Process for preparing a monofilament uniform ultra-high molecular weight polyethylene fiber

By using a pressure stabilizing chamber and a filter layer in the spinning assembly, combined with a step-by-step shaping process, the problem of unevenness in ultra-high molecular weight polyethylene fiber monofilaments was solved, thereby improving the uniformity and stability of the fibers, enhancing their bulletproof performance, and reducing production costs.

CN116623306BActive Publication Date: 2026-11-24SHANGHAI RES INST OF CHEM IND CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202310505906.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-06
Publication Date
2026-11-24
Estimated Expiration
2043-05-06

Smart Images

  • Figure CN116623306B_ABST
    Figure CN116623306B_ABST
Patent Text Reader

Abstract

This invention relates to a method for preparing uniformly oriented ultra-high molecular weight polyethylene (UHMWPE) fibers, comprising the following steps: (1) uniformly mixing raw materials including UHMWPE resin powder, additives, and solvents to obtain a spinning solution, which is then fed into a twin-screw extruder for dissolution; (2) passing the solution formed in step (1) through a melt filter and a metering pump, and then through a spinning assembly for pressure-stabilized spinning to obtain uniformly oriented solution strips; (3) subjecting the obtained solution strips to coagulation and shaping treatment to obtain the target product. Compared with the prior art, this invention can effectively remove the internal stress of the fiber, improve the fiber performance, and reduce the fiber variation rate. The final prepared fiber has a single filament diameter variation rate of <5% and a fiber fineness variation rate of <3%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of ultra-high molecular weight polyethylene fiber preparation technology, and relates to a method for preparing ultra-high molecular weight polyethylene fibers with uniform monofilaments. Background Technology

[0002] With the increasing application of ultra-high molecular weight polyethylene (UHMWPE) fibers in ballistic protection, the requirements for stability against projectile velocity limits are becoming increasingly stringent. Most ballistic products employ a unidirectional fabric structure. If the fibers constituting this fabric are uneven, it will directly affect the interface between the fibers and the adhesive, the distribution of thermal stress, and tensile strength. This unevenness will lead to amplified localized stress concentrations, thereby causing premature initiation and progression of the damage process.

[0003] Since the advent of ultra-high molecular weight polyethylene (UHMWPE) fiber in the late 1970s, numerous publications have reported methods for obtaining uniform and stable fibers. Chinese patent CN1995496A mentions carefully selecting and shaping the raw resin to prepare a uniform and stable dopant solution. Then, through controlled processes such as swelling, melting, and dissolving, increased filtration precision, and online pressurization, the uniformity and stability of fiber quality and excellent performance are achieved. Chinese patent CN102433597B provides a method for obtaining gelled pre-oriented filaments by controlling the dopant solution's structural viscosity index and nozzle stretching ratio, thereby producing fibers with more uniform crystal arrangement. Chinese patent application CN115559016A relates to a highly uniform environmentally friendly polyethylene fiber and its preparation method. This method prepares a gel solution through specific temperature and time, thereby improving fiber uniformity. These methods all focus on controlling the uniformity of the solution to obtain stable fibers, rarely addressing the uniformity between monofilaments.

[0004] As is well known, the uniformity of fiber monofilaments is also an important quality indicator, mainly encompassing two aspects: geometric non-uniformity and physical structural non-uniformity. For ultra-high molecular weight polyethylene fibers, geometric non-uniformity refers to the variation in thickness of a single fiber along its length, while physical structural non-uniformity includes two aspects: one is the appearance non-uniformity caused by factors such as inclusions and air bubbles, and the other is the microscopic non-uniformity due to solution crystallization and orientation. Besides being affected by the properties of the spinning solution, the spinning assembly is a crucial core element in addressing these issues, playing a vital role in the stability of the spinning process.

[0005] Chinese patent CN109468689A discloses a spinning method for ultra-high molecular weight polyethylene (UHMWPE) fibers. This method uses a two-stage gentle mixing mill for continuous and stable feeding and pressure building, allowing the spinning solution to be extruded more stably and uniformly at the spinneret, thereby increasing the fiber evenness. However, this method involves expensive equipment and complex process control. Chinese patent CN114775070A mentions a method for preparing UHMWPE fibers and its spinneret assembly. This assembly increases extrusion pressure by narrowing the diameter of the pressurized feeding section, thereby improving extrusion uniformity. However, this assembly has a complex structure, causing considerable trouble for installation and post-processing. Summary of the Invention

[0006] The purpose of this invention is to provide a method for preparing ultra-high molecular weight polyethylene fibers with uniform monofilaments. From the perspective of spinning components, this method aims to solve the problem of uneven output as much as possible at the source, ensure the uniformity between monofilaments, and then perform appropriate process shaping to make the microstructure more regular and the fibers more uniform. At the same time, it also reduces the internal stress of the fibers and makes the performance more stable.

[0007] The objective of this invention can be achieved through the following technical solutions:

[0008] A method for preparing uniform monofilament ultra-high molecular weight polyethylene fiber includes the following steps:

[0009] (1) Mix the raw materials, including ultra-high molecular weight polyethylene resin powder, additives and solvents, evenly to obtain spinning solution, and then send it into a twin-screw extruder for dissolution.

[0010] (2) The solution formed in step (1) passes through a melt filter and a metering pump, and then through a spinning assembly for pressure-stabilized spinning to obtain uniform monofilament solution strips.

[0011] (3) The resulting solution strips are then solidified and shaped to obtain the target product.

[0012] It should be noted that all raw materials can be known materials commonly used in the art, and the selection of their components is not a point of protection claimed by this invention. For example, specific raw material selection can be found in patent CN113622037A.

[0013] Furthermore, in step (2), the spinning assembly includes a pressure stabilizing chamber, a distribution plate, and a spinneret arranged sequentially along the solution travel direction. The pressure stabilizing chamber is equipped with a filter layer. One function of the filter layer is to filter the solution, removing mechanical impurities and gel particles from the solution. Another function is to ensure thorough mixing of the solution and prevent differences in solution viscosity. A third function is to build up pressure and evenly distribute the solution to each spinneret orifice, forming a fine flow of solution.

[0014] Furthermore, the thickness of the filter layer is 15-50 mm. A filter layer that is too thick will significantly increase the residence time of the solution, causing the solution to be compressed and heated, leading to macromolecular degradation and thus affecting performance. Additionally, the filter layer consists of 1-3 layers of filter media arranged from coarse to fine along the solution flow direction, preferably 2-3 layers. The first layer through which the solution flows is a coarse media layer, followed by the second and third layers, which are progressively finer media layers. The purpose of this is twofold: first, to form a tiered filtration system, increasing filtration effectiveness and improving filtration accuracy. If filtration relies solely on the first layer, the filter cake formed by impurities will quickly reduce the throughput and shorten the component's lifespan; second, to achieve more uniform pressure distribution, ensuring consistent output from each spinneret orifice.

[0015] Furthermore, the filter medium in the filter layer is one or more of the following: metal sand, sea sand, ultrafine glass beads, ceramic beads, diatomaceous earth, and sintered metal.

[0016] More preferably, the filter medium is granular with a particle size of 5-40 mesh, more preferably 5-30 mesh. If the particle size is too large, the filtration accuracy is low, making it impossible to establish a high discharge pressure, and it also affects the shear rate of the solution within the spinneret orifice, resulting in insufficient macromolecular orientation. Of course, the particle size also cannot be too small; if it is too small, the filter layer resistance is too high, and pressure loss within the filter layer is severe, leading to potentially low discharge pressure.

[0017] Furthermore, in step (2), the pressure for pressure-stabilized spinning is 1.2-5.5 MPa, more preferably 1.5-4.5 MPa. Under a certain component pressure, the ultra-high molecular weight polyethylene solution can generate a high shear rate, which can improve the rheological properties of the solution and increase its temperature during extrusion. However, the shear rate should not be too high, as this will make it difficult to control the uniformity of the initial filament stretching, and excessive temperature increase will cause macromolecular degradation, thus affecting performance. Conversely, if the initial component pressure is low, it will lead to uneven solution distribution and more fuzz and loose fibers at the spinneret edges.

[0018] Furthermore, in step (3), the shaping process includes sequentially performing a first-stage tension shaping, solvent removal, a second-stage tension shaping, multi-stage hot stretching, and heat shaping.

[0019] Furthermore, the tensile tension for a single tension setting is 1.0-2.5 CN / dtex, the time is no less than 10 s, and the temperature is 25-35℃. The main purpose of tension setting at this stage is to influence intermolecular forces through the action of tensile and shear fields, thereby improving the fiber's microstructure, making orientation and crystallization more regular, and thus resulting in more uniform monofilaments. It also reduces the internal stress generated in the nascent filaments during stretching, allowing macromolecules to relax and leading to more stable finished product performance. The temperature and time of tension setting are interdependent. Because the nascent filaments have a weak macromolecular network structure and contain a large amount of solvent, they cannot be completely set at this stage, but intermolecular forces can be interfered with. Higher temperatures require shorter setting times, but increased phase separation accelerates crystallization, which is detrimental to the regularity of crystallization. Conversely, lower temperatures increase the setting time. However, this requires correspondingly longer production equipment, increasing costs. In addition, after the solution filaments flowing out of the spinneret solidify, the initial filament morphology is a three-dimensional network-like gel. The network skeleton is composed of macromolecules or macromolecular chain bundles. Due to the phase separation and desolvation, the macromolecules will still be entangled. Therefore, a certain tensile tension is required to prevent the interaction between macromolecules and reduce back entanglement.

[0020] Furthermore, the tensile tension for secondary tension setting is 0.1-0.6 CN / dtex, the time is no less than 15 s, and the temperature is 30-45℃. After solvent removal, the filaments shrink rapidly due to rapid phase separation, resulting in high bundle tension. At this time, the crystallinity also increases rapidly with solvent evaporation. Therefore, the setting time should be appropriately extended to slow down the crystallization process, thereby making the crystals more regular and the monofilaments more uniform. However, when the temperature is >45℃, the solvent evaporation rate is too fast, and the crystallization process is difficult to control, macroscopically manifesting as fiber surface adhesion, poor openness, and insufficient softness. In addition, the nascent filaments at this stage are already dry semi-finished fibers after solvent removal, possessing a certain degree of orientation and crystallinity. If the tensile tension is too high, it will continue to induce orientation, increasing crystallinity and affecting subsequent hot stretching. However, if the tensile tension is too low, the distance between macromolecules increases, the intermolecular forces weaken, the structure becomes loose, and the tensile properties easily deteriorate.

[0021] Furthermore, the tensile tension during heat setting is ≤0.3 CN / dtex, the time is no less than 6 s, and the temperature is 130-140℃. The purpose of this heat setting differs from the previous setting; it primarily aims to eliminate internal stress and improve the thermal stability of the fiber during subsequent processing. Therefore, the setting temperature is chosen near the melting point, causing the macromolecular chains and even chain segments to shift due to thermal motion, rebuilding intermolecular forces in their new positions, and reaching the most stable state. Here, to allow the macromolecules to fully relax, the tensile tension should be as low as possible. At this point, small, poorly intact crystals will melt, while larger, more uniform crystals will enlarge or become more complete, resulting in a more stable structure after rearrangement and better monofilament consistency.

[0022] In summary, this invention controls spinning pressure by selecting appropriate component structures, thereby ensuring uniform output from each spinneret and guaranteeing the consistency of monofilaments. After the spinning solution solidifies, the macromolecular network structure saturated with solvent remains unstable. Compared to conventional preparation processes, this method implements a step-by-step shaping process to further optimize the microstructure, while simultaneously reducing internal stress in the fiber and stabilizing the performance of the finished product. The final obtained fiber monofilament diameter variation rate is <5%, and the fiber fineness variation rate is <3%.

[0023] Compared with the prior art, the present invention has the following advantages:

[0024] 1) By selecting appropriate processes, fiber performance was improved, and internal stress in the fibers was effectively removed, reducing the fiber variation rate.

[0025] 2) UD and composite fabrics made from fiber processing have a smooth surface, fewer bubbles, strong interlayer adhesion, high ballistic performance, and small V50 value variation.

[0026] 3) Products made from composite fabrics are not only lighter in weight but also thinner, while maintaining the same level of protection.

[0027] 4) After adopting the solution of the present invention, the fibers are uniform, the residual stress is low, the structure is stable, the thermal stretching efficiency is improved, the overall operation is convenient, and the production cost is reduced. Attached Figure Description

[0028] Figure 1 This is a flowchart of the preparation process of the present invention;

[0029] Figure 2 This is a schematic diagram of the spinning assembly.

[0030] Figure 3 The process parameters for each embodiment and comparative example are provided.

[0031] Explanation of markings in the diagram:

[0032] 1. Spinneret; 2. Distribution plate; 3. Pressure stabilizing chamber; 4. Filter screen; 5. Upper flow channel. Detailed Implementation

[0033] The present invention will now be described in detail with reference to specific embodiments. These embodiments are based on the technical solution of the present invention and provide detailed implementation methods and specific operating procedures. However, the scope of protection of the present invention is not limited to the following embodiments.

[0034] In the following embodiments, unless otherwise specified, the raw materials or processing techniques are conventional commercially available raw materials or conventional processing techniques in the art.

[0035] Tensile tension is measured by a handheld digital tension meter. Tensile tension = tension value / fineness.

[0036] Measurement of the variation rate of single filament diameter: First, several single filament diameter values ​​are measured by electron microscopy, and the average value and standard deviation are calculated. Variation rate = (standard deviation / average value) × 100%.

[0037] Calculation of the variation rate of fiber fineness: The fineness of the fiber is measured according to "GB / T14343-2008 Test Method for Linear Density of Chemical Fiber Filaments", and the average value and standard deviation are calculated. Variation rate = (standard deviation / average value) × 100%.

[0038] Example 1:

[0039] See Figure 1 and Figure 2 As shown, ultra-high molecular weight polyethylene resin powder with a viscosity-average molecular weight of 4.5 million is mixed evenly with antioxidant 168 at a mass ratio of 1000:5 in a mixing tank. Then, constant-temperature mineral oil is injected, with the mass ratio of ultra-high molecular weight polyethylene resin powder to mineral oil being 1:12. After the mixture is evenly dispersed, it is fed into a twin-screw extruder for dissolution. The resulting solution passes through a melt filter and a metering pump into the spinning assembly. The solution enters the pressure stabilizing chamber 3 through the upper flow channel 5 of the assembly (a filter screen 4 can be installed between the two), flows through the distribution plate 2 and the spinneret 1 in stages, and finally passes through a 20mm nitrogen-protected air gap section in the form of a thin flow of solution into the coagulation bath. The filter medium in the pressure stabilizing chamber is two layers of 30mm thick spherical sea sand, with the upper layer being 15mm thick 5-mesh coarse sea sand and the lower layer being 15mm thick 20-mesh fine sea sand. The pressure of the spinning assembly is 2.1MPa.

[0040] After solidification, the gel filaments underwent a 2.5-fold pre-stretch, followed by a first setting process at 30°C for 10 seconds with a tensile tension of 1.0 CN / dtex. Then, the filaments were desoldered and subjected to a second setting process at 45°C for 15 seconds with a tensile tension of 0.1 CN / dtex. Finally, after a three-stage hot-box stretching process, a third setting process was performed at 140°C for 6 seconds with a tensile tension of 0.3 CN / dtex. The resulting product was then wound to obtain ultra-high molecular weight polyethylene (UHMWPE) fibers, and the fiber properties were tested according to GB / T14344-2022.

[0041] Example 2:

[0042] The difference from Example 1 is that the upper layer of sea sand in the pressure stabilizing chamber is 15mm thick coarse sea sand of 10 mesh, and the lower layer is 15mm thick fine sea sand of 30 mesh; the pressure of the spinning assembly is 2.5MPa. Additionally, the first setting time is 10s, the setting temperature is 35℃, and the tensile tension is 2.0CN / dtex.

[0043] Example 3:

[0044] The difference from Example 1 is that the upper layer of sea sand in the pressure stabilizing chamber is 20mm thick coarse sea sand of 5 mesh, and the lower layer is 20mm thick fine sea sand of 40 mesh; the pressure of the spinning assembly is 2.4MPa. Additionally, the first setting time is 25s, the setting temperature is 25℃, and the tensile tension is 2.5CN / dtex.

[0045] Example 4:

[0046] The difference from Example 1 is that the filter medium in the pressure stabilizing chamber is a 50mm thick layer of three spherical sea sands: the upper layer is a 15mm thick layer of 5-mesh coarse sea sand, the middle layer is a 15mm thick layer of 20-mesh fine sea sand, and the lower layer is a 20mm thick layer of 40-mesh fine sea sand. The pressure of the spinning assembly is 3.3MPa. Additionally, the second setting time is 30s, the setting temperature is 30℃, and the tensile tension is 0.4CN / dtex.

[0047] Example 5:

[0048] The difference from Example 1 is that the filter medium in the pressure stabilizing chamber is a 15mm thick layer of 5-mesh spherical sea sand, and the pressure of the spinning assembly is 1.5MPa. Additionally, the second setting time is 25s, the setting temperature is 35℃, and the tensile tension is 0.6CN / dtex.

[0049] Example 6:

[0050] The difference from Example 1 is that the filter medium in the pressure stabilizing chamber is a 30mm thick layer of irregularly shaped 40-mesh metal sand, and the pressure of the spinning assembly is 4.5MPa. Additionally, the third setting time is 9s, the setting temperature is 140℃, and the tensile tension is 0.3CN / dtex.

[0051] Comparative Example 1:

[0052] The difference from Example 1 is that: after the gel filament is pre-stretched, it is directly desolvated and subjected to three-stage hot stretching, without a shaping process.

[0053] Comparative Example 2:

[0054] The difference from Example 1 is that the pressure stabilizing chamber is an empty cavity, and the solution is directly extruded and formed after passing through the pressure stabilizing chamber, the distribution plate, and the spinneret. The pressure of the spinning assembly is 1.2 MPa.

[0055] Comparative Example 3:

[0056] The difference from Example 1 is that the pressure stabilizing chamber is an empty cavity, and the solution is directly extruded and formed after passing through the pressure stabilizing chamber, the distribution plate, and the spinneret. The pressure of the spinning assembly is 1.2 MPa, and there is no shaping process.

[0057] The process parameters for the above embodiments and comparative examples are shown in [reference needed]. Figure 3 The corresponding performance evaluation is shown in Table 1.

[0058] Table 1

[0059] project Fineness variation rate (%) Variation rate of single filament diameter (%) Example 1 2.3 4.5 Example 2 2.1 4.2 Example 3 2.1 3.9 Example 4 1.8 3.5 Example 5 2.7 4.9 Example 6 2.9 3.6 Comparative Example 1 3.8 5.5 Comparative Example 2 5.2 5.6 Comparative Example 3 5.5 6.1

[0060] Test results show that the fiber product produced by this patented method has a low fineness variation rate and a low diameter variation rate. Comparative Example 1 did not implement a setting process, Comparative Example 2 had no pressure stabilization setting during spinning, and Comparative Example 3 had neither a setting process nor pressure stabilization considerations, representing the current production status of most manufacturers in the industry. This invention controls the spinning pressure by adjusting the material, shape, precision, and thickness of the filter medium in the pressure stabilization chamber of the component, thereby ensuring uniform solution output to each spinneret and obtaining uniform nascent filaments. Then, by controlling the tensile tension, the structure of the nascent filaments is adjusted, providing appropriate tension for setting, resulting in more regular fiber orientation and crystallization, more uniform filament bundles, and a lower unevenness rate.

[0061] Examples 7-11:

[0062] Compared with Example 1, most of them are the same, except that the sea sand is replaced with metal sand, ultrafine glass beads, ceramic beads, diatomaceous earth and sintered metal respectively.

[0063] Example 12:

[0064] Compared to Example 1, most aspects are the same, except that the following process parameters are adjusted accordingly:

[0065] The tensile tension for a single tension setting was 2.5 CN / dtex, the time was 10 s, and the temperature was 35℃.

[0066] The tensile tension for secondary tension setting was 0.6 CN / dtex, the time was 15 s, and the temperature was 40℃.

[0067] The heat setting tensile tension was 0.2 CN / dtex, the time was 8 s, and the temperature was 135℃.

[0068] Example 13:

[0069] Compared to Example 1, most aspects are the same, except that the following process parameters are adjusted accordingly:

[0070] The tensile tension for a single tension setting was 1.5 CN / dtex, the time was 12 s, and the temperature was 25℃.

[0071] The tensile tension for secondary tension setting was 0.3 CN / dtex, the time was 18 s, and the temperature was 30℃.

[0072] The heat setting tensile tension was 0.3 CN / dtex, the time was 7 s, and the temperature was 130℃.

[0073] The above description of the embodiments is provided to enable those skilled in the art to understand and use the invention. It will be apparent to those skilled in the art that various modifications can be made to these embodiments, and the general principles described herein can be applied to other embodiments without inventive effort. Therefore, the present invention is not limited to the above embodiments, and any improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the invention should be within the protection scope of the present invention.

Claims

1. A method for preparing ultra-high molecular weight polyethylene fibers with uniform monofilaments, characterized in that, Includes the following steps: (1) Mix the raw materials, including ultra-high molecular weight polyethylene resin powder, additives and solvents, evenly to obtain spinning solution, and then send it into a twin-screw extruder for dissolution. (2) The solution formed in step (1) passes through a melt filter and a metering pump, and then through a spinning assembly for pressure-stabilized spinning to obtain uniform monofilament solution strips; (3) The resulting solution strips are then solidified and shaped to obtain the target product; In step (2), the spinning assembly includes a pressure stabilizing chamber, a distribution plate and a spinneret arranged sequentially along the solution travel direction, and the pressure stabilizing chamber is equipped with a filter layer. The thickness of the filter layer is 15-50 mm, and it consists of 2-3 layers of filter media arranged from coarse to fine along the solution flow direction; The filter medium is in granular form with a particle size of 5-40 mesh; In step (2), the pressure for pressure-stabilized spinning is 1.2-5.5 MPa; In step (3), the shaping process includes sequentially performing primary tension shaping, solvent removal, secondary tension shaping, multi-stage hot stretching, and heat shaping. The tensile tension for a single tension setting is 1.0-2.5 cN / dtex, the time is not less than 10 s, and the temperature is 25~35℃; The tensile tension for secondary tension setting is 0.1-0.6 cN / dtex, the time is not less than 15s, and the temperature is 30-45℃.

2. The method for preparing uniform monofilament ultra-high molecular weight polyethylene fiber according to claim 1, characterized in that, The filter medium in the filter layer is one or a combination of several of the following: metal sand, sea sand, ultrafine glass beads, ceramic beads, diatomaceous earth, and sintered metal.

3. The method for preparing uniform monofilament ultra-high molecular weight polyethylene fiber according to claim 1, characterized in that, The heat setting tensile tension is ≤0.3CN / dtex, the time is not less than 6s, and the temperature is 130-140℃.

Citation Information

Patent Citations

  • Gelatinized pre-oriented yarn and preparation method thereof and ultra high molecular weight polyethylene fiber and preparation method thereof

    CN102433597B

  • Dual-order soft mixing machine and ultrahigh molecular weight polyethylene fiber jelly spinning method adopting same

    CN109468689A

  • Ultrahigh molecular weight polyethylene fiber as well as preparation method and application thereof

    CN113622037A

  • Preparation method of ultra-high molecular weight polyethylene fiber, spinneret plate assembly used in preparation method and obtained multifilament yarn

    CN114775070A

  • Environment-friendly polyethylene fiber with high uniformity and preparation method

    CN115559016A