A method for improving the LPCVD pass rate of TOPcon cells
By using micro-negative pressure conditions and oxygen stew operation in the TOPcon battery LPCVD process, the problem of hot air flow caused by high-temperature oxygenation is solved, the quality and conversion efficiency of the tunnel oxide layer are improved, and the through rate and overall performance of the battery are improved.
Patent Information
- Application Number
- CN202310677446.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-09
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2043-06-09
AI Technical Summary
In the TOPcon battery LPCVD process, high temperature and normal pressure oxygenation cause the hot air flow to impact the furnace door, damaging the sealing ring, causing gas leakage and deterioration of deposition quality, affecting the battery conversion efficiency and throughput rate.
Micro-negative pressure conditions (300~700torr) are used to deposit the tunnel oxide layer to avoid hot air flow impact and damage to the sealing ring, ensure stable air pressure in the reaction chamber, and control the oxidation reaction through oxygen stewing operation to form a high-quality tunnel oxide layer.
It improves the quality and conversion efficiency of the tunnel oxide layer, reduces the rework rate and production cost, and enhances the through rate and overall performance of the LPCVD process.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of photovoltaic cell manufacturing, and in particular to a method for improving the LPCVD pass rate of a TOPcon cell. Background Art
[0002] As TOPcon cells have replaced PERC cells with overwhelming conversion efficiency, the entire photovoltaic industry has gradually shifted towards TOPcon cells. However, high-efficiency cells also have very high cost requirements, especially because of the machine cost and yield loss caused by high temperature, as well as the complexity of its production process. The high yield loss and product rework rate caused by the complex and cumbersome process have gradually become the difficulties of TOPcon high-efficiency cells.
[0003] The LPCVD section in the TOPcon battery production process has a high rework rate due to many unfavorable factors such as high temperature, vacuum, and special gases, which indirectly affects the effective promotion of TOPcon products.
[0004] The LPCVD process mainly provides a tunneling oxide layer and an amorphous silicon thin layer for the battery. The tunneling oxide layer allows majority electrons to tunnel into the polysilicon layer while blocking the recombination of minority holes. Then, the electrons are transported laterally in the polysilicon layer and collected by the metal, which greatly reduces the metal contact recombination current and improves the open circuit voltage and short circuit current of the battery. During the preparation process, dry oxygen is used to oxidize the surface of the silicon wafer at high temperature to form an oxide layer, and then silane is introduced under low pressure to form an amorphous silicon thin layer.
[0005] In the above-mentioned process of preparing the tunneling oxide layer and the amorphous silicon thin layer by the LPCVD process, when preparing the tunneling oxide layer in the first step, it is necessary to first evacuate the furnace tube to a negative pressure, preheat, and then continuously introduce a large amount of oxygen to oxidize the silicon wafer. In the traditional process, there is no pressure effect during the oxygen passing process. Continuous oxygen passing will cause the pressure in the reaction chamber to gradually return to normal pressure. The deposition of the tunneling oxide layer is completed during the oxygen passing process, and then the furnace tube is evacuated to a negative pressure condition to carry out the second step of preparing the amorphous silicon thin layer.
[0006] This process has at least the following defects: (1) During the deposition of the tunnel oxide layer, the gas pressure in the reactor tube is at normal pressure. Since the reaction is carried out under high temperature conditions, a large amount of hot air flow will be generated. The hot air flow will impact the furnace door of the reactor tube under normal pressure conditions, causing the furnace door to be baked for a long time, resulting in deformation of the furnace door. In severe cases, it may even damage the sealing ring of the furnace door, destroying the sealing of the furnace door, causing gas leakage in the reaction chamber or air outside the furnace tube to mix into the reaction chamber, affecting the deposition quality of the tunnel oxide layer and the amorphous silicon thin layer, thereby affecting the conversion efficiency of the TOPcon battery. (2) From the perspective of production process, the damage to the sealing of the furnace tube will cause the furnace tube to be evacuated to negative pressure for a short time during the subsequent low-pressure deposition of the amorphous silicon thin layer, resulting in the complete rework of the entire tube battery cell, which affects the direct pass rate of the battery cell in the LPCVD process. Summary of the invention
[0007] In view of the shortcomings of the prior art described above, an object of the present invention is to provide a method for improving the direct pass rate of LPCVD of TOPcon cells, so as to solve the problem that the reaction furnace tube is at normal pressure during the continuous oxygen flow to prepare the tunneling oxide layer in the existing TOPcon cell LPCVD process, resulting in the hot air flow impacting and damaging the furnace door, causing the reaction gas to leak or mix with air, affecting the deposition quality of the tunneling oxide layer and the amorphous silicon thin layer, and causing the subsequent vacuum to be unable to be evacuated for a short time to negative pressure, resulting in the complete rework of the entire tube battery cell, affecting the direct pass rate of the LPCVD process battery cell.
[0008] To achieve the above-mentioned object and other related objects, the present invention provides a method for improving the LPCVD pass rate of a TOPcon cell, wherein a tunneling oxide layer is deposited on the surface of a silicon wafer using an LPCVD process under a slightly negative pressure condition; the slightly negative pressure condition is 300~700 torr, such as 300~400 torr, 400~450 torr, 450~550 torr, 550~600 torr, 600~700 torr.
[0009] Traditional LPCVD requires a large amount of oxygen to prepare the tunnel oxide layer. Oxygen causes the pressure in the reaction chamber to rise to normal pressure. The sealing ring at the sealed furnace door of the furnace tube is affected by the heat flow and has a probability of burning. If burned, it cannot be evacuated to a low pressure state in the subsequent process. It will also cause the reaction gas to leak or mix with air, affecting the deposition quality of the tunnel oxide layer and the amorphous silicon thin layer, thereby affecting the conversion efficiency of the TOPcon battery, resulting in process termination and rework, and reducing the pass rate.
[0010] The present application creatively adopts a micro-negative pressure deposition tunneling oxide layer process, so that during the entire reaction process of the LPCVD process, the pressure of the reaction chamber is kept below the atmospheric pressure, the air pressure will not gradually return to normal pressure, and a large amount of hot air flow will not be generated. There is no hot air flow passing through the furnace door and the sealing ring, which can avoid the impact and damage of the hot air flow on the furnace door, and avoid the furnace door being deformed or the sealing ring being burned by the heat flow, thereby ensuring the sealing of the furnace tube during the reaction process, and the subsequent vacuum to low pressure process in the deposition of the amorphous silicon layer remains stable, reducing the rework rate, and at the same time ensuring the stability of the air pressure and oxygen concentration in the reaction chamber, thereby improving the quality and preparation efficiency of the tunneling oxide layer, thereby improving the LPCVD pass rate in the TOPcon battery and the overall performance of the TOPcon battery.
[0011] Preferably, the method comprises the following steps:
[0012] 1) Place a silicon wafer in the reaction chamber, evacuate to a first low pressure condition under a sealed condition, heat to a first preset temperature, introduce oxygen to a slightly negative pressure condition, and stop introducing oxygen;
[0013] 2) Under the above-mentioned slightly negative pressure and first preset temperature conditions, oxygen is oxidized to deposit a tunnel oxide layer on the surface of the silicon wafer.
[0014] The conversion efficiency of TOPCon cells mainly depends on the quality and stability of the tunneling oxide layer. The tunneling oxide layer is a key part of the PN junction of the cell, and its thickness and quality have a very important influence on the performance and conversion efficiency of the cell. Therefore, preparing a high-quality and stable tunneling oxide layer is the key to improving the conversion efficiency of TOPCon cells.
[0015] In the above technical solution of the present application, by controlling the time of oxygen introduction in the process of depositing the tunneling oxide layer, the oxygen introduction is stopped when the normal pressure state is not reached, so that the reaction system maintains a slightly negative pressure condition, and the oxidation reaction is carried out by heating the oxygen in the reaction chamber, and the oxygen suffocation process is added to form a tunneling oxide layer. The present application creatively adopts the method of passing oxygen to a slightly negative pressure, stopping the oxygen introduction, and performing the oxygen suffocation operation to avoid problems such as excessive oxygen concentration or high temperature, which may lead to excessive oxidation reaction, silicon wafer surface contamination, or silicon wafer surface damage. This method can ensure the stability of the air pressure in the reaction chamber, so that the oxidation reaction is carried out under relatively stable conditions, thereby improving the quality and stability of the tunneling oxide layer, thereby improving the conversion efficiency of the TOPcon battery. From the perspective of production technology, at the same time, since the air pressure will not gradually return to normal pressure, a large amount of hot air flow will not be generated, and there is no hot air flow passing through the furnace door and the sealing ring, the impact and damage of the hot air flow on the furnace door can be avoided, and the LPCVD pass rate of the TOPcon battery can be improved.
[0016] Preferably, in step 1), the first low pressure condition is 5-100 mtorr, such as 5-10 mtorr, 10-50 mtorr, 50-100 mtorr.
[0017] Preferably, in step 1), the first preset temperature is 550-650°C, such as specifically 550-600°C, 600-650°C.
[0018] Preferably, in step 1), the heating rate is 10-20°C / min, such as 10-15°C / min, 15-20°C / min.
[0019] Preferably, in step 1), the oxygen flow rate is 20-40 slm, the slightly negative pressure condition is 300-700 torr, and the oxygen flow time is 100-400 s.
[0020] In the process of depositing the tunnel oxide layer under a slight negative pressure, the oxygen concentration and temperature in the reaction chamber need to be strictly controlled so that it can react with the surface of the silicon wafer and form a tunnel oxide layer. At the same time, it is necessary to avoid excessive oxygen concentration or temperature, which may lead to problems such as excessive oxidation reaction, silicon wafer surface contamination or silicon wafer surface damage.
[0021] Preferably, in step 2), the oxygen simmering time is 300-600 s, such as 300-450 s, 450-500 s, 500-600 s.
[0022] Preferably, the method further includes depositing an amorphous silicon layer on the surface of the tunneling oxide layer.
[0023] Preferably, the process of depositing an amorphous silicon layer on the surface of the tunneling oxide layer comprises the following steps: introducing silane into the reaction chamber under a second low pressure condition and a second preset temperature to deposit an amorphous silicon layer on the surface of the tunneling oxide layer.
[0024] The present application adopts a micro-negative pressure process to deposit a tunnel oxide layer. Since the air pressure will not gradually return to normal pressure and a large amount of hot air flow will not be generated, and no hot air flow passes through the furnace door and the sealing ring, the impact and damage of the hot air flow on the furnace door can be avoided, and the sealing of the reaction chamber can be effectively improved, and the gas leakage in the reaction chamber or the air outside the furnace tube is prevented from mixing into the reaction chamber, thereby ensuring the deposition quality of the amorphous silicon thin layer and further improving the conversion efficiency of the TOPcon battery. At the same time, from the perspective of production technology, it is also beneficial to make the vacuum operation more stable when depositing the amorphous silicon layer at low pressure, thereby improving the LPCVD pass rate of the TOPcon battery.
[0025] Preferably, the silane flow rate is 50-600 sccm, and the introduction time is 20-40 min. The deposition thickness of the amorphous silicon layer is related to the silane flow rate and the introduction time. By strictly controlling the above parameters within the scope of this application, the deposition quality of the amorphous silicon layer is ensured, and the overall performance of the TOPcon cell is guaranteed.
[0026] Preferably, the second low pressure condition is 100-270 mtorr, such as 100-120 mtorr, 120-150 mtorr, 150-180 mtorr, 180-200 mtorr, 200-270 mtorr. Since silane is introduced into the furnace tube, the second low pressure condition is slightly higher than the first low pressure condition.
[0027] Preferably, the second preset temperature is 550-650°C, such as specifically 550-600°C, 600-650°C.
[0028] Preferably, the reaction chamber is a furnace cavity of a furnace tube, and the furnace tube has a furnace mouth, a furnace center, and a furnace tail. Silane is introduced from the furnace mouth, the furnace center, and the furnace tail at the same time. The silane flow rate at the furnace mouth is 460-600 sccm; the silane flow rate at the furnace center is 430-460 sccm; and the silane flow rate at the furnace tail is 50-180 sccm. The method of introducing air from the furnace mouth, the furnace center, and the furnace tail can better control the uniformity of the amorphous silicon film for long furnace tubes with large production capacity. By controlling the flow rate of silane at different intake positions, the thickness of the amorphous silicon layer can be accurately controlled, which is conducive to obtaining the best film thickness matching each process to make the best conversion efficiency of the TOPcon battery.
[0029] Preferably, before the process of depositing an amorphous silicon layer on the surface of the tunnel oxide layer, the reaction chamber is first evacuated to the second low pressure condition, and then the pipeline is purged with nitrogen. More preferably, the nitrogen flow rate is 1000-5000sccm, specifically 1000-3000sccm, 3000-5000sccm. The nitrogen blowpipe is used to remove the remaining oxygen in the process of depositing the tunnel oxide layer inside the furnace tube, in preparation for the introduction of silane in the next step of depositing the amorphous silicon layer.
[0030] As described above, the method for improving the LPCVD pass rate of TOPcon cells according to the present invention has the following beneficial effects:
[0031] (1) The present application creatively adopts a micro-negative pressure deposition tunneling oxide layer process, so that during the entire reaction process of the LPCVD process, the pressure of the reaction chamber is kept below atmospheric pressure, and no hot air flows through the furnace door and the sealing ring, thereby preventing the furnace door from being deformed or the sealing ring from being burned by the heat flow, ensuring the sealing of the furnace tube during the reaction process, and maintaining a stable state in the subsequent vacuum to low-pressure process in the deposition of the amorphous silicon layer, thereby reducing the rework rate and improving the LPCVD pass rate in the TOPcon battery;
[0032] (2) The micro-negative pressure tunneling oxide layer deposition process can ensure the stability of the gas pressure and oxygen concentration in the reaction chamber, thereby improving the quality and preparation efficiency of the tunneling oxide layer; this process effectively improves the sealing of the reaction chamber, prevents gas leakage in the reaction chamber or air outside the furnace tube from mixing into the reaction chamber, ensures the deposition quality of the tunneling oxide layer and the amorphous silicon thin layer, and thus improves the conversion efficiency of the TOPcon cell;
[0033] (3) By synergistically optimizing various parameters of the LPCVD process, such as gas flow, deposition temperature, deposition time, etc., the first pass rate can be synergistically improved, thereby improving the production efficiency and cost-effectiveness of the process. At the same time, by improving the first pass rate, the scrap rate in the production process can be reduced, and the quality and stability of the product can be improved. DETAILED DESCRIPTION
[0034] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.
[0035] It should be noted that the process equipment or devices not specifically specified in the following embodiments are all conventional equipment or devices in the art.
[0036] In addition, it should be understood that one or more method steps mentioned in the present invention do not exclude the existence of other method steps before or after the combination step or the insertion of other method steps between these explicitly mentioned steps, unless otherwise specified; it should also be understood that the combination connection relationship between one or more devices / apparatuses mentioned in the present invention does not exclude the existence of other devices / apparatuses before or after the combination device / apparatus or the insertion of other devices / apparatuses between these explicitly mentioned two devices / apparatuses, unless otherwise specified. Moreover, unless otherwise specified, the numbering of each method step is only a convenient tool for identifying each method step, and is not intended to limit the order of arrangement of each method step or the scope of the present invention. Changes or adjustments in their relative relationships should also be regarded as the scope of the present invention without substantially changing the technical content.
[0037] Example 1
[0038] This embodiment provides a method for improving the LPCVD pass rate of a TOPcon cell, comprising the following steps:
[0039] 1) Place silicon wafers in the furnace chamber of the furnace tube, seal the furnace door, evacuate to 10mtorr under sealed conditions, control the heating rate to 15℃ / min, keep constant temperature after heating to 600℃, introduce oxygen to slightly negative pressure conditions, and stop oxygen supply; the slightly negative pressure condition is 500torr; the oxygen flow rate is 30slm, and the oxygen supply time is 300s;
[0040] 2) Oxygen immersion was performed under a slight negative pressure of 500 torr and a constant temperature of 600°C to deposit a tunnel oxide layer on the surface of the silicon wafer; the oxygen immersion time was 450 seconds;
[0041] 3) The furnace chamber was evacuated to a low pressure condition of 150 mtorr, and then the pipeline was purged with nitrogen at a nitrogen flow rate of 1000 sccm;
[0042] 4) Under the condition of 180 mtorr low pressure and 600°C, silane is introduced into the reaction chamber to deposit an amorphous silicon layer on the surface of the tunneling oxide layer. The furnace tube has a furnace mouth, a furnace center and a furnace tail. Silane is introduced from the furnace mouth, the furnace center and the furnace tail at the same time. The silane flow rate at the furnace mouth is 460 sccm; the silane flow rate at the furnace center is 430 sccm; the silane flow rate at the furnace tail is 180 sccm; the introduction time is 30 min;
[0043] 5) Break the vacuum, exit the boat, and take out the silicon wafer with a tunneling oxide layer (thickness of about 2 nm) and an amorphous silicon layer (thickness of about 140 nm) deposited on the surface.
[0044] Example 2
[0045] The difference between Example 2 and Example 1 is that the slightly negative pressure condition in step 1) and step 2) is 550 torr, and the rest of the processes are exactly the same.
[0046] Example 3
[0047] The difference between Example 3 and Example 1 is that the slightly negative pressure condition in step 1) and step 2) is 450 torr, and the rest of the processes are exactly the same.
[0048] Example 4
[0049] This embodiment provides a method for improving the LPCVD pass rate of a TOPcon cell, comprising the following steps:
[0050] 1) Place silicon wafers in the furnace chamber of the furnace tube, seal the furnace door, evacuate to 5mtorr low pressure under sealed conditions, control the heating rate to 10℃ / min, keep constant temperature after heating to 550℃, introduce oxygen to slightly negative pressure conditions, and stop oxygen supply; the slightly negative pressure condition is 400torr; the oxygen flow rate is 40slm, and the oxygen supply time is 100s;
[0051] 2) Under the conditions of a slight negative pressure of 400 torr and a constant temperature of 550°C, oxygen is oxidized to continue to deposit a tunneling oxide layer on the surface of the silicon wafer; the oxygen oxidization time is 300 seconds;
[0052] 3) Evacuate the furnace chamber to a low pressure of 120 mtorr, and then purge the pipeline with nitrogen at a nitrogen flow rate of 5000 sccm;
[0053] 4) Under the condition of 160 mtorr low pressure and 550°C constant temperature, silane is introduced into the reaction chamber to deposit an amorphous silicon layer on the surface of the tunneling oxide layer. The furnace tube has a furnace mouth, a furnace center and a furnace tail. Silane is introduced from the furnace mouth, the furnace center and the furnace tail at the same time. The silane flow rate at the furnace mouth is 600 sccm; the silane flow rate at the furnace center is 450 sccm; the silane flow rate at the furnace tail is 50 sccm; the introduction time is 40 min;
[0054] 5) Break the vacuum, exit the boat, and take out the silicon wafer with a tunneling oxide layer (thickness of about 2 nm) and an amorphous silicon layer (thickness of about 140 nm) deposited on the surface.
[0055] Example 5
[0056] This embodiment provides a method for improving the LPCVD pass rate of a TOPcon cell, comprising the following steps:
[0057] 1) Place silicon wafers in the furnace chamber of the furnace tube, seal the furnace door, evacuate to 100mtorr low pressure condition under sealed conditions, control the heating rate to 20℃ / min, keep constant temperature after heating to 650℃, introduce oxygen to slightly negative pressure condition, and stop oxygen; the slightly negative pressure condition is 600torr; the oxygen flow rate is 20slm, and the oxygen flow time is 400s;
[0058] 2) Oxygen immersion was performed under a slight negative pressure of 600 torr and a constant temperature of 650°C to deposit a tunnel oxide layer on the surface of the silicon wafer; the oxygen immersion time was 600 seconds;
[0059] 3) Purge constant temperature step: evacuate the furnace chamber to a low pressure condition of 180mtorr, and then purge the pipeline with nitrogen at a nitrogen flow rate of 3000sccm;
[0060] 4) Under the condition of 200 mtorr low pressure and 650°C constant temperature, silane is introduced into the reaction chamber to deposit an amorphous silicon layer on the surface of the tunneling oxide layer. The furnace tube has a furnace mouth, a furnace center and a furnace tail. Silane is introduced from the furnace mouth, the furnace center and the furnace tail at the same time. The silane flow rate at the furnace mouth is 550 sccm; the silane flow rate at the furnace center is 445 sccm; the silane flow rate at the furnace tail is 120 sccm; the introduction time is 20 min;
[0061] 5) Break the vacuum, exit the boat, and take out the silicon wafer with a tunneling oxide layer (thickness of about 2 nm) and an amorphous silicon layer (thickness of about 140 nm) deposited on the surface.
[0062] Comparative Example 1
[0063] Comparative Example 1 uses a conventional LPCVD process to prepare a tunnel oxide layer and an amorphous silicon layer, including the following steps:
[0064] 1) Place silicon wafers in the furnace chamber of the furnace tube, seal the furnace door, evacuate to low pressure, and perform heating and leak detection steps. The pressure is controlled at 10mtorr and the temperature is set at 600°C. A large amount of oxygen is introduced to the normal pressure state (10000Pa), the oxygen flow rate is 30 slm, and the oxygen flow time is continued for 500s to deposit a tunneling oxide layer on the surface of the silicon wafer.
[0065] 2) Purge and constant temperature: evacuate the furnace chamber to 150mtorr, purge the pipeline with nitrogen, the N2 flow rate is 1000sccm, and the temperature is constant at 600℃;
[0066] 3) Under the condition of 180 mtorr low pressure and 600°C, silane is introduced into the reaction chamber to deposit an amorphous silicon layer on the surface of the tunneling oxide layer. The furnace tube has a furnace mouth, a furnace center and a furnace tail. Silane is introduced from the furnace mouth, the furnace center and the furnace tail at the same time. The silane flow rate at the furnace mouth is 460 sccm; the silane flow rate at the furnace center is 430 sccm; the silane flow rate at the furnace tail is 180 sccm; the introduction time is 30 min;
[0067] 4) Break the vacuum, exit the boat, and take out the silicon wafer with a tunnel oxide layer and an amorphous silicon layer deposited on the surface.
[0068] Comparative Example 2
[0069] The difference between Comparative Example 2 and Example 1 is that the slightly negative pressure condition in step 1) and step 2) is 280 torr, and the rest of the processes are exactly the same.
[0070] Comparative Example 3
[0071] The difference between Comparative Example 3 and Example 1 is that the slightly negative pressure condition in step 1) and step 2) is 720 torr, and the rest of the processes are exactly the same.
[0072] The product pass rate is a parameter for the product to be qualified from the first process to the last process. It can understand the ability of the product to reach the finished product in all processes during the production process. It is one of the important indicators of output rate. It is a parameter that reflects the quality control ability of the enterprise. It reflects the ability of the enterprise to meet customer product requirements. The higher the pass rate, the stronger the ability. In order to verify the effect of the technical solution of this application on the LPCVD pass rate, the product pass rate after one month of using the process of Examples 1 to 5 and Comparative Examples 1 to 3 was tested respectively. The test results are shown in Table 1:
[0073] Table 1. The pass rate test results of the products obtained by the processes of Examples 1 to 5 and Comparative Examples 1 to 3
[0074]
[0075] In Table 1, "Oxidation step rework rate" refers to the rework defect rate caused by machine failure after preparing the tunnel oxide layer, and is calculated as: (abnormal number / input number)*100%; "Total pass rate" refers to the LPCVD section finished product rate, and is calculated as: (download number / input number)*100%.
[0076] It can be seen from Table 1 that by comparing Example 1 and Comparative Example 1, it can be known that after using the micro-negative pressure process of the present application for 1 month, the total straight pass rate of the LPCVD section is increased from the original 94.1% to 98.9%, and the abnormal rework rate of the oxidation step is directly reduced to 0%; by comparing Example 1 and Comparative Examples 1, 2, and 3, it can be known that the range of micro-negative pressure must be strictly controlled within the scope of the present application. Too low a pressure will lead to a decrease in the total straight pass rate, and too high a pressure will lead to an increase in the rework rate of the oxidation step.
[0077] In order to further verify the influence of the technical solution of the present application on the performance of the finally prepared TOPcon battery, the products obtained by the processes of Examples 1 to 5 and Comparative Examples 1 to 3 were respectively used to prepare TOPcon batteries. The present application example provides a method for preparing a TOPcon battery, which specifically includes the following steps:
[0078] S1: The original silicon wafer is subjected to alkali texturing to prepare a textured surface;
[0079] S2: Boron diffusion to prepare PN junction;
[0080] S3: Clean the silicon wafer and remove the borosilicate glass, etc.
[0081] S4: preparing a tunnel oxide layer and an amorphous silicon thin layer by using the processes of Examples 1 to 5 and Comparative Examples 1 to 3 respectively;
[0082] S5: Phosphorus diffusion, phosphorus doping on the back of the cell;
[0083] S6: cleaning the silicon wafer;
[0084] S7: Prepare a front aluminum oxide film to increase the passivation effect;
[0085] S8: preparing front and back silicon nitride films;
[0086] S9: Screen printing electrodes, sintering and testing.
[0087] The performance of TOPcon batteries prepared by the products obtained by the processes of Examples 1 to 5 and Comparative Examples 1 to 3 was tested respectively, and the measured values are shown in Table 2:
[0088] Table 2. Measured performance values of TOPcon batteries prepared using the products obtained by the processes of Examples 1 to 5 and Comparative Examples 1 to 3
[0089]
[0090] In order to more intuitively analyze the technical effects of the technical solution of the present application, the present application embodiment is based on the measured values in Table 2, taking the test results of Comparative Example 1 as a benchmark, and calculating the relative values of each embodiment and other comparative examples. The results are shown in Table 3:
[0091] Table 3. Relative performance values of TOPcon batteries prepared by the products obtained by the processes of Examples 1 to 5 and Comparative Examples 1 to 3
[0092]
[0093] In Tables 2 and 3: Isc is the short-circuit current, Voc is the open-circuit voltage, FF is the fill factor, Rs is the series resistance, Rsh is the parallel resistance, Eta is the conversion efficiency, and IRev2 is the reverse leakage current.
[0094] Combining Table 2 and Table 3, it can be seen that by comparing Example 1 and Comparative Example 1, it can be seen that after switching to the micro-negative pressure process of the present application, the overall performance of the TOPcon battery has also been significantly improved, and the conversion efficiency has been increased by 0.13%, mainly because the short-circuit current and the fill factor have a significant effect. This may be because the use of the micro-negative pressure process improves the sealing of the furnace tube, avoids gas leakage in the reaction chamber or air outside the furnace tube from mixing into the reaction chamber, and ensures the deposition quality of the tunneling oxide layer and the amorphous silicon thin layer. By comparing Example 1 with Examples 2 and 3, it can be seen that the conversion efficiency is best when the micro-negative pressure is controlled at 500torr. By comparing Example 1 with Comparative Examples 2 and 3, it can be seen that when the pressure of the micro-negative pressure process exceeds the range of 300~700torr, the conversion efficiency tends to decrease.
[0095] In summary, the method of improving the LPCVD straight pass rate of TOPcon batteries in this application is based on the improvement of a simple micro-negative pressure process, and the straight pass rate of LPCVD process products is effectively improved, and the damage to equipment spare parts is also greatly reduced, which indirectly saves a lot of time for replacing spare parts and rework. While improving the production capacity of the product, the overall performance of the TOPcon battery is also significantly improved. Therefore, the present invention effectively overcomes the various shortcomings of the prior art and has a high industrial utilization value.
[0096] The above is only a preferred embodiment of the present invention, and is not any formal or substantial limitation of the present invention. It should be pointed out that ordinary technicians in this technical field can make several improvements and supplements without departing from the method of the present invention, and these improvements and supplements should also be regarded as the protection scope of the present invention. Any technician familiar with this profession, without departing from the spirit and scope of the present invention, can make some changes, modifications and evolutions of the technical content disclosed above, which are equivalent embodiments of the present invention; at the same time, any changes, modifications and evolutions of any equivalent changes made to the above embodiments based on the essential technology of the present invention are still within the scope of the technical solution of the present invention.
Claims
1. A method to improve the LPCVD pass rate of TOPcon cells, It is characterized in that The following steps are involved: 1) Place a silicon wafer in the reaction chamber, evacuate to 5-100 mtorr under sealed conditions, heat to 550-650°C, introduce oxygen to a slight negative pressure of 300-700 torr, and stop oxygen flow; the oxygen flow rate is 20-40 slm, and the oxygen flow time is 100-400 s; 2) Under the above-mentioned slightly negative pressure and temperature conditions, oxygen is oxidized for 300 to 600 seconds to deposit a tunneling oxide layer on the surface of the silicon wafer; 3) At 100-200 mtorr and 550-650° C., silane is introduced into a reaction chamber to deposit an amorphous silicon layer on the surface of the tunnel oxide layer; the reaction chamber is a furnace chamber of a furnace tube, the furnace tube has a furnace mouth, a furnace center and a furnace tail, and silane is introduced from the furnace mouth, the furnace center and the furnace tail at the same time, and the silane flow rate at the furnace mouth is 460-600 sccm; the silane flow rate at the furnace center is 430-450 sccm; and the silane flow rate at the furnace tail is 50-180 sccm.
2. The method according to claim 1, Features: The silane introduction time is 20~40min.
Citation Information
Patent Citations
Process for horizontal coating of intrinsic silicon based on LPCVD technique
CN111286724A
Tunneling oxidation method based on horizontally-placed LPCVD equipment
CN111293189A
Manufacturing method of N-type crystalline silicon solar cell and manufacturing method of passivated contact structure on back surface of N-type crystalline silicon solar cell
CN112038444A
Preparation method of TOPCon battery
CN113851559A
HBC solar cell with back passivation contact structure and preparation method of HBC solar cell