutions: a method for improving the nitriding effect of steel by high temperature ball milling, comprising:
[0008] Preparation of matrix material: After quenching the workpiece, high temperature tempering treatment is performed to obtain the matrix material;
[0009] High temperature ball milling: put the grinding balls and the base material into the ball mill, and after ball milling at high temperature, wash and dry to obtain the base material after high temperature ball milling;
[0010] Nitriding treatment: The base material after high-temperature ball milling is placed in a nitriding furnace for gas nitriding treatment.
[0011] As a preferred embodiment of the method of the present invention, the workpiece is quenched at a temperature of 840 to 880° C. and a quenching time of 100 to 140 minutes.
[0012] As a preferred embodiment of the method of the present invention, the high temperature tempering treatment comprises a high temperature tempering temperature of 600 to 700° C. and a tempering time of 70 to 110 minutes.
[0013] As a preferred embodiment of the method of the present invention, the grinding balls have a particle size of 3 to 8 mm.
[0014] As a preferred embodiment of the method of the present invention, in the ball milling process, the drum speed during ball milling is 120 to 160 r / min.
[0015] As a preferred embodiment of the method of the present invention, the ball milling treatment is performed at a temperature of 200 to 400° C. and a ball milling treatment time of 120 to 240 minutes.
[0016] As a preferred embodiment of the method of the present invention, the cleaning comprises cleaning with water.
[0017] As a preferred embodiment of the method of the present invention, the nitriding treatment is performed at a temperature of 520 to 580° C. and a time of 100 to 140 minutes.
[0018] As a preferred embodiment of the method of the present invention, the gas nitriding treatment comprises ammonia.
[0019] Beneficial effects of the present invention:
[0020] (1) The present invention provides a method for improving the nitriding effect of steel by using high-temperature ball milling. The workpiece to be nitrided is subjected to ball milling treatment by using high-temperature ball milling. High-temperature ball milling promotes oxidation of the steel surface to produce an oxide film on the surface of the substrate. Appropriately increasing the roughness of the substrate surface will increase the contact area between the substrate and the gas, thereby increasing the adsorption of nitrogen atoms. Defects are formed on the substrate surface, and excess energy exists between the structures, providing more lattice channels for nitrogen atoms to penetrate into the interior of the substrate.
[0021] (2) Compared with the traditional gas nitriding process, the present invention has a higher nitriding efficiency. The energy required for nitrogen atoms to penetrate through the grain boundaries on the substrate surface is lower, the saturation is higher, and energy consumption can be saved, which is suitable for continuous production operations. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative labor. Among them:
[0023] Figure 1 The present invention is a process flow diagram of a method for improving the nitriding effect of steel by utilizing high temperature ball milling.
[0024] Figure 2 This is a microscopic morphology of the workpiece surface after high-temperature ball milling for 120 minutes in an embodiment of the present invention.
[0025] Figure 3 This is a microscopic morphology of the workpiece surface after high-temperature ball milling for 180 minutes in an embodiment of the present invention.
[0026] Figure 4 This is a morphological diagram of the workpiece surface after high-temperature ball milling for 240 minutes in an embodiment of the present invention.
[0027] Figure 5 It is the microstructure diagram of the carburized layer after conventional gas nitriding for 120 minutes in Comparative Example 1 of the present invention.
[0028] Figure 6 This is a microstructure diagram of the nitrided layer after high-temperature ball milling (200° C.) for 120 minutes in an embodiment of the present invention.
[0029] Figure 7 This is a microstructure diagram of the nitrided layer after high-temperature ball milling for 120 minutes in an embodiment of the present invention.
[0030] Figure 8 This is a microstructure diagram of the nitrided layer after high-temperature ball milling for 180 minutes in an embodiment of the present invention.
[0031] Fig. 9 This is a microstructure diagram of the nitrided layer after high-temperature ball milling for 240 minutes in an embodiment of the present invention.
[0032] Fig.10 This is a diagram of the oxide film produced on the base material after high-temperature ball milling (200° C.) in an embodiment of the present invention.
[0033] Fig.11 This is a diagram of the oxide film produced on the base material after high-temperature ball milling in an embodiment of the present invention. DETAILED DESCRIPTION
[0034] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification.
[0035] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.
[0036] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not refer to the same embodiment, nor is it a separate or selective embodiment that is mutually exclusive with other embodiments. The workpieces in the embodiments of the present invention are all 42CrMo steel.
[0037] Example 1
[0038] This embodiment provides a method for improving the nitriding effect of steel by high temperature ball milling. The process flow is as follows: Figure 1 As shown, the specific process steps are as follows:
[0039] (1) Preparation of base material: After quenching, the workpiece is subjected to high temperature tempering treatment. The quenching temperature is 860°C, the quenching time is 120 min, the high temperature tempering temperature is 650°C, and the tempering time is 90 min.
[0040] (2) High-temperature ball milling: Put a 5mm diameter stainless steel ball and the workpiece into a ball mill, set the temperature to 300°C, and perform ball milling. The ball mill drum speed is 140r / min, the ball milling time is 120min, and then the steel workpiece is taken out after ball milling, washed in water, and dried. The surface microstructure of the workpiece is as follows: Figure 2 As shown in Figure 2. After high-temperature ball milling, the surface of the workpiece shows many pits compared to the original workpiece.
[0041] (3) Nitriding treatment: Place the workpiece that has been subjected to high-temperature ball milling treatment into the nitriding furnace, cover the furnace lid and seal it, start the heating element, raise the temperature in the furnace and set it at 550°C. After the heating is completed, introduce nitrogen for 10 minutes (the pressure in the furnace is maintained at 1.3 standard atmospheric pressure) with a flow rate of 3m 3 / h, exhaust the air in the furnace.
[0042] Open the ammonia valve and introduce ammonia at a flow rate of 3m 3 / h, close the nitrogen valve, open the natural gas and ignite the leaked ammonia, keep the workpiece in the ammonia environment for 120 minutes, then close the ammonia valve and introduce nitrogen at a flow rate of 3m 3 / h, turn off the heating elements, turn off the natural gas when the temperature in the furnace drops to 450℃, and open the furnace cover to take out the workpiece when the temperature in the furnace drops below 100℃.
[0043] The nitriding layer structure was observed by scanning electron microscope. The nitriding layer structure obtained by the process of the present invention is as follows: Figure 7 It can be seen that the thickness of the nitrided layer is not changed compared with the nitrided layer thickness obtained by conventional gas nitriding, but the nitrided layer is uniform and dense.
[0044] Example 2
[0045] This embodiment provides a method for improving the nitriding effect of steel by high temperature ball milling. The process flow is as follows: Figure 1 As shown, the specific process steps are as follows:
[0046] (1) Preparation of base material: After quenching, the workpiece is subjected to high temperature tempering treatment. The quenching temperature is 860°C, the quenching time is 120 min, the high temperature tempering temperature is 650°C, and the tempering time is 90 min.
[0047] (2) High-temperature ball milling: Put a 5mm diameter stainless steel ball and the workpiece into a ball mill, set the temperature to 300°C, and perform ball milling. The ball mill drum speed is 140r / min, the ball milling time is 180min, and then the steel workpiece is taken out after ball milling, washed in water, and dried. The surface microstructure of the workpiece is as follows: Figure 3 shown.
[0048] After high-temperature ball milling, the surface of the workpiece shows many pits compared to the original workpiece.
[0049] (3) Nitriding treatment: Place the workpiece that has been subjected to high-temperature ball milling treatment into the nitriding furnace, cover the furnace lid and seal it, start the heating element, raise the temperature in the furnace and set it at 550°C. After the heating is completed, introduce nitrogen for 10 minutes (the pressure in the furnace is maintained at 1.3 standard atmospheric pressure) with a flow rate of 3m 3 / h, exhaust the air in the furnace.
[0050] Open the ammonia valve and introduce ammonia at a flow rate of 3m3 / h. Close the nitrogen valve and open the natural gas at the same time to ignite and burn the overflowed ammonia. Keep the workpiece in the ammonia environment for 120 minutes, then close the ammonia valve and introduce nitrogen at a flow rate of 3m3 / h. 3 / h, turn off the heating elements, turn off the natural gas when the temperature in the furnace drops to 450℃, and open the furnace cover to take out the workpiece when the temperature in the furnace drops below 100℃.
[0051] The nitriding layer structure was observed by scanning electron microscope. The nitriding layer structure obtained by the process of the present invention is as follows: Figure 8 As shown in the figure, it can be seen that the nitriding layer is uniform and dense. The thickness of the nitriding layer is about 0.1mm thicker than that of the nitriding layer obtained by conventional gas nitriding.
[0052] Example 3
[0053] This embodiment provides a method for improving the nitriding effect of steel by high temperature ball milling. The process flow is as follows: Figure 1 As shown, the specific process steps are as follows:
[0054] (1) Preparation of matrix material: After quenching, the workpiece is subjected to high temperature tempering treatment.
[0055] The quenching temperature is 860℃, the quenching time is 120min, the high temperature tempering temperature is 650℃, and the tempering time is 90min.
[0056] (2) High-temperature ball milling: Put a stainless steel ball with a diameter of 5 mm and the workpiece into a ball mill, set the temperature to 300°C, and perform ball milling. The speed of the ball mill drum is 140 r / min, and the ball milling time is 240 min. Then, the steel workpiece after ball milling is taken out, washed in water, and dried.
[0057] The oxide film produced by the base material after high temperature ball milling is shown in Figure 2. Fig.11 It can be seen that high temperature ball milling promotes the oxidation of steel surface and produces an oxide film on the surface of the substrate.
[0058] The obtained workpiece surface microstructure is as follows Figure 4 As shown in Figure 2. After high-temperature ball milling, the surface of the workpiece shows many pits compared to the original workpiece.
[0059] (3) Nitriding treatment: Place the workpiece that has been subjected to high-temperature ball milling treatment into the nitriding furnace, cover the furnace lid and seal it, start the heating element, raise the temperature in the furnace and set it at 550°C. After the heating is completed, introduce nitrogen for 10 minutes (the pressure in the furnace is maintained at 1.3 standard atmospheric pressure) with a flow rate of 3m 3 / h, exhaust the air in the furnace.
[0060] Open the ammonia valve and introduce ammonia at a flow rate of 3m 3 / h, close the nitrogen valve, open the natural gas and ignite the leaked ammonia, keep the workpiece in the ammonia environment for 120 minutes, then close the ammonia valve and introduce nitrogen at a flow rate of 3m 3 / h, turn off the heating elements, turn off the natural gas when the temperature in the furnace drops to 450℃, and open the furnace cover to take out the workpiece when the temperature in the furnace drops below 100℃.
[0061] The nitriding layer structure was observed by scanning electron microscope. The nitriding layer structure obtained by the process of the present invention is as follows: Fig. 9 As shown in the figure, it can be seen that the nitriding layer is uniform and dense. The thickness of the nitriding layer is about 0.2mm thicker than that of the nitriding layer obtained by traditional gas nitriding.
[0062] Example 4
[0063] This embodiment provides a method for improving the nitriding effect of steel by high temperature ball milling. The process flow is as follows: Figure 1 As shown, the specific process steps are as follows:
[0064] (1) Preparation of base material: After quenching, the workpiece is subjected to high temperature tempering treatment. The quenching temperature is 860°C, the quenching time is 120 min, the high temperature tempering temperature is 650°C, and the tempering time is 90 min.
[0065] (2) High-temperature ball milling: Put a 5mm diameter stainless steel ball and the workpiece into a ball mill, set the temperature to 200℃, and perform ball milling. The ball mill drum speed is 140r / min, the ball milling time is 120min, and then the steel workpiece after ball milling is taken out, washed in water, and dried. After high-temperature ball milling, the surface of the workpiece shows many pits compared to the original workpiece. The oxide film produced at 200℃ has poor morphology, which is not conducive to the adsorption of nitrogen atoms. Fig.10 shown.
[0066] (3) Nitriding treatment: Place the workpiece that has been subjected to high-temperature ball milling treatment into the nitriding furnace, cover the furnace lid and seal it, start the heating element, raise the temperature in the furnace and set it at 550°C. After the heating is completed, introduce nitrogen for 10 minutes (the pressure in the furnace is maintained at 1.3 standard atmospheric pressure) with a flow rate of 3m 3 / h, exhaust the air in the furnace.
[0067] Open the ammonia valve and introduce ammonia at a flow rate of 3m 3 / h, close the nitrogen valve, open the natural gas and ignite the leaked ammonia, keep the workpiece in the ammonia environment for 120 minutes, then close the ammonia valve and introduce nitrogen at a flow rate of 3m 3 / h, turn off the heating elements, turn off the natural gas when the temperature in the furnace drops to 450℃, and open the furnace cover to take out the workpiece when the temperature in the furnace drops below 100℃.
[0068] The nitriding layer structure was observed by scanning electron microscope. The nitriding layer structure obtained by the process of the present invention is as follows: Figure 6 It can be seen that the thickness of the nitriding layer is shallower than that of the nitriding layer obtained by traditional gas nitriding, and the structure of the nitriding layer is also uneven.
[0069] Comparative Example 1
[0070] Traditional gas nitriding process:
[0071] Put the workpiece to be nitrided into the nitriding furnace, cover the furnace cover and seal it, start the heating element, raise the temperature in the furnace and set it at 550℃. After the heating is completed, introduce nitrogen for 10 minutes (the pressure in the furnace is maintained at 1.3 standard atmospheric pressure) with a flow rate of 3m 3 / h, exhaust the air in the furnace. Keep the set temperature in the furnace unchanged, open the ammonia inlet to introduce ammonia into the furnace, and at the same time open the natural gas and ignite it. After processing for 120 minutes, close the ammonia inlet, introduce nitrogen into the furnace to replace the gas in the furnace cavity, place the workpiece in the nitrogen atmosphere, turn off the heating element, turn off the natural gas when the temperature in the furnace drops to 450℃, and open the furnace cover to take out the workpiece when the temperature in the furnace drops below 100℃.
[0072] The nitriding layer structure was observed by scanning electron microscopy. The nitriding layer structure obtained by conventional gas nitriding process is as follows: Figure 5 As shown in Figure 2, it can be seen that the nitrided layer obtained by the traditional gas nitriding process has a loose structure, uneven thickness and thinness.
[0073] The present invention provides a method for improving the nitriding effect of steel by high-temperature ball milling. The workpiece to be nitrided is ball milled by high-temperature ball milling. High-temperature ball milling promotes oxidation of the steel surface to produce an oxide film on the surface of the substrate. The roughness of the substrate surface is appropriately increased, which increases the contact area between the substrate and the gas, thereby increasing the adsorption of nitrogen atoms. Defects are formed on the substrate surface, and there is excess energy between the tissues, providing more lattice channels for nitrogen atoms to penetrate into the substrate. Compared with the traditional gas nitriding process, the present invention has a higher nitriding efficiency, and the energy required for nitrogen atoms to penetrate through the grain boundaries on the substrate surface is lower, the saturation is higher, and energy consumption can be saved, which is suitable for continuous production operations.
[0074] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the present invention.
Claims
1. A method for improving the nitriding effect of steel by high temperature ball milling. Features: include, Preparation of matrix material: After quenching the workpiece, high temperature tempering treatment is performed to obtain the matrix material; High temperature ball milling: put the grinding balls and the base material into the ball mill, and after ball milling at high temperature, wash and dry to obtain the base material after high temperature ball milling, wherein the ball milling temperature is 300~400℃, and the ball milling time is 120~240min; Nitriding treatment: The base material after high-temperature ball milling is placed in a nitriding furnace for gas nitriding treatment.
2. The method according to claim 1, Features: The workpiece is quenched at a temperature of 840-880° C. and a quenching time of 100-140 min.
3. The method according to claim 1 or 2, Features: The high temperature tempering treatment, wherein the high temperature tempering temperature is 600-700° C., and the tempering time is 70-110 min.
4. The method according to claim 1, Features: The grinding balls have a particle size of 3 to 8 mm.
5. The method according to claim 1 or 4, Features: The ball milling process comprises the following steps: the roller speed during ball milling is 120-160 r / min.
6. The method according to claim 1, Features: The cleaning includes cleaning with water.
7. The method according to claim 1, Features: The nitriding treatment is carried out at a temperature of 520-580° C. and a time of 100-140 min.
8. The method according to claim 1, Features: The gas nitridation process, wherein the gas includes ammonia.