A nonlinear Hall device based on a two-dimensional electron gas at the LaAlO3 / KTaO3 interface and its fabrication method.

By growing amorphous LaAlO₃ thin films on KTaO₃ single-crystal substrates and using photoresist isolation layers, a nonlinear Hall device with a two-dimensional electron gas at the LaAlO₃/KTaO₃ interface was fabricated. This solved the application limitations and complexity of diode rectifiers in the prior art, realized a stable nonlinear Hall effect on KTaO₃ single-crystal substrates, simplified the fabrication process, and achieved lateral second harmonic conversion of longitudinal AC signals at low temperatures.

CN116615090BActive Publication Date: 2026-11-24SHANGHAI QI ZHI INSTITUTE
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310622523.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-30
Publication Date
2026-11-24
Estimated Expiration
2043-05-30

AI Technical Summary

Technical Problem

The limitations and complexity of existing diode rectifiers make it difficult to achieve a stable nonlinear Hall effect in homogeneous materials, especially in van der Waals two-dimensional materials where the fabrication process is complex and unstable.

Method used

A nonlinear Hall device employing a two-dimensional electron gas at the LaAlO₃/KTaO₃ interface is constructed by growing an amorphous LaAlO₃ thin film on a KTaO₃ single-crystal substrate, using a photoresist isolation layer to form conductive and insulating regions, and combining the spin-orbit coupling characteristics of KTaO₃ to realize the conversion of longitudinal AC signals into transverse second-harmonic nonlinear Hall voltages.

Benefits of technology

It achieves stable performance in the temperature range of 2 to 100 K, simplifies the preparation process, has obvious nonlinear Hall signal, and can convert longitudinal AC signal into transverse second harmonic signal, which is convenient for information transmission and rectification.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116615090B_ABST
    Figure CN116615090B_ABST
Patent Text Reader

Abstract

This invention discloses a nonlinear Hall device based on a two-dimensional electron gas at a LaAlO3 / KTaO3 interface and its fabrication method. The device consists of a LaAlO3 / KTaO3 thin-film heterojunction and photoresist. After spin-coating a layer of photoresist and undergoing patterned exposure and development, the KTaO3 substrate is divided into covered and uncovered regions. Amorphous LaAlO3 (LAO) is grown on the uncovered region of the substrate via pulsed laser deposition, generating a two-dimensional electron gas at the oxide interface in the uncovered region, thus separating the conductive and insulating regions and obtaining the LAO / KTaO conductive interface in the shape of a Hall device. The device of this invention is suitable for low-temperature operation. Utilizing the nonlinear Hall effect of this interface, it successfully generates a nonlinear Hall voltage perpendicular to the current direction, enabling frequency doubling and rectification applications.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the interdisciplinary field of oxide electronics and nonlinear electronic devices, specifically to a nonlinear Hall device based on a two-dimensional electron gas at the LaAlO3 / KTaO3 interface and its fabrication method. Background Technology

[0002] A diode, composed of a semiconductor PN junction, has the ability to conduct electricity in one direction only. It can convert the relatively low-voltage AC output from an AC step-down circuit into unidirectional pulsating DC current, and is therefore widely used in rectifier devices. By reasonably connecting diodes with components such as resistors, capacitors, and inductors, circuits with different functions can be constructed, which can realize various functions such as AC rectification, modulation signal detection, limiting and clamping, and voltage regulation of power supply.

[0003] However, the DC current obtained by a diode rectifier is in the same direction as the original current, and can only extract the DC signal completely destructively, which has certain application limitations. In recent years, the nonlinear Hall effect observed in materials with broken spatial inversion symmetry has attracted attention. Unlike the rectification effect of a diode, this nonlinear voltage signal appears in the transverse direction perpendicular to the current, which can achieve the effect of displaying the input signal and the nonlinear signal of the output in different directions. Moreover, this effect exists in homogeneous materials and does not require the fabrication of semiconductor PN structures. However, currently this effect mainly appears in some van der Waals type two-dimensional materials, which have relatively complex fabrication processes, are not very stable, and are difficult to apply. Summary of the Invention

[0004] To address the shortcomings of existing technologies, this invention proposes a nonlinear Hall device based on a two-dimensional electron gas at the LaAlO3 / KTaO3 interface. This device can obtain a frequency-doubled signal in the direction perpendicular to the current, and has advantages such as convenient fabrication, simple structure, stable performance, and easy measurement.

[0005] The present invention adopts the following technical solution.

[0006] This invention provides a nonlinear Hall device based on a two-dimensional electron gas at a LaAlO3 / KTaO3 interface, which is used to convert a longitudinal AC signal into a frequency-doubled nonlinear Hall voltage of a certain magnitude. It includes a KTaO3 single-crystal substrate, photoresist, and an amorphous LaAlO3 (LAO) thin film. After the photoresist is coated on the KTaO3 (KTaO) single-crystal substrate, it undergoes patterned exposure and development, dividing the upper surface of the KTaO3 single-crystal substrate into a covered region and an uncovered region. In the uncovered region, an amorphous LaAlO3 thin film is grown on the KTaO3 single-crystal substrate, providing oxygen vacancies to the surface of the KTaO3 single-crystal substrate to form a conductive two-dimensional electron gas interface. The covered region is an insulating region, and the photoresist acts as an isolation layer to spatially separate a portion of the surface of the KTaO3 single-crystal substrate from the amorphous LaAlO3 thin film.

[0007] In the nonlinear Hall device of this invention, KTO, an insulating material with a high dielectric constant, is used as the substrate. Due to the presence of Ta atoms on the KTO substrate, there is strong spin-orbit coupling, and KTO serves as the primary signal source. An amorphous insulating material is grown on the KTO substrate to provide oxygen vacancies on the KTO substrate surface, forming a conductive region. This invention utilizes the difference in polarity between LAO and KTO; oxygen atoms in KTO are attracted to the LAO layer, leaving positively charged oxygen vacancies in KTO, thus forming a conductive two-dimensional electron gas interface (conductive region, the LAO / KTO conductive interface in the shape of the Hall device). Photoresist, as an insulating layer, spatially separates part of the KTO substrate surface from the LAO film, achieving separation of the insulating and conductive regions. This invention uses an ammeter to apply an alternating current of a certain frequency in the circuit, and then uses a lock-in amplifier to measure the second harmonic signal in the circuit, which can characterize the nonlinear electrical properties of the device.

[0008] In this invention, the thickness of the LAO thin film is 2 nm or more to form a conductive two-dimensional electron gas in the LAO / KTO heterojunction. The thickness of the KTO substrate and the type and thickness of the photoresist do not affect the performance of the device.

[0009] In this invention, the operating temperature of the nonlinear Hall device is between 2 and 100K.

[0010] The present invention also provides a method for fabricating the above-mentioned nonlinear Hall device, comprising the following steps:

[0011] (1) Select a KTaO3 single crystal substrate, coat the substrate with photoresist, and then use an ultraviolet lithography machine to perform mask exposure and development to obtain a substrate with some areas exposed and some areas covered by photoresist.

[0012] (2) Using laser pulse deposition, LaAlO3 thin films are grown in the exposed areas on the substrate surface.

[0013] In step (2) above, the laser energy is 230 mJ, the laser frequency is 2 Hz, and the background pressure is 2 × 10⁻⁶ mJ. -8 mTorr, with a growth rate of 0.3 nm / min.

[0014] The working principle of this invention is that, due to the strong spin-orbit coupling characteristics of KTO and the breaking of spatial inversion symmetry at the interface of the two oxides, the conductive heterojunction interface of KTO will have a strong second-order nonlinear Hall effect, which can convert an applied AC signal of a certain frequency into a transverse second harmonic AC signal and a DC signal.

[0015] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0016] In the device of this invention, when a current is applied in the longitudinal direction of the Hall device, due to the nonlinear Hall effect, a nonlinear Hall signal of a certain magnitude, proportional to the square of the current, will appear perpendicular to the current direction. The magnitude of the nonlinear signal can be characterized by a lock-in amplifier. In this way, a fundamental frequency signal of a certain frequency in the longitudinal direction can be converted into a stable transverse frequency harmonic signal, which can also be used for information transmission and rectification.

[0017] The device of the present invention has the advantages of convenient preparation, simple structure, stable performance and easy measurement; the device of the present invention has obvious nonlinear Hall signal in the temperature range of 2 to 100K, realizing frequency doubling detection in the Hall direction. Attached Figure Description

[0018] Figure 1 This is a fabrication process for a complex oxide nonlinear electronic device according to an embodiment of the present invention.

[0019] Figure 2 This is the detection method of the present invention.

[0020] Figure 3 This is a flowchart illustrating the working process of the present invention.

[0021] Figure 4 It represents the relationship between the nonlinear Hall signal in the device and the applied current.

[0022] Figure 5 It is the dependence of the device's nonlinear Hall signal on temperature. Detailed Implementation

[0023] To make the technical solution of the present invention clearer, it will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the embodiments described below are only used to explain the present invention and are not intended to limit the present invention.

[0024] The following description is a selection of several possible embodiments of the present invention, intended to provide a basic understanding of the invention, and is not intended to identify key or decisive elements of the invention or to limit the scope of protection sought.

[0025] like Figure 1 The diagram illustrates the device fabrication process according to an embodiment of the present invention. A 5mm*5mm*0.5mm KTO single-crystal substrate is selected. A drop of AZ5214 photoresist is dropped onto the substrate. A spin coater is used to spin the substrate at speeds of 600 rpm and 4000 rpm for 6 seconds and 30 seconds respectively, thereby forming a photoresist film with a thickness of approximately 1.7 μm on the KTO substrate. After spin coating, the substrate is baked on a hot plate at 90°C for 2 minutes, followed by mask exposure using an ultraviolet lithography machine. After development for 30 seconds, a substrate with the Hall device region exposed and the remaining portion covered by photoresist is obtained. After completing the above steps, an LAO thin film is grown on the developed substrate using laser pulse deposition technology. Since LAO (lattice constant)... ) and KTO (lattice constant) With a 5.2% lattice mismatch, the LAO film grown on the KTO substrate at high temperature is amorphous, so room temperature growth of the LAO film can be directly chosen. The laser energy was 230 mJ, the frequency was 2 Hz, the base voltage was 2E-8 mTorr, the growth rate was 0.3 nm / min, and the growth time was 13 min. The LAO film thickness was about 4 nm, and the thickness of the film has little impact on the final device performance. Because the KTO in the non-Hall device region is covered with a photoresist isolation layer, the LAO in this region is not in direct contact with KTO and cannot form a two-dimensional electron gas. However, the LAO in the Hall device region not covered by photoresist can directly contact KTO. Due to the different polarities of the two materials, oxygen atoms in KTO will move to the LAO layer, leaving conductive oxygen vacancies on the KTO surface, thus generating a two-dimensional electron gas at the interface.

[0026] The fabricated devices and measurement methods are as follows: Figure 2 As shown. Aluminum wires were used to connect the six contacts of the Hall effect device to the conductive electrodes of the sample holder using a wire bonding machine, facilitating subsequent electrical transport measurements. A 17.3 Hz AC signal was applied along the x-axis using a 6221 current source meter. Four lock-in amplifiers were used to measure the longitudinal and transverse AC signals at 17.3 Hz and 34.6 Hz, respectively, with a focus on extracting the second harmonic signal from the transverse signal. Simultaneously, silver paste was uniformly applied to the bottom of the KTO substrate as a bottom gate. A voltage could then be applied between the bottom gate and the sample conductive channel to adjust the carrier concentration in the channel. The main structure is as follows. Figure 3 As shown, with only the necessary components, a current source, and a nonlinear Hall signal detection device, it is possible to successfully realize and observe the conversion of an AC signal of a certain frequency into a second harmonic AC signal of a certain magnitude.

[0027] The nonlinear signal magnitude of a nonlinear Hall device based on a two-dimensional electron gas at the LAO / KTO interface was investigated below. Measurements were performed using a Power Property Measurement System (PPMS), and the device's performance was studied at 2 K. At 2 K, the surface resistivity of the sample in the device was 172 kΩ / sq., and the mobility was 530 cm⁻¹. 2 ·V -1 ·s -1 The carrier concentration is 4.73 × 10⁻⁶. 13 / cm 2 Without a magnetic field, applying an alternating current with a frequency of 17.3 Hz in the longitudinal direction produces a nonlinear signal in the transverse direction. For example... Figure 4 As shown, as the current increases from 30 μA to 300 μA, the second-order Hall voltage increases from 1 μV to 110 μV, exhibiting a square-law relationship with the applied current. This demonstrates that applying an alternating current in the longitudinal direction results in a second-order Hall voltage observed in the direction perpendicular to the current, and this voltage is proportional to the square of the current. The fundamental characteristics satisfy the formula... It can successfully achieve frequency doubling detection in the Hall direction.

[0028] The magnitude of a nonlinear signal can be measured using the second-order Hall conductivity. It indicates. Among them, V represents the transverse second-order Hall voltage. x The first-order voltage is represented by σ, the longitudinal conductivity of the channel is represented by L = 115 μm, the length between the two Hall effect sensor tips is represented by W = 20 μm, and the width of the main channel is represented by W = 20 μm. The variation of the second-order Hall conductivity with temperature is shown below. Figure 5 As shown, the nonlinear signal decreases with increasing temperature. This result indicates that the proposed nonlinear Hall device is suitable for operation at low temperatures, exhibiting a significant nonlinear Hall signal in the temperature range of 2–100 K, and its performance gradually increases as the temperature decreases.

Claims

1. A nonlinear Hall device based on a two-dimensional electron gas at the LaAlO3 / KTaO3 interface, characterized in that, It is used to convert longitudinal AC signals into a second-harmonic nonlinear Hall voltage of a certain magnitude; it includes a KTaO3 single crystal substrate, photoresist, and an amorphous LaAlO3 thin film; after the photoresist is coated on the KTaO3 single crystal substrate, it is patterned, exposed, and developed, and the upper surface of the KTaO3 single crystal substrate is divided into a covered area and an uncovered area; in the uncovered area, an amorphous LaAlO3 thin film is grown on the KTaO3 single crystal substrate, and the amorphous LaAlO3 thin film provides oxygen vacancies to the surface of the KTaO3 single crystal substrate, forming a conductive two-dimensional electron gas interface; the covered area is an insulating area, and the photoresist acts as an isolation layer to spatially separate part of the surface of the KTaO3 single crystal substrate from the amorphous LaAlO3 thin film.

2. The nonlinear Hall device according to claim 1, characterized in that, The thickness of the LaAlO3 film is greater than 2 nm.

3. The nonlinear Hall device according to claim 1, characterized in that, Its operating temperature is between 2 and 100K.

4. A method for fabricating a nonlinear Hall device according to claim 1, characterized in that, Includes the following steps: (1) Select a KTaO3 single crystal substrate, coat the substrate with photoresist, and then use an ultraviolet lithography machine to perform mask exposure and development to obtain a substrate with some areas exposed and some areas covered by photoresist. (2) Using laser pulse deposition, LaAlO3 thin films are grown in the exposed areas on the substrate surface.

5. The preparation method according to claim 4, characterized in that, In step (2), the laser energy was 230 mJ, the laser frequency was 2 Hz, the base pressure was 2 x 10 -8 mTorr, and the growth rate was 0.3 nm / min.

Citation Information

Patent Citations

  • Hall element of two-dimensional electronic gas structure and manufacturing method thereof

    CN102403450A

  • Field effect transistor device

    US20140253183A1