Light emitting diode epitaxial structure and preparation method thereof, and light emitting diode
Patent Information
- Application Number
- CN202310652872.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-05
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-06-05
AI Technical Summary
[0004]本发明的目的在于针对已有的技术现状,提供一种发光二极管外延结构及其制备方法、发光二极管,本发明在N型GaN层与多量子阱层之间插入应力调控层,可在有效缓解InGaN量子阱与N型GaN层之间存在的失配应力的同时,释放GaN外延层累积的应力,从而有效防止因应力失配所引发的InGaN量子阱存在In组分并入困难、晶体缺陷多和极化电场大等问题以及外延层张应力累积所引发的外延层易断裂的问题,提升多量子阱层中电子与空穴的波函数的空间重叠度,外延结构表面平整度高,裂纹少,可靠性佳,发光效率高
Smart Images

Figure CN116632129B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of semiconductor technology, and in particular to an epitaxial structure of a light-emitting diode and its fabrication method, and a light-emitting diode. Background Technology
[0002] In the existing epitaxial structure of GaN-based light-emitting diodes, the active region generally uses InGaN quantum wells. Due to the large mismatch stress between the InGaN quantum well and the N-type GaN layer, problems such as difficulty in the incorporation of In components, numerous crystal defects, and large polarization electric fields can easily occur in the InGaN quantum well.
[0003] To address the aforementioned issues, existing technologies typically insert a stress relief layer between the N-type GaN layer and the active region to buffer the mismatch stress in the active region. A common stress relief layer is the InGaN / GaN superlattice layer. However, this stress relief layer cannot release the large tensile stress between the substrate and the GaN epitaxial layer, and the continuous accumulation of tensile stress can even lead to the fracture of the epitaxial layer. In addition, the high lattice torsion energy of GaN also results in insufficient stress relief. Summary of the Invention
[0004] The purpose of this invention is to address the existing technological limitations by providing a light-emitting diode epitaxial structure and its fabrication method, as well as the light-emitting diode itself. This invention inserts a stress-regulating layer between the N-type GaN layer and the multiple quantum well layer. This effectively alleviates the mismatch stress between the InGaN quantum well and the N-type GaN layer while releasing the accumulated stress in the GaN epitaxial layer. This effectively prevents problems caused by stress mismatch, such as difficulty in In component incorporation, numerous crystal defects, and large polarization electric fields in the InGaN quantum well, as well as the problem of easy fracture of the epitaxial layer caused by accumulated tensile stress. It also improves the spatial overlap of the wave functions of electrons and holes in the multiple quantum well layer, resulting in a high surface flatness, fewer cracks, good reliability, and high luminous efficiency in the epitaxial structure.
[0005] To achieve the above objectives, the present invention adopts the following technical solution:
[0006] First, this invention provides a method for fabricating a light-emitting diode epitaxial structure, comprising:
[0007] Provide substrate;
[0008] A buffer layer, an undoped GaN layer, an N-type GaN layer, a stress modulation layer, a multiple quantum well layer, an electron blocking layer, and a P-type GaN layer are sequentially deposited on the substrate.
[0009] The stress regulation layer comprises a first regulation layer and a second regulation layer deposited sequentially along the epitaxial direction, wherein the first regulation layer is Sc. x Al 1-x N layers, the second control layer is Scy Al z Ga 1-y-z N / InN superlattice structure layer.
[0010] In some embodiments, in the first control layer, 0.5 ≥ x ≥ 0.01, and in the second control layer, 0.1 ≥ y ≥ 0.01, 0.5 ≥ z ≥ 0.01.
[0011] In some embodiments, the Sc y Al z Ga 1-y-z The N / InN superlattice structure layers consist of periodically alternating stacks of Sc y Al z Ga 1-y-z The N sublayer and InN sublayer have 2 to 20 periods.
[0012] In some embodiments, the Sc x Al 1-x The thickness of the N layer is 1 nm to 100 nm, and the Sc y Al z Ga 1-y-z The thickness of the N sublayer is 5nm to 500nm, and the thickness of the InN sublayer is 0.5nm to 10nm.
[0013] In some embodiments, the Sc y Al z Ga 1-y-z The growth atmosphere of the N / InN superlattice structure layer is N2 / NH3, and the flow ratio between N2 and NH3 is 1:(0.1~10).
[0014] In some embodiments, the Sc x Al 1-x The growth temperature of the N layer is 900℃~1100℃, and the Sc y Al z Ga 1-y- z The growth temperature of the N / InN superlattice structure layer is 800℃~1000℃.
[0015] In some embodiments, the multi-quantum-well layer includes periodically alternating InGaN quantum well layers and AlGaN quantum barrier layers, with 6 to 12 periods. The growth temperature of the InGaN quantum well layer is 790°C to 810°C, and the thickness is 2 nm to 5 nm. The growth temperature of the AlGaN quantum barrier layer is 800°C to 900°C, and the thickness is 5 nm to 15 nm.
[0016] In some embodiments, the buffer layer consists of an AlN buffer layer and a GaN buffer layer stacked sequentially, and the preparation steps of the buffer layer are as follows:
[0017] An AlN buffer layer was sputtered onto the substrate using a PVD sputtering process.
[0018] The substrate with the sputtered AlN buffer layer was transferred into the MOCVD equipment for H2 pretreatment and nitriding pretreatment. The atmosphere for H2 pretreatment was H2, the treatment temperature was 1000℃~1200℃, and the treatment time was 1min~10min.
[0019] Secondly, the present invention also provides a light-emitting diode epitaxial structure, which is prepared according to the above-described method for preparing a light-emitting diode epitaxial structure.
[0020] Furthermore, the present invention also provides a light-emitting diode, comprising an epitaxial structure prepared by the above-described method for preparing an epitaxial structure of a light-emitting diode.
[0021] The beneficial effects of this invention are as follows:
[0022] In this invention, a stress modulation layer is inserted between an N-type GaN layer and a multiple quantum well layer, and the stress modulation layer comprises a first modulation layer and a second modulation layer. The first modulation layer is a Sc x Al 1-x N layers, due to Sc x Al 1-x The lattice constant of the N-layer is smaller than that of GaN, thus generating compressive stress on the GaN epitaxial layer and alleviating the tensile stress exerted by the GaN epitaxial layer on the substrate. Simultaneously, the introduced Sc element effectively reduces the potential barrier and strain relaxation of GaN's crystal axis torsion, better releasing the tensile stress of the GaN epitaxial layer. Secondly, the second control layer uses Sc. y Al z Ga 1-y-z In the N / InN superlattice structure layer, on the one hand, since GaN and ScN have similar lattice constants, the Sc in the second control layer... y Al z Ga 1-y-z N sublayer and Sc of the first regulatory layer x Al 1-x The N-layer has a smaller lattice phase difference and a higher lattice matching degree, which improves the crystal quality. On the other hand, due to the Sc y Al z Ga 1-y-zThe lattice constant of the N-sublayer is smaller than that of the InN-sublayer. The two material layers are periodically stacked alternately, and their tensile and compressive stresses change alternately, effectively releasing the stress accumulated in the GaN epitaxial layer and alleviating the mismatch stress between the InGaN quantum well and the N-type GaN layer. This effectively prevents problems caused by stress mismatch, such as difficulty in the incorporation of In composition, many crystal defects, and large polarization electric field in the InGaN quantum well, as well as the problem of easy fracture of the epitaxial layer caused by the accumulation of tensile stress. It also improves the spatial overlap of the wave functions of electrons and holes in the multi-quantum-well layer, resulting in high surface flatness, fewer cracks, good reliability, and high luminous efficiency of the epitaxial structure. Attached Figure Description
[0023] Figure 1 This is a schematic diagram of the epitaxial structure of the light-emitting diode of the present invention.
[0024] Figure 2 This is a flowchart of the method for preparing the epitaxial structure of the light-emitting diode according to the present invention.
[0025] Figure 3 This is a flowchart of step S200 of the method for preparing the epitaxial structure of a light-emitting diode according to the present invention. Detailed Implementation
[0026] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be described in further detail below.
[0027] First, refer to Figure 1 and Figure 2 As shown, this invention discloses a method for fabricating an epitaxial structure of a light-emitting diode, comprising:
[0028] S100. Provide substrate 1, wherein substrate 1 may be any one of sapphire substrate, SiO2-sapphire substrate, silicon substrate, silicon carbide substrate, gallium nitride substrate, and zinc oxide substrate;
[0029] S200. A buffer layer 2, an undoped GaN layer 3, an N-type GaN layer 4, a stress modulation layer 5, a multiple quantum well layer 6, an electron blocking layer 7, and a P-type GaN layer 8 are sequentially deposited on substrate 1.
[0030] The stress regulation layer 5 includes a first regulation layer 51 and a second regulation layer 52 deposited sequentially along the epitaxial direction. The first regulation layer 51 is Sc x Al 1-x N layers, the second control layer 52 is Sc y Al z Ga 1-y-z N / InN superlattice structure layer.
[0031] In this invention, a stress modulation layer 5 is inserted between the N-type GaN layer 4 and the multiple quantum well layer 6, and the stress modulation layer 5 is provided with a first modulation layer 51 and a second modulation layer 52. The first modulation layer 51 is a Sc x Al 1-x N layers, due to Sc x Al 1-x The lattice constant of the N layer is smaller than that of GaN, thus generating compressive stress on the GaN epitaxial layer and alleviating the tensile stress exerted by the GaN epitaxial layer on the substrate 1. Simultaneously, the introduced Sc element effectively reduces the potential barrier and strain relaxation of GaN's crystal axis torsion, better releasing the tensile stress of the GaN epitaxial layer. Furthermore, the second control layer 52 uses Sc. y Al z Ga 1-y-z In the N / InN superlattice structure layer, on the one hand, since GaN and ScN have similar lattice constants, the Sc in the second control layer 52... y Al z Ga 1-y-z N sublayer 521 and the Sc of the first control layer 51 x Al 1-x The N-layer has a smaller lattice phase difference and a higher lattice matching degree, which improves the crystal quality. On the other hand, due to the Sc y Al z Ga 1-y-z The lattice constant of the N sublayer 521 is smaller than that of the InN sublayer 522. The two material layers are periodically stacked alternately, and their tensile stress and compressive stress change alternately, effectively releasing the stress accumulated in the GaN epitaxial layer and alleviating the mismatch stress between the InGaN quantum well and the N-type GaN layer 4. This effectively prevents problems such as difficulty in the incorporation of In composition, many crystal defects and large polarization electric field in the InGaN quantum well caused by stress mismatch, as well as the problem of easy fracture of the epitaxial layer caused by the accumulation of tensile stress in the epitaxial layer. It also improves the spatial overlap of the wave functions of electrons and holes in the multi-quantum-well layer 6. The epitaxial structure has high surface flatness, few cracks, good reliability and high luminous efficiency.
[0032] In the first regulatory layer 51, 0.5 ≥ x ≥ 0.01; in the second regulatory layer 52, 0.1 ≥ y ≥ 0.01, 0.5 ≥ z ≥ 0.01; when Sc x Al 1-x When x in layer N is too large, the crystal quality of the material layer will decrease, and the released stress will be reduced. When Sc y Al z Ga 1-y- z When the values of y and z of N are too large, Sc y Al z Ga 1-y-zIf the lattice mismatch between N and InN is too large, the crystal quality of the material layer will decrease.
[0033] Among them, Sc y Al z Ga 1-y-z The N / InN superlattice structure layers consist of periodically alternating stacks of Sc y Al z Ga 1-y-z The N sublayer 521 and the InN sublayer 522 have 1 to 20 cycles, more preferably 2 to 20 cycles. For example, the number of cycles is 2, 6, 10, 15, 18 or 20, but is not limited to these. Appropriately increasing the number of cycles can increase the number of alternations between tensile stress and compressive stress, which is beneficial to releasing the stress accumulated in the GaN epitaxial layer. However, too many cycles can easily lead to an increase in defects.
[0034] Among them, Sc x Al 1-x The thickness of the N layer is 1nm to 100nm, for example, Sc x Al 1-x The thickness of the N layer can be 1nm, 20nm, 30nm, 50nm, 80nm, or 100nm, but is not limited to these. y Al z Ga 1-y-z The thickness of the N sublayer 521 is 5nm to 500nm, for example, Sc y Al z Ga 1-y-z The thickness of the N sublayer 521 is 5nm, 20nm, 80nm, 150nm, 250nm, 300nm, 420nm, or 480nm, but is not limited thereto. The thickness of the InN sublayer 522 is 0.5nm to 10nm. For example, the thickness of the InN sublayer 522 is 1nm, 3nm, 7nm, or 10nm, but is not limited thereto. More preferably, the thickness of the Sc sublayer 521 is... x Al 1-x The thickness of the N layer is 30nm to 100nm, Sc y Al z Ga 1-y-z The thickness of the N sublayer 521 is 200nm–500nm, the thickness of the InN sublayer 522 is 0.5nm–10nm, and the thickness of the InN sublayer 522 is 2nm–10nm. x Al 1-x When the N-layer thickness is too small, the accumulated compressive stress is insufficient, making it difficult to adequately alleviate the tensile stress in the GaN epitaxial layer. When the Sc... y Al z Ga 1-y-zWhen the thickness of the N sublayer 521 and the InN sublayer 522 is too small, the stress alternation is not obvious, the stress release effect is poor, and the Sc y Al z Ga 1-y-z If the N-sublayer 521 thickness is too small, the lattice quality decreases, and when Sc y Al z Ga 1-y-z When the thickness of the N sublayer 521 and the InN sublayer 522 is too large, the defect density increases.
[0035] Among them, Sc y Al z Ga 1-y-z The growth atmosphere for the N / InN superlattice structure layer is N2 / NH3, and the flow ratio between N2 and NH3 is 1:(0.1~10). If H2 is used as the growth atmosphere, H2 will cause InN to decompose and will also lead to excessive carbon content. By using N2 / NH3 as the growth atmosphere, the above problems can be effectively avoided. At the same time, the N2 content should not be too high, as excessive N2 can easily lead to a decrease in the crystal quality of the superlattice structure layer.
[0036] Among them, Sc x Al 1-x The growth temperature of the N layer is 900℃~1100℃, Sc y Al z Ga 1-y-z The growth temperature of the N / InN superlattice structure layer is 800℃~1000℃. For example, Sc x Al 1-x The growth temperature of the N layer is 900℃, 950℃, 1000℃ or 1100℃, but not limited to these. The growth temperature of the ScyAlzGa1-y-zN / InN superlattice structure layer is 800℃, 850℃, 950℃ or 1000℃, but not limited to these. When the growth temperature is too high, Sc and In tend to diffuse outward. When the growth temperature is too low, the defect density increases.
[0037] The multi-quantum-well layer 6 comprises periodically alternating InGaN quantum well layers and AlGaN quantum barrier layers, with 6 to 12 periods. The InGaN quantum well layers are grown at 790℃ to 810℃ with a thickness of 2nm to 5nm, while the AlGaN quantum barrier layers are grown at 800℃ to 900℃ with a thickness of 5nm to 15nm. By controlling the growth temperature, period, and thickness of the multi-quantum-well layer 6, the overlap of electron and hole wave functions is significantly increased, thereby improving the luminous efficiency of the LED device.
[0038] In this process, buffer layer 2 consists of an AlN buffer layer and a GaN buffer layer stacked sequentially. The thickness of buffer layer 2 is 10 nm to 50 nm. The preparation step S210 of buffer layer 2 is as follows:
[0039] S211. An AlN buffer layer is sputtered on substrate 1 using a PVD sputtering process;
[0040] S212. The substrate 1 with the sputtered AlN buffer layer is transferred into the MOCVD equipment for H2 pretreatment and nitriding pretreatment. The atmosphere of H2 pretreatment is H2, the treatment temperature is 1000℃~1200℃, and the treatment time is 1min~10min.
[0041] S213. Deposit a GaN buffer layer on the treated AlN buffer layer.
[0042] The AlN buffer layer provides nucleation centers with the same orientation as substrate 1, releasing the stress caused by the lattice mismatch between the GaN epitaxial layer and substrate 1, as well as the thermal stress caused by the mismatch in the coefficient of thermal expansion. It provides a flat nucleation surface for further growth, reduces the contact angle of its nucleation growth, and enables the island-grown GaN grains to connect into a surface within a smaller thickness, transforming into two-dimensional epitaxial growth.
[0043] By sputtering an AlN buffer layer using PVD sputtering, a relatively thin and more compact AlN buffer layer can be formed. Subsequent H2 pretreatment and nitriding pretreatment promote the growth of the AlN buffer layer crystal quality, providing a high-quality growth platform for the subsequent growth of epitaxial layers.
[0044] Among them, see Figure 3 As shown, step S200 includes the following steps:
[0045] S210. Deposit buffer layer 2 on substrate 1;
[0046] S220. Deposit undoped GaN layer 3 on buffer layer 2:
[0047] The growth temperature of the undoped GaN layer 3 is 1050℃~1200℃, the growth pressure is 100torr~600torr, and the thickness is 1μm~5μm.
[0048] In this invention, the growth temperature of the undoped GaN layer 3 is relatively high and the pressure is relatively low, resulting in a GaN material layer with superior crystal quality. At the same time, as the GaN thickness increases, the compressive stress is released through stacking faults, reducing line defects, improving crystal quality, and reducing reverse leakage current. However, increasing the thickness of the undoped GaN layer 3 consumes a large amount of Ga source material, which greatly increases the epitaxial cost of LEDs. Therefore, when the thickness is controlled between 1μm and 5μm, it is possible to save production costs while ensuring that the undoped GaN layer 3 has high crystal quality.
[0049] S230. Deposit an N-type GaN layer 4 on the undoped GaN layer 3:
[0050] The N-type GaN layer 4 was grown at a temperature of 1050℃ to 1200℃, a growth pressure of 100 torr to 600 torr, a thickness of 2 μm to 3 μm, and a Si doping concentration of 1.0 × 10⁻⁶. 19 cm -3 ~5.0×10 19 cm -3 Sufficient thickness of the N-type GaN layer 4 can effectively release stress.
[0051] S240. Deposit stress-regulating layer 5 on N-type GaN layer 4:
[0052] S241. Deposit a first control layer 51 on the N-type GaN layer 4. The first control layer 51 is a Sc x Al 1-x N layers;
[0053] S242. Deposit a second control layer 52 on the first control layer 51. The second control layer 52 is Sc. y Al z Ga 1-y-z N / InN superlattice structure layer.
[0054] S250. A multi-quantum well layer 6 is deposited on the stress-controlled layer 5.
[0055] S260. Deposit an electron blocking layer 7 on the multi-quantum-well layer 6:
[0056] Electron blocking layer 7 is Al i In j Ga 1-i-j The N-layer has a thickness of 10 nm to 40 nm, a growth temperature of 900 °C to 1000 °C, a growth pressure of 100 torr to 300 torr, an Al content i of 0.1 > i > 0.05 with increasing Al content along the epitaxial direction, and an In content j of 0.2 > j > 0.01. The electron blocking layer 7 effectively restricts electron overflow and reduces hole blocking, improving hole injection efficiency into the multi-quantum-well layer 6, reducing Auger recombination of charge carriers, and increasing the luminous efficiency of the light-emitting diode.
[0057] S270. Deposit a P-type GaN layer 8 on the electron blocking layer 7:
[0058] The growth temperature of the p-type GaN layer 8 is 900℃~1050℃, the thickness is 10nm~50nm, the growth pressure is 100torr~600torr, and the Mg doping concentration is 1.0×10 19cm -3 ~1.0×10 21 cm -3 Excessive Mg doping concentration can compromise crystal quality, while insufficient doping concentration can affect hole concentration. Meanwhile, the higher growth temperature of the p-type GaN layer 8 is beneficial for merging V-shaped defects that easily occur during epitaxial layer growth, resulting in a smooth LED epitaxial wafer.
[0059] Secondly, the present invention also discloses a light-emitting diode epitaxial structure, which is prepared according to the above-described method for preparing a light-emitting diode epitaxial structure.
[0060] Furthermore, the present invention also discloses a light-emitting diode, comprising an epitaxial structure prepared by the above-described method for preparing an epitaxial structure of a light-emitting diode.
[0061] The present invention will be further described below with reference to the accompanying drawings and embodiments:
[0062] Example 1
[0063] This embodiment discloses a method for fabricating a light-emitting diode epitaxial structure, including:
[0064] S10. Provide a substrate;
[0065] S20. Sequentially deposit a buffer layer, an undoped GaN layer, an N-type GaN layer, a stress modulation layer, a multiple quantum well layer, an electron blocking layer, and a P-type GaN layer on the substrate.
[0066] The stress modulation layer comprises a first modulation layer and a second modulation layer deposited sequentially along the epitaxial direction. The first modulation layer is Sc. x Al 1-x N layers, the second control layer is Sc y Al z Ga 1-y-z N / InN superlattice structure layer.
[0067] In the first control layer, x is 0.1, and in the second control layer, y is 0.05 and z is 0.1.
[0068] Among them, Sc y Al z Ga 1-y-z The N / InN superlattice structure layers consist of periodically alternating stacks of Sc y Al z Ga 1-y-z The N sublayer and InN sublayer have a period of 6.
[0069] Among them, Sc x Al 1-x The thickness of the N layer is 45 nm, and the Sc layer... y Al zGa 1-y-z The thickness of the N sublayer is 230 nm, and the thickness of the InN sublayer is 3.2 nm.
[0070] Among them, Sc y Al z Ga 1-y-z The growth atmosphere of the N / InN superlattice structure layer is N2 / NH3, and the flow ratio of N2 to NH3 is 1:1.5.
[0071] Among them, Sc x Al 1-x The growth temperature of the N layer is 1000℃, Sc y Al z Ga 1-y-z The growth temperature of the N / InN superlattice structure layer is 890℃.
[0072] The multi-quantum-well layer includes periodically alternating InGaN quantum-well layers and AlGaN quantum-barrier layers, with 10 periods. The growth temperature of the InGaN quantum-well layer is 795℃, the thickness is 3.5nm, and the In content is 0.22%. The growth temperature of the AlGaN quantum-barrier layer is 855℃, the thickness is 9.8nm, and the Al content is 0.05%.
[0073] The buffer layer consists of an AlN buffer layer and a GaN buffer layer stacked sequentially. The preparation steps of the buffer layer are as follows:
[0074] An AlN buffer layer was sputtered onto the substrate using a PVD sputtering process.
[0075] The substrate with the sputtered AlN buffer layer was transferred into the MOCVD equipment for H2 pretreatment and nitriding pretreatment. The atmosphere for H2 pretreatment was H2, the treatment temperature was 1200℃, and the treatment time was 10 min.
[0076] The undoped GaN layer was grown at a temperature of 1100℃, a growth pressure of 150 torr, and a thickness of 3 μm.
[0077] The N-type GaN layer was grown at a temperature of 1120℃, a growth pressure of 100 torr, and a thickness of 3 μm. The Si doping concentration was 2.5 × 10⁻⁶. 19 cm -3 .
[0078] Among them, the electron blocking layer is Al i In j Ga 1-i-j The N layer has a thickness of 15 nm, a growth temperature of 965 °C, a growth pressure of 200 torr, and an Al content that increases from 0.01 to 0.05 along the epitaxial direction, while the In content is 0.01.
[0079] The p-type GaN layer was grown at a temperature of 985℃, with a thickness of 15 nm, a growth pressure of 200 torr, and a Mg doping concentration of 2.0 × 10⁻⁶. 20 cm -3 .
[0080] This embodiment also discloses a light-emitting diode epitaxial structure, which is prepared according to the above-described method for preparing a light-emitting diode epitaxial structure.
[0081] Example 2
[0082] This embodiment discloses a method for fabricating a light-emitting diode epitaxial structure, including:
[0083] S10. Provide a substrate;
[0084] S20. Sequentially deposit a buffer layer, an undoped GaN layer, an N-type GaN layer, a stress modulation layer, a multiple quantum well layer, an electron blocking layer, and a P-type GaN layer on the substrate.
[0085] The stress modulation layer comprises a first modulation layer and a second modulation layer deposited sequentially along the epitaxial direction. The first modulation layer is Sc. x Al 1-x N layers, the second control layer is Sc y Al z Ga 1-y-z N / InN superlattice structure layer.
[0086] In the first control layer, x is 0.1, and in the second control layer, y is 0.05 and z is 0.1.
[0087] Among them, Sc y Al z Ga 1-y-z The N / InN superlattice structure layers consist of periodically alternating stacks of Sc y Al z Ga 1-y-z The N sublayer and InN sublayer have a period of 6.
[0088] Among them, Sc x Al 1-x The thickness of the N layer is 65nm, Sc y Al z Ga 1-y-z The thickness of the N sublayer is 300 nm, and the thickness of the InN sublayer is 5 nm.
[0089] Among them, Sc y Al z Ga 1-y-zThe growth atmosphere of the N / InN superlattice structure layer is N2 / NH3, and the flow ratio of N2 to NH3 is 1:1.5.
[0090] Among them, Sc x Al 1-x The growth temperature of the N layer is 1000℃, Sc y Al z Ga 1-y-z The growth temperature of the N / InN superlattice structure layer is 890℃.
[0091] The multi-quantum-well layer includes periodically alternating InGaN quantum-well layers and AlGaN quantum-barrier layers, with 10 periods. The growth temperature of the InGaN quantum-well layer is 795℃, the thickness is 3.5nm, and the In content is 0.22%. The growth temperature of the AlGaN quantum-barrier layer is 855℃, the thickness is 9.8nm, and the Al content is 0.05%.
[0092] The buffer layer consists of an AlN buffer layer and a GaN buffer layer stacked sequentially. The preparation steps of the buffer layer are as follows:
[0093] An AlN buffer layer was sputtered onto the substrate using a PVD sputtering process.
[0094] The substrate with the sputtered AlN buffer layer was transferred into the MOCVD equipment for H2 pretreatment and nitriding pretreatment. The atmosphere for H2 pretreatment was H2, the treatment temperature was 1200℃, and the treatment time was 10 min.
[0095] The undoped GaN layer was grown at a temperature of 1100℃, a growth pressure of 150 torr, and a thickness of 3 μm.
[0096] The N-type GaN layer was grown at a temperature of 1120℃, a growth pressure of 100 torr, and a thickness of 3 μm. The Si doping concentration was 2.5 × 10⁻⁶. 19 cm -3 .
[0097] Among them, the electron blocking layer is Al i In j Ga 1-i-j The N layer has a thickness of 15 nm, a growth temperature of 965 °C, a growth pressure of 200 torr, and an Al content that increases from 0.01 to 0.05 along the epitaxial direction, while the In content is 0.01.
[0098] The p-type GaN layer was grown at a temperature of 985℃, with a thickness of 15 nm, a growth pressure of 200 torr, and a Mg doping concentration of 2.0 × 10⁻⁶. 20 cm -3 .
[0099] This embodiment also discloses a light-emitting diode epitaxial structure, which is prepared according to the above-described method for preparing a light-emitting diode epitaxial structure.
[0100] Example 3
[0101] This embodiment discloses a method for fabricating a light-emitting diode epitaxial structure, including:
[0102] S10. Provide a substrate;
[0103] S20. Sequentially deposit a buffer layer, an undoped GaN layer, an N-type GaN layer, a stress modulation layer, a multiple quantum well layer, an electron blocking layer, and a P-type GaN layer on the substrate.
[0104] The stress modulation layer comprises a first modulation layer and a second modulation layer deposited sequentially along the epitaxial direction. The first modulation layer is Sc. x Al 1-x N layers, the second control layer is Sc y Al z Ga 1-y-z N / InN superlattice structure layer.
[0105] In the first control layer, x is 0.1, and in the second control layer, y is 0.05 and z is 0.1.
[0106] Among them, Sc y Al z Ga 1-y-z The N / InN superlattice structure layers consist of periodically alternating stacks of Sc y Al z Ga 1-y-z The N sublayer and InN sublayer have a period of 6.
[0107] Among them, Sc x Al 1-x The thickness of the N layer is 25nm, Sc y Al z Ga 1-y-z The thickness of the N sublayer is 100 nm, and the thickness of the InN sublayer is 2 nm.
[0108] Among them, Sc y Al z Ga 1-y-z The growth atmosphere of the N / InN superlattice structure layer is N2 / NH3, and the flow ratio of N2 to NH3 is 1:1.5.
[0109] Among them, Sc x Al 1-x The growth temperature of the N layer is 1000℃, Sc y Al z Ga1-y-z The growth temperature of the N / InN superlattice structure layer is 890℃.
[0110] The multi-quantum-well layer includes periodically alternating InGaN quantum-well layers and AlGaN quantum-barrier layers, with 10 periods. The growth temperature of the InGaN quantum-well layer is 795℃, the thickness is 3.5nm, and the In content is 0.22%. The growth temperature of the AlGaN quantum-barrier layer is 855℃, the thickness is 9.8nm, and the Al content is 0.05%.
[0111] The buffer layer consists of an AlN buffer layer and a GaN buffer layer stacked sequentially. The preparation steps of the buffer layer are as follows:
[0112] An AlN buffer layer was sputtered onto the substrate using a PVD sputtering process.
[0113] The substrate with the sputtered AlN buffer layer was transferred into the MOCVD equipment for H2 pretreatment and nitriding pretreatment. The atmosphere for H2 pretreatment was H2, the treatment temperature was 1200℃, and the treatment time was 10 min.
[0114] The undoped GaN layer was grown at a temperature of 1100℃, a growth pressure of 150 torr, and a thickness of 3 μm.
[0115] The N-type GaN layer was grown at a temperature of 1120℃, a growth pressure of 100 torr, and a thickness of 3 μm. The Si doping concentration was 2.5 × 10⁻⁶. 19 cm -3 .
[0116] Among them, the electron blocking layer is Al i In j Ga 1-i-j The N layer has a thickness of 15 nm, a growth temperature of 965 °C, a growth pressure of 200 torr, and an Al content that increases from 0.01 to 0.05 along the epitaxial direction, while the In content is 0.01.
[0117] The p-type GaN layer was grown at a temperature of 985℃, with a thickness of 15 nm, a growth pressure of 200 torr, and a Mg doping concentration of 2.0 × 10⁻⁶. 20 cm -3 .
[0118] This embodiment also discloses a light-emitting diode epitaxial structure, which is prepared according to the above-described method for preparing a light-emitting diode epitaxial structure.
[0119] Example 4
[0120] This embodiment discloses a method for fabricating a light-emitting diode epitaxial structure, including:
[0121] S10. Provide a substrate;
[0122] S20. Sequentially deposit a buffer layer, an undoped GaN layer, an N-type GaN layer, a stress modulation layer, a multiple quantum well layer, an electron blocking layer, and a P-type GaN layer on the substrate.
[0123] The stress modulation layer comprises a first modulation layer and a second modulation layer deposited sequentially along the epitaxial direction. The first modulation layer is Sc. x Al 1-x N layers, the second control layer is Sc y Al z Ga 1-y-z N / InN superlattice structure layer.
[0124] In the first control layer, x is 0.3, and in the second control layer, y is 0.05 and z is 0.1.
[0125] Among them, Sc y Al z Ga 1-y-z The N / InN superlattice structure layers consist of periodically alternating stacks of Sc y Al z Ga 1-y-z The N sublayer and InN sublayer have a period of 6.
[0126] Among them, Sc x Al 1-x The thickness of the N layer is 45 nm, and the Sc layer... y Al z Ga 1-y-z The thickness of the N sublayer is 230 nm, and the thickness of the InN sublayer is 3.2 nm.
[0127] Among them, Sc y Al z Ga 1-y-z The growth atmosphere of the N / InN superlattice structure layer is N2 / NH3, and the flow ratio of N2 to NH3 is 1:1.5.
[0128] Among them, Sc x Al 1-x The growth temperature of the N layer is 1000℃, Sc y Al z Ga 1-y-z The growth temperature of the N / InN superlattice structure layer is 890℃.
[0129] The multi-quantum-well layer includes periodically alternating InGaN quantum-well layers and AlGaN quantum-barrier layers, with 10 periods. The growth temperature of the InGaN quantum-well layer is 795℃, the thickness is 3.5nm, and the In content is 0.22%. The growth temperature of the AlGaN quantum-barrier layer is 855℃, the thickness is 9.8nm, and the Al content is 0.05%.
[0130] The buffer layer consists of an AlN buffer layer and a GaN buffer layer stacked sequentially. The preparation steps of the buffer layer are as follows:
[0131] An AlN buffer layer was sputtered onto the substrate using a PVD sputtering process.
[0132] The substrate with the sputtered AlN buffer layer was transferred into the MOCVD equipment for H2 pretreatment and nitriding pretreatment. The atmosphere for H2 pretreatment was H2, the treatment temperature was 1200℃, and the treatment time was 10 min.
[0133] The undoped GaN layer was grown at a temperature of 1100℃, a growth pressure of 150 torr, and a thickness of 3 μm.
[0134] The N-type GaN layer was grown at a temperature of 1120℃, a growth pressure of 100 torr, and a thickness of 3 μm. The Si doping concentration was 2.5 × 10⁻⁶. 19 cm -3 .
[0135] Among them, the electron blocking layer is Al i In j Ga 1-i-j The N layer has a thickness of 15 nm, a growth temperature of 965 °C, a growth pressure of 200 torr, and an Al content that increases from 0.01 to 0.05 along the epitaxial direction, while the In content is 0.01.
[0136] The p-type GaN layer was grown at a temperature of 985℃, with a thickness of 15 nm, a growth pressure of 200 torr, and a Mg doping concentration of 2.0 × 10⁻⁶. 20 cm -3 .
[0137] This embodiment also discloses a light-emitting diode epitaxial structure, which is prepared according to the above-described method for preparing a light-emitting diode epitaxial structure.
[0138] Example 5
[0139] This embodiment discloses a method for fabricating a light-emitting diode epitaxial structure, including:
[0140] S10. Provide a substrate;
[0141] S20. Sequentially deposit a buffer layer, an undoped GaN layer, an N-type GaN layer, a stress modulation layer, a multiple quantum well layer, an electron blocking layer, and a P-type GaN layer on the substrate.
[0142] The stress modulation layer comprises a first modulation layer and a second modulation layer deposited sequentially along the epitaxial direction. The first modulation layer is Sc. x Al 1-x N layers, the second control layer is Sc y Al z Ga 1-y-z N / InN superlattice structure layer.
[0143] In the first control layer, x is 0.05, and in the second control layer, y is 0.05 and z is 0.1.
[0144] Among them, Sc y Al z Ga 1-y-z The N / InN superlattice structure layers consist of periodically alternating stacks of Sc y Al z Ga 1-y-z The N sublayer and InN sublayer have a period of 6.
[0145] Among them, Sc x Al 1-x The thickness of the N layer is 45 nm, and the Sc layer... y Al z Ga 1-y-z The thickness of the N sublayer is 230 nm, and the thickness of the InN sublayer is 3.2 nm.
[0146] Among them, Sc y Al z Ga 1-y-z The growth atmosphere of the N / InN superlattice structure layer is N2 / NH3, and the flow ratio of N2 to NH3 is 1:1.5.
[0147] Among them, Sc x Al 1-x The growth temperature of the N layer is 1000℃, Sc y Al z Ga 1-y-z The growth temperature of the N / InN superlattice structure layer is 890℃.
[0148] The multi-quantum-well layer includes periodically alternating InGaN quantum-well layers and AlGaN quantum-barrier layers, with 10 periods. The growth temperature of the InGaN quantum-well layer is 795℃, the thickness is 3.5nm, and the In content is 0.22%. The growth temperature of the AlGaN quantum-barrier layer is 855℃, the thickness is 9.8nm, and the Al content is 0.05%.
[0149] The buffer layer consists of an AlN buffer layer and a GaN buffer layer stacked sequentially. The preparation steps of the buffer layer are as follows:
[0150] An AlN buffer layer was sputtered onto the substrate using a PVD sputtering process.
[0151] The substrate with the sputtered AlN buffer layer was transferred into the MOCVD equipment for H2 pretreatment and nitriding pretreatment. The atmosphere for H2 pretreatment was H2, the treatment temperature was 1200℃, and the treatment time was 10 min.
[0152] The undoped GaN layer was grown at a temperature of 1100℃, a growth pressure of 150 torr, and a thickness of 3 μm.
[0153] The N-type GaN layer was grown at a temperature of 1120℃, a growth pressure of 100 torr, and a thickness of 3 μm. The Si doping concentration was 2.5 × 10⁻⁶. 19 cm -3 .
[0154] Among them, the electron blocking layer is Al i In j Ga 1-i-j The N layer has a thickness of 15 nm, a growth temperature of 965 °C, a growth pressure of 200 torr, and an Al content that increases from 0.01 to 0.05 along the epitaxial direction, while the In content is 0.01.
[0155] The p-type GaN layer was grown at a temperature of 985℃, with a thickness of 15 nm, a growth pressure of 200 torr, and a Mg doping concentration of 2.0 × 10⁻⁶. 20 cm -3 .
[0156] This embodiment also discloses a light-emitting diode epitaxial structure, which is prepared according to the above-described method for preparing a light-emitting diode epitaxial structure.
[0157] Example 6
[0158] This embodiment discloses a method for fabricating a light-emitting diode epitaxial structure, including:
[0159] S10. Provide a substrate;
[0160] S20. Sequentially deposit a buffer layer, an undoped GaN layer, an N-type GaN layer, a stress modulation layer, a multiple quantum well layer, an electron blocking layer, and a P-type GaN layer on the substrate.
[0161] The stress modulation layer comprises a first modulation layer and a second modulation layer deposited sequentially along the epitaxial direction. The first modulation layer is Sc. x Al 1-xN layers, the second control layer is Sc y Al z Ga 1-y-z N / InN superlattice structure layer.
[0162] In the first control layer, x is 0.1, and in the second control layer, y is 0.08 and z is 0.3.
[0163] Among them, Sc y Al z Ga 1-y-z The N / InN superlattice structure layers consist of periodically alternating stacks of Sc y Al z Ga 1-y-z The N sublayer and InN sublayer have a period of 6.
[0164] Among them, Sc x Al 1-x The thickness of the N layer is 45 nm, and the Sc layer... y Al z Ga 1-y-z The thickness of the N sublayer is 230 nm, and the thickness of the InN sublayer is 3.2 nm.
[0165] Among them, Sc y Al z Ga 1-y-z The growth atmosphere of the N / InN superlattice structure layer is N2 / NH3, and the flow ratio of N2 to NH3 is 1:1.5.
[0166] Among them, Sc x Al 1-x The growth temperature of the N layer is 1000℃, Sc y Al z Ga 1-y-z The growth temperature of the N / InN superlattice structure layer is 890℃.
[0167] The multi-quantum-well layer includes periodically alternating InGaN quantum-well layers and AlGaN quantum-barrier layers, with 10 periods. The growth temperature of the InGaN quantum-well layer is 795℃, the thickness is 3.5nm, and the In content is 0.22%. The growth temperature of the AlGaN quantum-barrier layer is 855℃, the thickness is 9.8nm, and the Al content is 0.05%.
[0168] The buffer layer consists of an AlN buffer layer and a GaN buffer layer stacked sequentially. The preparation steps of the buffer layer are as follows:
[0169] An AlN buffer layer was sputtered onto the substrate using a PVD sputtering process.
[0170] The substrate with the sputtered AlN buffer layer was transferred into the MOCVD equipment for H2 pretreatment and nitriding pretreatment. The atmosphere for H2 pretreatment was H2, the treatment temperature was 1200℃, and the treatment time was 10 min.
[0171] The undoped GaN layer was grown at a temperature of 1100℃, a growth pressure of 150 torr, and a thickness of 3 μm.
[0172] The N-type GaN layer was grown at a temperature of 1120℃, a growth pressure of 100 torr, and a thickness of 3 μm. The Si doping concentration was 2.5 × 10⁻⁶. 19 cm -3 .
[0173] Among them, the electron blocking layer is Al i In j Ga 1-i-j The N layer has a thickness of 15 nm, a growth temperature of 965 °C, a growth pressure of 200 torr, and an Al content that increases from 0.01 to 0.05 along the epitaxial direction, while the In content is 0.01.
[0174] The p-type GaN layer was grown at a temperature of 985℃, with a thickness of 15 nm, a growth pressure of 200 torr, and a Mg doping concentration of 2.0 × 10⁻⁶. 20 cm -3 .
[0175] This embodiment also discloses a light-emitting diode epitaxial structure, which is prepared according to the above-described method for preparing a light-emitting diode epitaxial structure.
[0176] Example 7
[0177] This embodiment discloses a method for fabricating a light-emitting diode epitaxial structure, including:
[0178] S10. Provide a substrate;
[0179] S20. Sequentially deposit a buffer layer, an undoped GaN layer, an N-type GaN layer, a stress modulation layer, a multiple quantum well layer, an electron blocking layer, and a P-type GaN layer on the substrate.
[0180] The stress modulation layer comprises a first modulation layer and a second modulation layer deposited sequentially along the epitaxial direction. The first modulation layer is Sc. x Al 1-x N layers, the second control layer is Sc y Al z Ga 1-y-z N / InN superlattice structure layer.
[0181] In the first control layer, x is 0.1, and in the second control layer, y is 0.03 and z is 0.6.
[0182] Among them, Sc y Al z Ga 1-y-z The N / InN superlattice structure layers consist of periodically alternating stacks of Sc y Al z Ga 1-y-z The N sublayer and the InN sublayer have a period of 6.
[0183] Among them, Sc x Al 1-x The thickness of the N layer is 45 nm, Sc y Al z Ga 1-y-z The thickness of the N sublayer is 230 nm, and the thickness of the InN sublayer is 3.2 nm.
[0184] Among them, Sc y Al z Ga 1-y-z The growth atmosphere of the N / InN superlattice structure layer is N2 / NH3, and the flow ratio of N2 to NH3 is 1:1.5.
[0185] Among them, Sc x Al 1-x The growth temperature of the N layer is 1000℃, and the Sc layer... y Al z Ga 1-y-z The growth temperature of the N / InN superlattice structure layer is 890℃.
[0186] The multi-quantum-well layer includes periodically alternating InGaN quantum-well layers and AlGaN quantum-barrier layers, with 10 periods. The growth temperature of the InGaN quantum-well layer is 795℃, the thickness is 3.5nm, and the In content is 0.22%. The growth temperature of the AlGaN quantum-barrier layer is 855℃, the thickness is 9.8nm, and the Al content is 0.05%.
[0187] The buffer layer consists of an AlN buffer layer and a GaN buffer layer stacked sequentially. The preparation steps of the buffer layer are as follows:
[0188] An AlN buffer layer was sputtered onto the substrate using a PVD sputtering process.
[0189] The substrate with the sputtered AlN buffer layer was transferred into the MOCVD equipment for H2 pretreatment and nitriding pretreatment. The atmosphere for H2 pretreatment was H2, the treatment temperature was 1200℃, and the treatment time was 10 min.
[0190] The undoped GaN layer was grown at a temperature of 1100℃, a growth pressure of 150 torr, and a thickness of 3 μm.
[0191] The N-type GaN layer was grown at a temperature of 1120℃, a growth pressure of 100 torr, and a thickness of 3 μm. The Si doping concentration was 2.5 × 10⁻⁶. 19 cm -3 .
[0192] Among them, the electron blocking layer is Al i In j Ga 1-i-j The N layer has a thickness of 15 nm, a growth temperature of 965 °C, a growth pressure of 200 torr, and an Al content that increases from 0.01 to 0.05 along the epitaxial direction, while the In content is 0.01.
[0193] The p-type GaN layer was grown at a temperature of 985℃, with a thickness of 15 nm, a growth pressure of 200 torr, and a Mg doping concentration of 2.0 × 10⁻⁶. 20 cm -3 .
[0194] This embodiment also discloses a light-emitting diode epitaxial structure, which is prepared according to the above-described method for preparing a light-emitting diode epitaxial structure.
[0195] Example 8
[0196] This embodiment discloses a method for fabricating a light-emitting diode epitaxial structure, including:
[0197] S10. Provide a substrate;
[0198] S20. Sequentially deposit a buffer layer, an undoped GaN layer, an N-type GaN layer, a stress modulation layer, a multiple quantum well layer, an electron blocking layer, and a P-type GaN layer on the substrate.
[0199] The stress modulation layer comprises a first modulation layer and a second modulation layer deposited sequentially along the epitaxial direction. The first modulation layer is Sc. x Al 1-x N layers, the second control layer is Sc y Al z Ga 1-y-z N / InN superlattice structure layer.
[0200] In the first control layer, x is 0.1, and in the second control layer, y is 0.05 and z is 0.1.
[0201] Among them, Sc y Al z Ga 1-y-z The N / InN superlattice structure layers consist of periodically alternating stacks of Sc y Al z Ga 1-y-zThe N sublayer and InN sublayer have 8 cycles.
[0202] Among them, Sc x Al 1-x The thickness of the N layer is 45 nm, and the Sc layer... y Al z Ga 1-y-z The thickness of the N sublayer is 230 nm, and the thickness of the InN sublayer is 3.2 nm.
[0203] Among them, Sc y Al z Ga 1-y-z The growth atmosphere of the N / InN superlattice structure layer is N2 / NH3, and the flow ratio of N2 to NH3 is 1:1.5.
[0204] Among them, Sc x Al 1-x The growth temperature of the N layer is 1000℃, Sc y Al z Ga 1-y-z The growth temperature of the N / InN superlattice structure layer is 890℃.
[0205] The multi-quantum-well layer includes periodically alternating InGaN quantum-well layers and AlGaN quantum-barrier layers, with 10 periods. The growth temperature of the InGaN quantum-well layer is 795℃, the thickness is 3.5nm, and the In content is 0.22%. The growth temperature of the AlGaN quantum-barrier layer is 855℃, the thickness is 9.8nm, and the Al content is 0.05%.
[0206] The buffer layer consists of an AlN buffer layer and a GaN buffer layer stacked sequentially. The preparation steps of the buffer layer are as follows:
[0207] An AlN buffer layer was sputtered onto the substrate using a PVD sputtering process.
[0208] The substrate with the sputtered AlN buffer layer was transferred into the MOCVD equipment for H2 pretreatment and nitriding pretreatment. The atmosphere for H2 pretreatment was H2, the treatment temperature was 1200℃, and the treatment time was 10 min.
[0209] The undoped GaN layer was grown at a temperature of 1100℃, a growth pressure of 150 torr, and a thickness of 3 μm.
[0210] The N-type GaN layer was grown at a temperature of 1120℃, a growth pressure of 100 torr, and a thickness of 3 μm. The Si doping concentration was 2.5 × 10⁻⁶. 19 cm -3 .
[0211] Among them, the electron blocking layer is Ali In j Ga 1-i-j The N layer has a thickness of 15 nm, a growth temperature of 965 °C, a growth pressure of 200 torr, and an Al content that increases from 0.01 to 0.05 along the epitaxial direction, while the In content is 0.01.
[0212] The p-type GaN layer was grown at a temperature of 985℃, with a thickness of 15 nm, a growth pressure of 200 torr, and a Mg doping concentration of 2.0 × 10⁻⁶. 20 cm -3 .
[0213] This embodiment also discloses a light-emitting diode epitaxial structure, which is prepared according to the above-described method for preparing a light-emitting diode epitaxial structure.
[0214] Example 9
[0215] This embodiment discloses a method for fabricating a light-emitting diode epitaxial structure, including:
[0216] S10. Provide a substrate;
[0217] S20. Sequentially deposit a buffer layer, an undoped GaN layer, an N-type GaN layer, a stress modulation layer, a multiple quantum well layer, an electron blocking layer, and a P-type GaN layer on the substrate.
[0218] The stress modulation layer comprises a first modulation layer and a second modulation layer deposited sequentially along the epitaxial direction. The first modulation layer is Sc. x Al 1-x N layers, the second control layer is Sc y Al z Ga 1-y-z N / InN superlattice structure layer.
[0219] In the first control layer, x is 0.1, and in the second control layer, y is 0.05 and z is 0.1.
[0220] Among them, Sc y Al z Ga 1-y-z The N / InN superlattice structure layers consist of periodically alternating stacks of Sc y Al z Ga 1-y-z The N sublayer and the InN sublayer have a period of 4.
[0221] Among them, Sc x Al 1-x The thickness of the N layer is 45 nm, and the Sc layer... y Al z Ga 1-y-zThe thickness of the N sublayer is 230 nm, and the thickness of the InN sublayer is 3.2 nm.
[0222] Among them, Sc y Al z Ga 1-y-z The growth atmosphere of the N / InN superlattice structure layer is N2 / NH3, and the flow ratio of N2 to NH3 is 1:1.5.
[0223] Among them, Sc x Al 1-x The growth temperature of the N layer is 1000℃, and the Sc layer... y Al z Ga 1-y-z The growth temperature of the N / InN superlattice structure layer is 890℃.
[0224] The multi-quantum-well layer includes periodically alternating InGaN quantum-well layers and AlGaN quantum-barrier layers, with 10 periods. The growth temperature of the InGaN quantum-well layer is 795℃, the thickness is 3.5nm, and the In content is 0.22%. The growth temperature of the AlGaN quantum-barrier layer is 855℃, the thickness is 9.8nm, and the Al content is 0.05%.
[0225] The buffer layer consists of an AlN buffer layer and a GaN buffer layer stacked sequentially. The preparation steps of the buffer layer are as follows:
[0226] An AlN buffer layer was sputtered onto the substrate using a PVD sputtering process.
[0227] The substrate with the sputtered AlN buffer layer was transferred into the MOCVD equipment for H2 pretreatment and nitriding pretreatment. The atmosphere for H2 pretreatment was H2, the treatment temperature was 1200℃, and the treatment time was 10 min.
[0228] The undoped GaN layer was grown at a temperature of 1100℃, a growth pressure of 150 torr, and a thickness of 3 μm.
[0229] The N-type GaN layer was grown at a temperature of 1120℃, a growth pressure of 100 torr, and a thickness of 3 μm. The Si doping concentration was 2.5 × 10⁻⁶. 19 cm -3 .
[0230] Among them, the electron blocking layer is Al i In j Ga 1-i-j The N layer has a thickness of 15 nm, a growth temperature of 965 °C, a growth pressure of 200 torr, and an Al content that increases from 0.01 to 0.05 along the epitaxial direction, while the In content is 0.01.
[0231] The p-type GaN layer was grown at a temperature of 985℃, with a thickness of 15 nm, a growth pressure of 200 torr, and a Mg doping concentration of 2.0 × 10⁻⁶. 20 cm -3 .
[0232] This embodiment also discloses a light-emitting diode epitaxial structure, which is prepared according to the above-described method for preparing a light-emitting diode epitaxial structure.
[0233] Comparative Example 1
[0234] The difference between this embodiment and Embodiment 1 is that the stress regulation layer of the light-emitting diode epitaxial structure in this embodiment does not contain a first regulation layer.
[0235] Specifically, this comparative example discloses a method for fabricating a light-emitting diode epitaxial structure, including:
[0236] S10. Provide a substrate;
[0237] S20. Sequentially deposit a buffer layer, an undoped GaN layer, an N-type GaN layer, a stress modulation layer, a multiple quantum well layer, an electron blocking layer, and a P-type GaN layer on the substrate.
[0238] The stress modulation layer consists only of the second modulation layer, which is Sc. y Al z Ga 1-y-z N / InN superlattice structure layer.
[0239] Comparative Example 2
[0240] The difference between this embodiment and Embodiment 1 is that the stress regulation layer of the light-emitting diode epitaxial structure in this embodiment does not contain a second regulation layer.
[0241] Specifically, this comparative example discloses a method for fabricating a light-emitting diode epitaxial structure, including:
[0242] S10. Provide a substrate;
[0243] S20. Sequentially deposit a buffer layer, an undoped GaN layer, an N-type GaN layer, a stress modulation layer, a multiple quantum well layer, an electron blocking layer, and a P-type GaN layer on the substrate.
[0244] The stress regulation layer consists only of the first regulation layer, which is Sc. x Al 1-x N layers.
[0245] Comparative Example 3
[0246] The difference between this comparative example and Example 1 is that the epitaxial structure of the light-emitting diode in this example does not contain a stress-regulating layer.
[0247] Specifically, this comparative example discloses a method for fabricating a light-emitting diode epitaxial structure, including:
[0248] S10. Provide a substrate;
[0249] S20. Sequentially deposit a buffer layer, an undoped GaN layer, an N-type GaN layer, a multiple quantum well layer, an electron blocking layer, and a P-type GaN layer on the substrate.
[0250] (I) Luminous efficacy improvement rate test
[0251] Test method: The epitaxial structures of Examples 1 to 9 and Comparative Examples 1 to 3 were fabricated into chips of 10mil*24mil. 300 LED chips were randomly selected from each experimental group and tested at 120mA / 60mA current to obtain the luminous efficacy improvement rate of Examples 1 to 9 and Comparative Examples 1 to 2 compared with Comparative Example 3.
[0252] The test results are as follows:
[0253]
[0254]
[0255] Experimental results show that the stress regulation layer of the present invention can effectively improve luminous efficiency through the cooperation between the first regulation layer and the second regulation layer.
[0256] (II) Surface roughness and curvature test
[0257] Test methods: According to the preparation methods of Example 1, Comparative Example 1 and Comparative Example 2, a buffer layer, an undoped GaN layer, an N-type GaN layer, a stress modulation layer and a multiple quantum well layer were sequentially deposited on the substrate to prepare samples. According to the preparation method of Comparative Example 3, a buffer layer, an undoped GaN layer, an N-type GaN layer and a multiple quantum well layer were sequentially deposited on the substrate to prepare samples. Fifty samples from each experimental group were taken and their surface roughness and curvature were tested to obtain the average surface roughness and average curvature.
[0258] The test results are as follows:
[0259] experimental group Average surface roughness / nm Average curvature / μm Example 1 0.45 1.1 Comparative Example 1 0.6 1.45 Comparative Example 2 0.75 1.65 Comparative Example 3 0.8 1.7
[0260] Experimental results show that, compared with the comparative example, the epitaxial wafer of the present invention has a smooth surface, no cracks, low curvature, and the stress accumulated in the epitaxial layer is released.
[0261] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art can make some modifications or alterations to the above-described technical content to create equivalent embodiments without departing from the scope of the present invention. Any simple modifications, equivalent changes, and alterations made to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention shall still fall within the scope of the present invention.
Claims
1. A method for fabricating an epitaxial structure of a light-emitting diode, characterized in that, include: Provide substrate; A buffer layer, an undoped GaN layer, an N-type GaN layer, a stress modulation layer, a multiple quantum well layer, an electron blocking layer, and a P-type GaN layer are sequentially deposited on the substrate. The stress regulation layer comprises a first regulation layer and a second regulation layer deposited sequentially along the epitaxial direction, wherein the first regulation layer is Sc. x Al 1-x N layers, the second control layer is Sc y Al z Ga 1-y-z N / InN superlattice structure layer; The Sc y Al z Ga 1-y-z The N / InN superlattice structure layers consist of periodically alternating stacks of Sc y Al z Ga 1-y-z The N sublayer and InN sublayer have 2 to 20 cycles. The Sc x Al 1-x The thickness of the N layer is 1nm~100nm, and the Sc y Al z Ga 1-y-z The thickness of the N sublayer is 5nm~500nm, and the thickness of the InN sublayer is 0.5nm~10nm.
2. The method for fabricating a light-emitting diode epitaxial structure according to claim 1, characterized in that, In the first control layer, 0.5 ≥ x ≥ 0.01; in the second control layer, 0.1 ≥ y ≥ 0.01, and 0.5 ≥ z ≥ 0.
01.
3. The method for fabricating a light-emitting diode epitaxial structure according to claim 1, characterized in that, The Sc y Al z Ga 1-y-z The growth atmosphere of the N / InN superlattice structure layer is N2 / NH3, and the flow ratio between N2 and NH3 is 1:(0.1~10).
4. The method for fabricating a light-emitting diode epitaxial structure according to claim 1, characterized in that, The Sc x Al 1-x The growth temperature of the N layer is 900℃~1100℃, and the Sc y Al z Ga 1-y-z The growth temperature of the N / InN superlattice structure layer is 800℃~1000℃.
5. The method for fabricating a light-emitting diode epitaxial structure according to claim 1, characterized in that, The multiple quantum well layer comprises periodically alternating InGaN quantum well layers and AlGaN quantum barrier layers, with 6 to 12 periods. The growth temperature of the InGaN quantum well layer is 790℃ to 810℃, and the thickness is 2nm to 5nm. The growth temperature of the AlGaN quantum barrier layer is 800℃ to 900℃, and the thickness is 5nm to 15nm.
6. The method for fabricating a light-emitting diode epitaxial structure according to claim 1, characterized in that, The buffer layer consists of an AlN buffer layer and a GaN buffer layer stacked sequentially. The preparation steps of the buffer layer are as follows: An AlN buffer layer was sputtered onto the substrate using a PVD sputtering process. The substrate with the sputtered AlN buffer layer was transferred into the MOCVD equipment for H2 pretreatment and nitriding pretreatment. The atmosphere for H2 pretreatment was H2, the treatment temperature was 1000℃~1200℃, and the treatment time was 1min~10min.
7. A light-emitting diode epitaxial structure, characterized in that, It is prepared by the method for preparing the epitaxial structure of a light-emitting diode according to any one of claims 1 to 6.
8. A light-emitting diode, characterized in that, The epitaxial structure includes the epitaxial structure prepared by the method for preparing a light-emitting diode epitaxial structure according to any one of claims 1 to 6.
Citation Information
Patent Citations
LED substrate structure and production method thereof
CN104201270A
Flip-chip optical semiconductor element
JP1999340514A