Positive electrode active material for lithium secondary battery and lithium secondary battery comprising the same

By coating the surface of lithium nickel compounds with a coating material of a specific composition, the problem of structural collapse of positive electrode active materials in lithium secondary batteries during charging and discharging was solved, thereby improving electrochemical stability and cycle life and reducing the rate of increase in resistance.

CN116601797BActive Publication Date: 2026-11-20POSCO HLDG INC +2
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202180085367.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-12-18
Filing Date
2021-11-15
Publication Date
2026-11-20
Estimated Expiration
2041-11-15

AI Technical Summary

Technical Problem

The existing layered high-capacity positive electrode active material LiNiO₂ used in lithium secondary batteries is prone to structural collapse during charge and discharge, has low thermal stability, and is difficult to commercialize.

Method used

The positive electrode active material of a lithium secondary battery uses a lithium nickel compound containing more than 80 mol% Ni as the core, and is coated with a first coating containing one or more elements from Group V and Group VI and S, and a second coating containing B, LiOH, Li₂CO₃ and Li₂SO₄. The ratio of the long axis to the short axis length satisfies 0.1 < (L2/L1) < 1.00.

Benefits of technology

It improves the electrochemical stability of lithium secondary batteries, exhibits excellent cycle life characteristics and a low resistance increase rate, and enhances high-temperature cycling characteristics and initial resistance reduction effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116601797B_ABST
    Figure CN116601797B_ABST
Patent Text Reader

Abstract

The present invention relates to a positive electrode active material for a lithium secondary battery and a lithium secondary battery including the same, the positive electrode active material for a lithium secondary battery including: a core including a lithium-nickel compound having a Ni content of 80 mol% or more; and a coating material located on at least a portion of a surface of the core, the coating material including a first coating material including one or more of a fifth group element and a sixth group element and S, and a second coating material including B, LiOH, Li2CO3, and Li2SO4, the second coating material being a needle-shaped material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a positive electrode active material for lithium secondary batteries and a lithium secondary battery containing the material. Background Technology

[0002] Recently, with the explosive increase in demand for IT mobile devices and low-power drive devices (electric bicycles, small EVs, etc.) and the demand for electric vehicles with a driving range of more than 400km, the world is actively developing secondary batteries with high capacity and high energy density to power these devices.

[0003] To manufacture such high-capacity batteries, high-capacity positive electrode active materials are required. As such high-capacity positive electrode active materials, especially as layered high-capacity positive electrode active materials, LiNiO2 (275mAh / g) has been proposed with the best capacity. However, this active material is prone to structural collapse during charge and discharge, and its thermal stability is low due to oxidation number issues, making it difficult to commercialize.

[0004] Therefore, research on high-capacity positive electrode active materials continues. Summary of the Invention

[0005] Technical issues

[0006] One embodiment provides a positive electrode active material for lithium secondary batteries with excellent electrochemical stability.

[0007] Another implementation provides a lithium secondary battery comprising the positive electrode active material.

[0008] Problem-solving methods

[0009] According to one embodiment, a positive electrode active material for a lithium secondary battery is provided, comprising: a core containing a lithium nickel compound with a Ni content of 80 mol% or more; and a coating material located on at least a portion of the surface of the core, the coating material comprising a first coating and a second coating, the first coating containing one or more of group V and group VI elements and S, the second coating containing B, LiOH, Li2CO3 and Li2SO4, and the second coating being a needle-like material.

[0010] The needle-like material has a long axis and a short axis, and the length ratio of the long axis L1 to the short axis L2 can satisfy the relationship of Equation 1 below.

[0011] [Formula 1]

[0012] 0.1 < (L2 / L1) < 1.00

[0013] The core may include secondary particles, which are granulated from at least one primary particle containing a lithium-nickel compound.

[0014] The lithium-nickel compound can be represented by the following chemical formula 1.

[0015] [Chemical Formula 1]

[0016] Li(Ni 1-(x+y) Co x Mn y X z O2,

[0017] (In the chemical formula, 0 < (x + y) < 0.2, 0 ≤ x ≤ 0.2, 0 ≤ y ≤ 0.2 and 0 ≤ z ≤ 0.2, and X includes at least one of Zr, Al, Ti, B, Mg, Ce, Si, Na and Zn)

[0018] The first coating may be applied to at least a portion of the surface of the primary particles and at least a portion of the surface of the secondary particles. Furthermore, the second coating may be applied to at least a portion of the surface of the secondary particles.

[0019] One or more of the fifth and sixth group elements may be V, Nb, W, or a combination thereof.

[0020] The content of the Group 5 and Group 6 elements, based on the entire positive electrode active material, can be from 10 ppm to 10,000 ppm.

[0021] The content of LiOH, based on the entire positive electrode active material, can be from 100 ppm to 10,000 ppm.

[0022] The content of Li2SO4, based on the entire positive electrode active material, can be from 10 ppm to 3000 ppm.

[0023] According to another embodiment, a lithium secondary battery is provided, comprising: a positive electrode containing the positive electrode active material; a negative electrode containing the negative electrode active material; and a non-aqueous electrolyte.

[0024] Invention Effects

[0025] According to one embodiment, the positive electrode active material for lithium secondary batteries exhibits excellent cycle life characteristics and a low rate of increase in resistance. Attached Figure Description

[0026] Figure 1 This is a diagram schematically illustrating the structure of a lithium secondary battery according to an implementation example.

[0027] Figure 2This is an SEM image of the positive electrode active material prepared according to Example 1.

[0028] Figure 3 It means Figure 2 The images shown are the major and minor axes of the SEM image.

[0029] Figure 4 This is a SEM image of the positive electrode active material prepared according to Comparative Example 1.

[0030] Figure 5 This is a SEM image of the positive electrode active material prepared according to Comparative Example 2.

[0031] Figure 6 This is a SEM image of the positive electrode active material prepared according to Comparative Example 3. Detailed Implementation

[0032] The following is a detailed description of implementation examples of the present invention. However, these implementation examples are provided by way of illustration only, and the present invention is not limited thereto; the present invention is defined only by the scope of the claims.

[0033] In this specification, unless otherwise specified, % means wt%, and 1ppm means 0.0001wt%.

[0034] According to one embodiment, a positive electrode active material for a lithium secondary battery includes: a core containing a lithium nickel compound with a Ni content of 80 mol% or more; and a coating material located on at least a portion of the surface of the core, the coating material comprising a first coating and a second coating, the first coating containing one or more of a group V element and a group VI element and S, and the second coating containing B, LiOH, Li2CO3 and Li2SO4.

[0035] In particular, the second coating may be a needle-like material. This needle-like material has a long axis and a short axis, and the length ratio of the long axis L1 to the short axis L2 can satisfy the relationship of Equation 1 below.

[0036] [Formula 1]

[0037] 0.1 < (L2 / L1) < 1.00

[0038] When the length ratio L2 / L1 of the major axis L1 and minor axis L2 of the needle-like material satisfies Equation 1, it exhibits superior cycle life characteristics and a lower rate of resistance increase. According to one implementation example, the length ratio L2 / L1 of the major axis L1 and minor axis L2 can exceed 0.2 and be less than 0.5.

[0039] If the ratio of the lengths of the major axis L1 and the minor axis L2, L2 / L1, is less than 0.1, the length of the major axis is too large compared to the length of the minor axis, which may contain impurities and thus increase resistance. If the ratio of the lengths of the major axis L1 and the minor axis L2, L2 / L1, is greater than 1.0, this situation is considered to be the case where the lengths of the major axis and the minor axis are the same or the length of the minor axis is greater than the length of the major axis, and therefore it is not suitable.

[0040] Furthermore, according to one embodiment, the positive electrode active material, by including both a first coating and a second coating as coating materials, ensures high capacity, excellent high-temperature cycling characteristics, and reduces initial resistance and resistance increase rate. Regarding the effects achieved by including such coating materials, this effect is obtained when both a first coating and a second coating are included, especially when the second coating is a needle-like material, wherein the first coating includes one or more elements from Group V and Group VI, and S, and the second coating includes B, LiOH, Li₂CO₃, and Li₂SO₄.

[0041] Furthermore, regarding the effects achieved by using this coating material, when a high-nickel lithium-nickel compound with a Ni content of 80 mol% or more is used as the core, for example, a compound represented by the following chemical formula 1, the effect is even more superior. Even in the case of a coating material comprising a first coating and a second coating according to an embodiment, when a lithium-nickel compound with a Ni content of less than 80 mol% is used as the core, or a compound that does not contain nickel is used, the resistance and the rate of increase in resistance are sufficiently low, and therefore the effect achieved by comprising the first coating and the second coating cannot be obtained.

[0042] [Chemical Formula 1]

[0043] Li(Ni 1-(x+y) Co x Mn y X z O2,

[0044] (In the chemical formula, 0 < (x + y) < 0.2, 0 ≤ x ≤ 0.2, 0 ≤ y ≤ 0.2 and 0 ≤ z ≤ 0.2, and X includes at least one of Zr, Al, Ti, B, Mg, Ce, Si, Na and Zn.)

[0045] In one embodiment, X can be Zr or Al. Since Zr ions occupy Li sites, Zr can act as a pillar material and, during charging and discharging, can alleviate the contraction of the lithium ion path, further stabilizing the layered structure. Furthermore, Al can further stabilize the layered structure of the positive electrode active material. Therefore, the lifespan characteristics of the lithium-ion secondary battery can be further improved.

[0046] The core may include secondary particles, which are granulated from at least one primary particle containing the lithium-nickel compound. In this case, the first coating may simultaneously be located on at least a portion of the surface of the primary particle and at least a portion of the surface of the secondary particle, and the second coating may be located only on at least a portion of the surface of the secondary particle. Thus, with the first coating simultaneously located on the surface of both the primary and secondary particles, and the second coating located only on the surface of the secondary particle, a resistance increase rate suppression effect and a lifetime improvement effect can be obtained. This effect cannot be obtained when both the first and second coatings are located only on the surface of the secondary particle because the surface of the primary particle deteriorates. Alternatively, when both the first and second coatings are located on the surface of both the primary and secondary particles, the resistance increase rate suppression effect and lifetime improvement effect according to one embodiment cannot be obtained because of the increased resistance. Moreover, when the first coating is located only on the surface of the secondary particle, and the second coating is located simultaneously on the surface of both the primary and secondary particles, the desired effect cannot be obtained due to the increased resistance.

[0047] In the first coating, one or more of the group 5 and group 6 elements may be V, Nb, W or a combination thereof.

[0048] In the positive electrode active material, the content of the Group V and Group VI elements, based on the entire positive electrode active material, can be from 10 ppm to 10,000 ppm, from 30 ppm to 5,000 ppm, from 80 ppm to 2,000 ppm, or from 300 ppm to 800 ppm. When the content of the Group V and Group VI elements in the positive electrode active material is included within the above range, excellent cycle life characteristics can be exhibited without increasing the rate of increase in resistance.

[0049] The LiOH content, based on the entire positive electrode active material, can range from 100 ppm to 10,000 ppm, more specifically from 500 ppm to 7,000 ppm, and even more specifically from 1,200 ppm to 3,000 ppm. When the LiOH content in the positive electrode active material meets the aforementioned range, it can further improve the excellent initial charge-discharge efficiency and cycle life characteristics.

[0050] The Li2CO3 content, based on the entire positive electrode active material, can be from 1000 ppm to 5000 ppm, more specifically from 1500 ppm to 4000 ppm, and even more specifically from 2000 ppm to 3500 ppm. When the Li2CO3 content meets the above range, it can further improve the excellent room temperature and high temperature life characteristics, and further reduce the resistance increase rate.

[0051] The Li₂SO₄ content, based on the entire positive electrode active material, can range from 10 ppm to 10,000 ppm, more specifically from 80 ppm to 3,000 ppm, further specifically from 100 ppm to 2,000 ppm, further specifically from 100 ppm to 800 ppm, and further specifically from 100 ppm to 400 ppm. When the Li₂SO₄ content meets the above range, excellent capacity characteristics can be well ensured, while further improving cycle life characteristics and further reducing the initial resistance value.

[0052] The content of B, based on the entire positive electrode active material, can be from 300 ppm to 2000 ppm, or from 300 ppm to 1000 ppm. When the content of B meets the above range, excellent capacity characteristics can be well ensured, while further improving cycle life characteristics and further reducing the initial resistance value.

[0053] Another embodiment provides a method for preparing the aforementioned positive electrode active material. The method includes: a step of preparing a first mixture by mixing a precursor compound containing nickel, cobalt, and manganese with a compound containing X (X being at least one of Zr, Al, Ti, B, Mg, Ce, Si, Na, and Zn); a step of preparing a cooling product by subjecting the first mixture to a primary heat treatment and then cooling it; a step of preparing a cleaning product by washing the cooling product with a solution containing a compound containing one or more elements from Group V and Group VI and an S source; a step of forming a second mixture by mixing the cleaning product with LiOH, a boron compound, and Li₂SO₄; and a step of subjecting the second mixture to a secondary heat treatment.

[0054] The preparation method will now be described in further detail.

[0055] First, a first mixture is prepared by mixing a precursor compound containing nickel, cobalt and manganese, a lithium-containing compound and an X-containing compound (X being at least one of Zr, Al, Ti, B, Mg, Ce, Si, Na and Zn).

[0056] The precursor compound containing nickel, cobalt, and manganese can be formed by preparing an aqueous solution of a metal salt by mixing nickel, cobalt, and manganese raw materials in water, followed by a co-precipitation reaction, filtration, and drying. The amounts of nickel, cobalt, and manganese raw materials used can be appropriately adjusted to obtain the final core composition of Formula 1.

[0057] To prevent the oxidation of metal ions, the coprecipitation reaction can be carried out by purging an inert gas, and can be carried out at a temperature of 10°C to 70°C.

[0058] The inactive gas may be N2, argon, or a combination thereof.

[0059] Furthermore, the coprecipitation reaction can be carried out by adding a chelating agent and a pH adjuster to the aqueous solution of the metal salt. The chelating agent may be NH4(OH), but is not limited thereto, and the pH adjuster may be NaOH, but is not limited thereto.

[0060] The drying process can be carried out at 80°C to 200°C for 1 hour to 48 hours.

[0061] The average particle size (D50) of the precursor compound may be from 10 μm to 20 μm, but is not limited thereto. Unless otherwise defined in this specification, the average particle size (D50) means the diameter of particles that constitute 50% of the cumulative volume in the particle size distribution, which can be detected by a particle size analyzer (PSA).

[0062] Lithium hydroxide, lithium carbonate, lithium nitrate, their hydrates, or combinations thereof can be used as the lithium compound.

[0063] The X-containing raw material may be an X-containing oxide, an X-containing nitrate, an X-containing hydroxide, or a combination thereof.

[0064] The mixing ratio of the precursor compound, the lithium compound, and the X-containing raw material can be appropriately adjusted to obtain the core of chemical formula 1.

[0065] Next, the first mixture is subjected to a primary heat treatment and then cooled to prepare a cooled product. This primary heat treatment process can be implemented, for example, by preheating in the range of 300°C to 500°C, then heating to the range of 700°C to 900°C at a heating rate of 1°C / min to 10°C / min, and then holding at that temperature for 1 hour to 48 hours. This primary heat treatment process can be implemented simultaneously by allowing oxygen to flow in at a rate of 100 ml / min to 100,000 ml / min.

[0066] Under the stated temperature conditions, especially when the primary heat treatment process is carried out while oxygen is being introduced, it offers the advantage of improved lifespan. Secondary particles can be formed by granulation of primary particles from the core of Formula 1 through the primary heat treatment process.

[0067] The cooling process can be implemented to room temperature using conventional methods, such as natural cooling.

[0068] A cleaned product is prepared by cleaning the cooled product using a first solution and a second solution, wherein the first solution contains a compound containing one or more elements from Group V and Group VI, and the second solution contains a sulfur source. This process removes residual lithium from the surface of the product. Furthermore, the cooled product can be coated with a solution containing a compound containing one or more elements from Group V and Group VI and a sulfur source. In this case, the first and second solutions can be impregnated within the primary particles.

[0069] The compound containing one or more elements from Group V and Group VI may be ammonium meta-tungstate, ammonium para-tungstate, tungsten oxide, tungsten halide (the halide may be F, Cl, I or a combination thereof), tungsten hexaethoxide, tungsten isopropoxide, tungsten boride, tungsten nitride, tungsten carbonyl or a combination thereof, and the source of sulfur may be ammonium sulfate, Li2SO4, sulfur or a combination thereof.

[0070] In the solution, the solvent may be water, ethanol, propanol, or a combination thereof.

[0071] The solution may contain 0.0001 M to 0.1 M of a compound containing one or more elements from Group V and Group VI, or it may contain 0.001 M to 0.005 M of the compound. Furthermore, the solution may contain 0.01 M to 0.5 M of sulfur (S) source material, or it may contain 0.01 M to 0.2 M of the S source material. When the solution contains the compound containing the aforementioned elements and the S source material within the specified range, it is possible to effectively prepare a positive electrode active material with further improved cycle life characteristics and a lower resistance increase rate while maintaining excellent initial efficiency and initial resistance.

[0072] Next, the cleaning product is mixed with a second coating material to form a second mixture. This mixing process can be carried out using a dry process without solvents. The second coating material may contain boron compounds, LiOH, and Li₂SO₄. That is, the Li₂CO₃ contained in the second coating of the finally obtained positive electrode active material is formed through an internal reaction between the raw materials introduced during the preparation process, rather than through the introduction of additional raw materials.

[0073] The boron compound may be H3BO3, boron oxide, boron nitride, B4C, B2H6, B2F4, B2Cl4, B2Br4, B2I4, or a combination thereof. Regarding the amount of the boron compound used, it may be used in a manner that contains 300 ppm to 2000 ppm of boron based on the entire second coating material, more specifically, 300 ppm to 1000 ppm of boron.

[0074] Based on the entire second coating material, the amount of LiOH used can be from 100 ppm to 1000 ppm, more specifically from 50 ppm to 700 ppm, and even more specifically from 120 ppm to 300 ppm. When the content of LiOH added as the second coating material meets the above range, the gelation phenomenon of the slurry caused by residual lithium is suppressed, thereby enabling the preparation of a slurry that can be coated onto the electrode during the manufacture of the positive electrode.

[0075] Based on the entire second coating material, the Li₂SO₄ content can be from 10 ppm to 500 ppm, more specifically from 10 ppm to 200 ppm, more specifically from 10 ppm to 100 ppm, and even more specifically from 20 ppm to 5 ppm. When the Li₂SO₄ content meets the above range, a Li-BC-SO₄ ionic conductor is formed on the surface, thereby improving the mobility of lithium ions on the surface of the positive electrode active material, thus realizing a lithium secondary battery with excellent lifespan characteristics.

[0076] That is, in one implementation example, the amount of LiOH and Li2SO4 added is less than that of LiOH and Li2SO4 present in the second coating material, which is the final positive electrode active material. It is predicted that this phenomenon is due to the reaction of lithium and metal raw materials present in the lithium oxide during the secondary heat treatment process after mixing with the second coating material.

[0077] Next, the second mixture can be subjected to a second heat treatment. This second heat treatment process can be carried out at a temperature range of 200°C to 450°C, and the heat treatment time can be in the range of 1 hour to 12 hours.

[0078] During the second heat treatment process, compounds containing one or more elements from Group V and Group VI, along with sulfur (S) source material, contained in the first and second solutions, are decomposed, resulting in a first coating material containing one or more elements from Group V and Group VI and S within the positive electrode active material. Furthermore, boron compounds are also decomposed, thus existing as boron (B) within the positive electrode active material. LiOH and Li₂SO₄ remain in their added state, existing as LiOH and Li₂SO₄ within the positive electrode active material. Moreover, through the second heat treatment process, a portion of the LiOH can react with atmospheric CO₂ to form Li₂CO₃, which can then exist within the positive electrode active material.

[0079] The compound containing one or more elements from Group 5 and Group 6, and the sulfur source, being used in solution form, can, as previously described, impregnate between primary particles and also exist on the surface of secondary particles. Therefore, in the final active material, the compound and the sulfur source are present on at least a portion of the surface of the primary particles and at least a portion of the surface of the secondary particles. This further effectively reduces the rate of increase in resistivity.

[0080] Furthermore, the mixing with LiOH, boron compounds, and Li2SO4 is carried out through a dry process, so LiOH, B, and Li2SO4 exist only on the surface of the secondary particles, and Li2CO3 also exists only on the surface of the secondary particles.

[0081] According to another implementation example, a lithium secondary battery including a positive electrode, a negative electrode, and an electrolyte is provided.

[0082] The positive electrode includes a current collector and a layer of positive electrode active material containing a positive electrode active material formed on the current collector. The positive electrode active material includes a positive electrode active material according to one embodiment.

[0083] In the positive electrode, the content of the positive electrode active material can be from 90 wt% to 98 wt% relative to the total weight of the positive electrode active material layer.

[0084] In one implementation, the positive electrode active material layer may further comprise a binder and a conductive material. In this case, the content of the binder and the conductive material, relative to the total weight of the positive electrode active material layer, may be from 1 wt% to 5 wt%.

[0085] The adhesive serves to ensure good adhesion between the positive electrode active material particles and to the current collector. Representative examples of the adhesive include polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polymers containing ethylene oxide, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, acrylated styrene-butadiene rubber, epoxy resin, nylon, etc., but are not limited to these.

[0086] The conductive material is used to impart conductivity to the electrode. Any conductive material that does not cause chemical changes can be used in the constructed electrode. Examples of conductive materials include: carbonaceous materials such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, and carbon fiber; metallic materials such as metal powders or fibers of copper, nickel, aluminum, and silver; conductive polymers such as polyphenylene derivatives; or mixtures of these materials.

[0087] Aluminum foil, nickel foil, or a combination thereof may be used as the current collector, but are not limited thereto.

[0088] For the positive electrode active material layer, the active material composition is prepared by mixing the positive electrode active material, binder, and conductive material (if necessary) in a solvent, and then coating the active material composition onto a current collector to form the positive electrode active material layer. This method of forming the active material layer is well known in the art, and therefore its detailed description is omitted in this specification. N-methylpyrrolidone and the like can be used as the solvent, but the method is not limited to these.

[0089] The negative electrode may include a current collector and a negative electrode active material layer formed on the current collector and containing the negative electrode active material according to an embodiment.

[0090] In the negative electrode active material layer, the content of the negative electrode active material relative to the total weight of the negative electrode active material layer can be from 80 wt% to 98 wt%.

[0091] The negative electrode active material layer may include a binder, and optionally further include a conductive material. In the negative electrode active material layer, the binder content may be 1 wt% to 5 wt% relative to the total weight of the negative electrode active material layer. Furthermore, when further including conductive material, 90 wt% to 98 wt% of the negative electrode active material, 1 wt% to 5 wt% of the binder, and 1 wt% to 5 wt% of the conductive material may be used.

[0092] The negative electrode active material includes a substance capable of reversibly intercalating / deintercalating lithium ions, metallic lithium, an alloy of metallic lithium, a substance capable of doping and dedoping lithium, or a transition metal oxide.

[0093] The substance capable of reversibly intercalating / deintercalating lithium ions is a carbon substance, and any carbon-based negative electrode active material commonly used in lithium ion secondary batteries can be used, and representative examples thereof may use crystalline carbon or amorphous carbon, or both at the same time.

[0094] As the alloy of metallic lithium, an alloy of lithium and a metal selected from Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al and Sn can be used.

[0095] Examples of the substance capable of doping and dedoping lithium include Si, SiO x (0<x<2), Si-Y alloy (the Y is an element selected from alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements, transition metals, rare earth elements and combinations thereof, but not Si), Sn, SnO2, Sn-Y (the Y is an element selected from alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements, transition metals, rare earth elements and combinations thereof, but not Sn), and the like.

[0096] Examples of the transition metal oxide include vanadium oxide, lithium vanadium oxide and the like. The negative electrode active material layer may further include a binder, and may optionally further include a conductive material.

[0097] The binder functions to make the negative electrode active material particles adhere well to each other, and also make the negative electrode active material adhere well to the current collector. As the binder, a non-aqueous binder, an aqueous binder, or a combination thereof can be used.

[0098] Examples of the non-aqueous binder include ethylene propylene copolymer, polyacrylonitrile, polystyrene, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyamideimide, polyimide, or a combination thereof.

[0099] Examples of the aqueous binder include styrene-butadiene rubber, acrylated styrene-butadiene rubber, acrylonitrile-butadiene rubber, acrylic rubber, butyl rubber, fluororubber, ethylene oxide-containing polymer, polyvinylpyrrolidone, polyepichlorohydrin, polyphosphazene, ethylene propylene diene copolymer, polyvinylpyridine, chlorosulfonated polyethylene, latex, polyester resin, acrylic resin, phenolic resin, epoxy resin, polyvinyl alcohol, or a combination thereof.

[0100] When an aqueous binder is used as the negative electrode binder, it may further contain a cellulose compound that imparts viscosity. This cellulose compound may be a mixture of one or more of carboxymethyl cellulose, hydroxypropyl methyl cellulose, methyl cellulose, or their alkali metal salts. The alkali metal may be Na, K, or Li. The amount of this tackifier used may be from 0.1 parts by weight to 3 parts by weight relative to 100 parts by weight of the negative electrode active material.

[0101] The conductive material is used to impart conductivity to the electrode. Any conductive material that does not cause chemical changes can be used in the constructed electrode. Examples of conductive materials include: carbonaceous materials such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, and carbon fiber; metallic materials such as metal powders or fibers of copper, nickel, aluminum, and silver; conductive polymers such as polyphenylene derivatives; or mixtures of these materials.

[0102] The current collector may be selected from copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, polymer substrate coated with conductive metal, and combinations thereof.

[0103] For the negative electrode, an active material composition is prepared by mixing the negative electrode active material, a binder, and, if necessary, a conductive material in a solvent, and then coating the active material composition onto a current collector to form the negative electrode. Water can be used as the solvent.

[0104] This method of forming the negative electrode is well known in the art, and therefore its detailed description is omitted in this specification.

[0105] The electrolyte includes a non-aqueous organic solvent and a lithium salt.

[0106] The non-aqueous organic solvent acts as a medium for the movement of ions that can participate in the electrochemical reactions of the battery.

[0107] The non-aqueous organic solvents mentioned above can be carbonates, esters, ethers, ketones, alcohols, or aprotic solvents.

[0108] Dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), methyl ethyl carbonate (MEC), ethylene carbonate (EC), propylene carbonate (PC), and butyl carbonate (BC) can be used as carbonate solvents. Methyl acetate, ethyl acetate, n-propyl acetate, dimethyl acetate, methyl propionate, ethyl propionate, propyl propionate, decanolide, mevalonolactone, and caprolactone can be used as ester solvents. Dibutyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, dimethoxyethane, 2-methyltetrahydrofuran, and tetrahydrofuran can be used as ether solvents. Furthermore, cyclohexanone and other ketone solvents can be used. In addition, ethanol, isopropanol, etc. can be used as the alcohol solvent, and nitriles such as R-CN (R is a hydrocarbon group with a straight chain, branched chain or cyclic structure having 2 to 20 carbon atoms, and may include double bonds, aromatic rings or ether bonds, etc.) and amides such as dimethylformamide, dioxolane such as 1,3-dioxolane, sulfolane, etc. can be used as the aprotic solvent.

[0109] The non-aqueous organic solvent can be used alone or in combination of two or more. The mixing ratio when using two or more solvents can be adjusted appropriately according to the desired battery performance, which will be widely understood by those skilled in the art.

[0110] Furthermore, in the case of the carbonate solvent, it is preferable to use a mixture of cyclic and chain carbonates. In this case, when the cyclic and chain carbonates are mixed in a volume ratio of 1:1 to 1:9, the electrolyte exhibits excellent performance.

[0111] When using the non-aqueous organic solvent, a mixed solvent of cyclic carbonates and chain carbonates, a mixed solvent of cyclic carbonates and propionate solvents, or a mixed solvent of cyclic carbonates, chain carbonates, and propionate solvents can be used. Methyl propionate, ethyl propionate, propyl propionate, or combinations thereof can be used as the propionate solvent.

[0112] In this case, when used in combination with cyclic carbonates and chain carbonates, or with cyclic carbonates and propionate solvents, the electrolyte exhibits excellent performance when mixed at a volume ratio of 1:1 to 1:9. Furthermore, when used in combination with cyclic carbonates, chain carbonates, and propionate solvents, a volume ratio of 1:1:1 to 3:3:4 can be achieved. Of course, the mixing ratio of the solvents can be appropriately adjusted according to the desired characteristics.

[0113] The non-aqueous organic solvent may further comprise an aromatic hydrocarbon organic solvent in the carbonate solvent. In this case, the carbonate solvent and the aromatic hydrocarbon organic solvent can be mixed in a volume ratio of 1:1 to 30:1.

[0114] Aromatic hydrocarbon compounds of the following chemical formula 2 can be used as the aromatic hydrocarbon organic solvent.

[0115] [Chemical Formula 2]

[0116]

[0117] (In the stated chemical formula 2, R1 to R6 may be the same as or different from each other, and are selected from hydrogen, halogens, alkyl groups having 1 to 10 carbon atoms, haloalkyl groups, and combinations thereof.)

[0118] Specific examples of the aromatic hydrocarbon organic solvents are selected from benzene, fluorobenzene, 1,2-difluorobenzene, 1,3-difluorobenzene, 1,4-difluorobenzene, 1,2,3-trifluorobenzene, 1,2,4-trifluorobenzene, chlorobenzene, 1,2-dichlorobenzene, 1,3-dichlorobenzene, 1,4-dichlorobenzene, 1,2,3-trichlorobenzene, 1,2,4-trichlorobenzene, iodobenzene, 1,2-diiodobenzene, 1,3-diiodobenzene, 1,4-diiodobenzene, 1,2,3-triiodobenzene, 1,2,4-triiodobenzene, toluene, and others. Fluorotoluene, 2,3-difluorotoluene, 2,4-difluorotoluene, 2,5-difluorotoluene, 2,3,4-trifluorotoluene, 2,3,5-trifluorotoluene, chlorotoluene, 2,3-dichlorotoluene, 2,4-dichlorotoluene, 2,5-dichlorotoluene, 2,3,4-trichlorotoluene, 2,3,5-trichlorotoluene, iodotoluene, 2,3-diiodotoluene, 2,4-diiodotoluene, 2,5-diiodotoluene, 2,3,4-triiodotoluene, 2,3,5-triiodotoluene, xylene and combinations thereof.

[0119] To improve battery life, the electrolyte may further contain vinylene carbonate or a compound of the following chemical formula 3 as an additive to improve life.

[0120] [Chemical Formula 3]

[0121]

[0122] (In the chemical formula 3, R7 and R8 may be the same as or different from each other, and are selected from hydrogen, halogen, cyano (CN), nitro (NO2) and fluorinated alkyl groups having 1 to 5 carbon atoms. At least one of R7 and R8 is selected from halogen, cyano (CN), nitro (NO2) and fluorinated alkyl groups having 1 to 5 carbon atoms, but R7 and R8 are not both hydrogen.)

[0123] Representative examples of the aforementioned ethylene carbonate compounds include difluoroethylene carbonate, chloroethylene carbonate, dichloroethylene carbonate, bromoethylene carbonate, dibromoethylene carbonate, nitroethylene carbonate, cyanoethylene carbonate, or fluoroethylene carbonate. When further using this life-enhancing additive, its dosage can be appropriately adjusted.

[0124] The electrolyte may further comprise vinyl ethylene carbonate, propanesulfonate lactone, succinic acid, or a combination thereof, in which case the amount used may be adjusted appropriately.

[0125] The lithium salt is dissolved in an organic solvent and acts as a lithium-ion supply source within the battery, thereby enabling the basic operation of a lithium secondary battery. It is a substance that promotes the movement of lithium ions between the positive and negative electrodes. Representative examples of such lithium salts are selected from LiPF6, LiBF4, LiSbF6, LiAsF6, LiN(SO2C2F5)2, Li(CF3SO2)2N, LiN(SO3C2F5)2, LiC4F9SO3, LiClO4, LiAlO2, LiAlCl4, and LiN(C x F 2x+1 SO2)(C y F 2y+1 SO2 (where x and y are natural numbers, for example, integers from 1 to 20), LiCl, LiI, and LiB(C2O4)2 (lithium bis(oxalato)borate: LiBOB) are included as supporting electrolytes. The concentration of the lithium salt used is preferably in the range of 0.1 M to 2.0 M. When the concentration of the lithium salt falls within this range, the electrolyte has suitable conductivity and viscosity, thus exhibiting excellent performance and enabling efficient movement of lithium ions.

[0126] Depending on the type of lithium-ion secondary battery, a separator may be present between the positive and negative electrodes. Such a separator can be made of polyethylene, polypropylene, polyvinylidene fluoride, or multilayer membranes of two or more layers thereof. Of course, mixed multilayer membranes such as polyethylene / polypropylene two-layer membranes, polyethylene / polypropylene / polyethylene three-layer membranes, and polypropylene / polyethylene / polypropylene three-layer membranes can also be used.

[0127] exist Figure 1 The figure shows an exploded perspective view of a lithium secondary battery according to an embodiment of the present invention. Although an example of a lithium secondary battery with a triangular shape is described, the present invention is not limited thereto and can be applied to batteries of various shapes such as cylindrical or pouch-shaped.

[0128] Reference Figure 1One embodiment of the lithium secondary battery 100 may include an electrode assembly 40 and a housing 50. The electrode assembly 40 is formed by winding a separator 30 between a positive electrode 10 and a negative electrode 20. The electrode assembly 40 is disposed within the housing 50. The positive electrode 10, the negative electrode 20, and the separator 30 may be immersed in an electrolyte (not shown).

[0129] Detailed Description of the Embodiments

[0130] The following describes embodiments and comparative examples of the present invention. These embodiments are merely one example of the present invention, and the present invention is not limited to these embodiments.

[0131] Preparation Example 1 - Preparation of Positive Electrode Active Material Precursor

[0132] NiSO4·6H2O was used as the raw material for nickel, CoSO4·7H2O was used as the raw material for cobalt, and MnSO4·H2O was used as the raw material for manganese. These raw materials were dissolved in distilled water to prepare an aqueous solution of metal salts.

[0133] The metal salt aqueous solution is purged with N2 using a coprecipitation reactor, wherein NH4(OH) is added to the coprecipitation reactor as a chelating agent while the reactor temperature is maintained at 50°C, and NaOH is used to adjust the pH, thereby implementing the coprecipitation process.

[0134] The precipitate obtained by the co-precipitation process was filtered, washed with distilled water, and then dried in an oven at 100°C for 24 hours to prepare (Ni) particles with an average particle size of 14.8 μm. 0.88 Co 0.05 Mn 0.07 (OH)2 is a precursor of positive electrode active material.

[0135] Comparative Example 1 - Preparation of Ni 85% positive electrode active material

[0136] Based on 1 mol of the positive electrode active material precursor prepared in Preparation Example 1, 1.05 mol of LiOH·H2O (Samchun Chemical Co., Ltd., battery grade) and the X-containing compound were uniformly mixed to prepare a first mixture. ZrO2 (Aldrich, 3N) and Al(OH)3 (Aldrich, 4N) were used as the X-containing compound. The amount of the X-containing compound used was determined to achieve the desired compound composition.

[0137] After the first mixture was loaded into a tube furnace, a primary heat treatment was performed while oxygen was introduced at a rate of 200 mL / min. The primary heat treatment process consisted of a five-hour preheating at 480°C, followed by heating to 760°C at a rate of 5°C / min and holding at that temperature for 16 hours. The product was then allowed to cool naturally to 25°C to prepare LiNi. 0.85 Co 0.09 Mn 0.06 Zr 0.0037 Al 0.0001 The cooling product represented by O2 is the positive electrode active material. The cooling product is formed into secondary particles by granulation of primary particles.

[0138] Comparative Example 2 - Preparation of Ni 85% positive electrode active material containing 2500 ppm LiOH and 2000 ppm Li2CO3

[0139] The cooled product prepared in Comparative Example 1 was washed with distilled water, filtered, and dried.

[0140] The obtained dried product was subjected to a second heat treatment at 280°C for five hours to prepare a positive electrode active material. The positive electrode active material includes a core and a coating layer formed on the surface of the core. The core comprises a material composed of LiNi... 0.85 Co 0.09 Mn 0.06 Zr 0.0037 Al 0.0001 O2 represents secondary particles formed by granulation of primary particles, and the coating layer contains 2500 ppm LiOH and 2000 ppm Li2CO3.

[0141] Comparative Example 3 - Ni 85% positive electrode active material containing 200 ppm W, 2500 ppm LiOH and 2000 ppm Li2CO3

[0142] The cooling product prepared in Comparative Example 1 was subjected to a water washing process using an aqueous solution of distilled water containing 0.0004M ammonium meta-tungstate (AMT), followed by filtration and drying.

[0143] The obtained dried product was subjected to a second heat treatment at 280°C for five hours to prepare a positive electrode active material. The positive electrode active material includes a core and a coating layer formed on the surface of the core. The core comprises a material composed of LiNi... 0.85 Co 0.09 Mn 0.06 Zr 0.0037 Al 0.0001O2 represents secondary particles formed by granulation of primary particles, and the coating layer contains 2500 ppm LiOH, 2000 ppm Li2CO3, 500 ppm B and 300 ppm Li2SO4.

[0144] Example 1 - Ni 85% positive electrode active material containing 200 ppm W, 2500 ppm LiOH, 2000 ppm Li2CO3, 500 ppm B and 500 ppm Li2SO4

[0145] The cooling product prepared in Comparative Example 1 was washed with an aqueous solution of distilled water containing 0.0004 M AMT (ammonium meta-tungstate) and 0.04 M ammonium sulfate (AS), then filtered and dried.

[0146] The obtained dried product was dry-mixed with 500 ppm LiOH, 500 ppm H3BO3, and 30 ppm Li2SO4, and then subjected to a second heat treatment at 280°C for five hours to prepare a positive electrode active material. The prepared positive electrode active material includes a core and a coating material on the surface of the core, wherein the core comprises a coating material made of LiNi... 0.85 Co 0.09 Mn 0.06 Zr 0.0037 Al 0.0001 O2 represents secondary particles formed by granulation of primary particles, and the positive electrode active material contains W and S on the surface of the primary particles and W, S, LiOH, Li2CO3, B and Li2SO4 on the surface of the secondary particles. At this time, the content of W is 200ppm, the content of LiOH is 2500ppm, the content of Li2CO3 is 2000ppm, the content of B is 500ppm, and the content of Li2SO4 is 500ppm.

[0147] The AMT and AS contents used in Example 1 and Comparative Examples 1 to 3, as well as the contents of W, S and Li2SO4 contained in the active substance, are summarized and shown in Table 1 below.

[0148] [Table 1]

[0149]

[0150] (Preparation Example 2) Preparation of Half-Cell

[0151] A positive electrode active material slurry was prepared by mixing the positive electrode active material, acetylene black conductive material, and polyvinylidene fluoride adhesive (product name: KF1100) prepared according to Example 1 and Comparative Examples 1 to 3 at a weight ratio of 92.5:3.5:4, and adding the mixture to an N-methyl-2-pyrrolidone solvent in such a way that the solid content is about 30 wt%.

[0152] The slurry was coated onto the positive current collector, i.e., aluminum foil (15 μm thick), using a doctor blade, and then rolled after drying to prepare the positive electrode. The loading of the positive electrode was 14.6 mg / cm³. 2 The rolling density is 3.1 g / cm³. 3 .

[0153] A 2032 coin-type half-cell was prepared using the aforementioned positive electrode, a lithium metal anode (200 μm thick, Honzo metal), an electrolyte, and a polypropylene separator via conventional methods. The electrolyte was prepared by dissolving 1 M LiPF6 in a mixed solvent consisting of ethylene carbonate (EC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC) in a volume ratio of EC:DMC:EMC = 3:4:3, and adding 1.5 wt% ethylene carbonate relative to 100 wt% of the total product.

[0154] Experiment Example 1: SEM Evaluation

[0155] SEM images of the positive electrodes prepared using the positive electrode active materials prepared in Example 1 and Comparative Examples 1 to 3 were examined, and the results are presented in [the table]. Figures 2 to 5 middle( Figure 2 and Figure 3 Example 1, Figure 4 Compare with Example 1. Figure 5 Compare with Example 2. Figure 5 (Comparative Example 3).

[0156] It can be seen that, as Figure 4 As shown, the surface of the positive electrode active material in Comparative Example 1, which did not undergo a water washing process, is uneven; conversely, as shown... Figure 5 As shown, the surface of the positive electrode active material in Comparative Example 2, which underwent a water washing process, is smooth. Furthermore, it can be seen that... Figure 6 As shown, the positive electrode active material of Comparative Example 3, which contains only the first coating, does not have needle-like coatings on its surface.

[0157] Conversely, it is evident that the positive electrode active material of Example 1, which includes the first coating and the second coating, is as follows: Figure 2As shown, needle-like substances exist on the surface. Furthermore, from... Figure 2 SEM images, showing the major and minor axes. Figure 3 The result of calculating the ratio of the major axis to the minor axis (average ratio) is 0.27.

[0158] Experimental Example 2: Evaluation of charge / discharge capacity, initial efficiency, and initial resistance at room temperature (25℃)

[0159] The prepared coin-shaped half-cells were aged at room temperature (25°C) for 10 hours before being charged and discharged.

[0160] For charge and discharge, a 0.1C charge and a 0.1C discharge were performed under constant current / constant voltage conditions from 2.5V to 4.25V and a 1 / 20C cutoff point. The charge and discharge capacities were calculated and the results are shown in Table 1 below. Furthermore, the ratio of discharge capacity to charge capacity was calculated and the result is shown as the efficiency in Table 2 below. The baseline capacity for capacity evaluation was 215 mAh / g.

[0161] For the initial resistor, it was fully charged at 0.2C (charge rate: 100%) to 4.25V and then discharged at 0.2C. Simultaneously, the voltage value after 60 seconds was measured and calculated, along with the change in voltage value relative to the applied current, i.e., the voltage variation over 60 seconds. The results are shown in Table 2 below.

[0162] Experimental Example 3: Evaluation of High-Temperature (45℃) Cyclic Life and Resistance Increase Rate

[0163] The prepared coin-shaped half-cell was subjected to 30 cycles of 0.3C charging and 0.3C discharging at 45°C under constant current / constant voltage conditions from 2.5V to 4.25V and at a 1 / 20C cutoff point. The ratio of the discharge capacity per cycle to the discharge capacity after 30 cycles was calculated, and the results are presented as the cycle life characteristics in Table 3 below.

[0164] Furthermore, regarding the rate of increase in resistance, the resistance was calculated by fully charging at 0.2C (charge rate: 100%) to 4.25V and then discharging at 0.2C at high temperature (45°C), and measuring the voltage change over 60 seconds. This process was repeated 30 times, and the voltage change over 60 seconds was then measured to calculate the resistance over 30 cycles. The results are shown in Table 3 below. Additionally, the ratio of the resistance over 30 cycles to the resistance over 1 cycle was calculated, and the results are also shown in Table 3 below.

[0165] [Table 2]

[0166]

[0167] [Table 3]

[0168]

[0169] As shown in Tables 2 and 3 above, the half-cell using the positive electrode active material of Example 1 maintains a low initial resistance, excellent primary efficiency, and high-temperature cycle life while exhibiting a low rate of increase in high-temperature resistance. Conversely, it can be seen that the positive electrode active materials of Comparative Examples 1 to 3 exhibit lower primary efficiency and a very high rate of increase in resistance.

[0170] This invention is not limited to the embodiments described above, but can be implemented in many different forms. Those skilled in the art will understand that this invention can be implemented in other specific forms without altering its technical concept and essential technical features. Therefore, it should be understood that the above embodiments are illustrative in all respects and not limiting.

Claims

1. A positive electrode active material for lithium secondary batteries, comprising: The core contains lithium-nickel compounds with a Ni content of over 80 mol%; and A coating material is located on at least a portion of the surface of the core. The coating material comprises a first coating and a second coating, wherein the first coating comprises one or more elements from Group V and Group VI, and sulfur (S), and the second coating comprises boron (B), liOH, li₂CO₃, and li₂SO₄. The second coating is a needle-like substance. The core of the positive electrode active material comprises secondary particles granulated from at least one primary particle containing the lithium-nickel compound. The first coating is located on at least a portion of the surface of the primary particles and at least a portion of the surface of the secondary particles, and The second coating is located on at least a portion of the surface of the secondary particles.

2. The positive electrode active material for lithium secondary batteries according to claim 1, wherein, The needle-like substance has a long axis and a short axis, and the length ratio of the long axis L1 to the short axis L2 satisfies the relationship of Equation 1 below. [Formula 1] 0.1 < (L2 / L1) < 1.

00.

3. The positive electrode active material for lithium secondary batteries according to claim 1, wherein, The lithium-nickel compound is represented by the following chemical formula 1. [Chemical Formula 1] Li (Ni 1-(x+y) Co x Mr y X z )O2, In the chemical formula, 0 < (x + y) < 0.2, 0 ≤ x ≤ 0.2, 0 ≤ y ≤ 0.2, and 0 ≤ z ≤ 0.

2. X includes at least one of Zr, Al, Ti, B, Mg, Ce, Si, Na, and Zn.

4. The positive electrode active material for lithium secondary batteries according to claim 1, wherein, One or more of the fifth and sixth group elements are V, Nb, W, or combinations thereof.

5. The positive electrode active material for lithium secondary batteries according to claim 1, wherein, The content of the Group 5 and Group 6 elements is 10 ppm to 10,000 ppm based on the entire positive electrode active material.

6. The positive electrode active material for lithium secondary batteries according to claim 1, wherein, The content of LiOH is between 100 ppm and 10,000 ppm based on the total amount of the positive electrode active material.

7. The positive electrode active material for lithium secondary batteries according to claim 1, wherein, The content of Li2SO4 is between 10 ppm and 3000 ppm based on the total positive electrode active material.

8. A lithium secondary battery, comprising: A positive electrode comprising the positive electrode active material according to any one of claims 1 to 7; negative electrode; and Non-aqueous electrolyte.

Citation Information

Patent Citations

  • Positive electrode active material for nonaqueous electrolytic secondary battery

    JP2014197540A

  • Positive active material for rechargeable lithium battery, method of preparing the same, and rechargeable lithium battery including the same