Light emitting diode epitaxial wafer and preparation method thereof, and light emitting diode
By fabricating MoSe₂ islands and periodic V-pit layers in GaN-based light-emitting diodes, optimizing V-pit distribution and hole injection, the problem of V-pit inhomogeneity was solved, and the luminous efficiency and wavelength uniformity were improved.
Patent Information
- Application Number
- CN202310769690.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-28
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-06-28
AI Technical Summary
In existing GaN-based light-emitting diodes, the V-pits are unevenly distributed and the aperture size is small, which affects the luminous efficiency and wavelength uniformity.
MoSe₂ islands were fabricated on N-type GaN layers and GaN fill layers were grown to form pores. Subsequently, periodic V-pit layers and multiple quantum well layers, including InGaN and AlGaN layers, were grown to optimize the V-pit distribution and hole injection probability.
By optimizing the V-pit distribution and hole injection, the luminous efficiency and wavelength uniformity of the light-emitting diodes were significantly improved.
Smart Images

Figure CN116632136B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of semiconductor optoelectronic devices, and more particularly to a light-emitting diode epitaxial wafer and its fabrication method, and a light-emitting diode. Background Technology
[0002] In GaN-based light-emitting diodes (LEDs), dislocations are generated due to lattice and thermal mismatches between the GaN material and the substrate. These dislocations penetrate into the multi-quantum-well active region, forming V-shaped defects (V-pits). Studies have shown that V-pits can shield dislocations, and holes can also be injected into the multi-quantum-well active region from the sidewalls of the V-pits, improving luminous efficiency. However, existing V-pits have poor uniformity in distribution, relatively small opening sizes, and narrow hole channels, limiting their effect on improving luminous efficiency and affecting the wavelength uniformity of the LED. Summary of the Invention
[0003] The technical problem to be solved by the present invention is to provide an epitaxial wafer for a light-emitting diode and a method for preparing the same, which can improve the luminous efficiency and wavelength uniformity of the light-emitting diode.
[0004] Another technical problem that this invention aims to solve is to provide a light-emitting diode with high luminous efficiency.
[0005] To address the above problems, this invention discloses a light-emitting diode epitaxial wafer, which includes a substrate, and a buffer layer, an undoped GaN layer, an N-type GaN layer, a V-pit preparation layer, a V-pit layer, a multiple quantum well layer, an electron blocking layer, and a P-type GaN layer sequentially stacked on the substrate. The V-pit preparation layer includes a template layer, a GaN filler layer, and a first AlGaN layer stacked sequentially on the N-type GaN layer; the template layer includes multiple MoSe2 islands distributed in an array on the N-type GaN layer, and the thickness of the GaN filler layer is slightly greater than the height of the MoSe2 islands, so that after the GaN filler layer grows, a hole is formed on the top of the MoSe2 island; The V-pit layer has a periodic structure with 3 to 10 periods, and each period of the V-pit layer includes sequentially stacked In layers. x Ga 1-x The N-layer and the first GaN layer, where x is 0.22~0.3.
[0006] As an improvement to the above technical solution, the height of the MoSe2 island is 30nm~80nm, and the width of the MoSe2 island is 80nm~200nm; The thickness of the GaN filler layer is 40nm~100nm, and the thickness of the first AlGaN layer is 20nm~100nm; The In x Ga 1-xThe thickness of the N layer is 2nm~5nm, and the thickness of the first GaN layer is 10nm~30nm.
[0007] As an improvement to the above technical solution, the template layer is prepared by growing a MoO3 layer on the N-type GaN layer, annealing it in an oxygen-containing atmosphere at 500℃~600℃ for 10min~30min, and then selenizing it in an atmosphere containing a selenium source at 600℃~700℃ for 30min~60min to obtain multiple MoSe2 islands.
[0008] As an improvement to the above technical solution, the V-pit layer forms multiple V-pits, and the distribution density of the V-pits is 5×10⁻⁶. 6 cm -2 ~6×10 7 cm -2 The first opening radius of the V-shaped pit is 60nm~120nm, and the second opening radius is 100nm~160nm; Wherein, the first opening radius is the radius of the V-pit after the V-pit layer is grown, and the second opening radius is the radius of the V-pit after the multi-quantum-well layer is grown.
[0009] As an improvement to the above technical solution, the multi-quantum well layer includes a first multi-quantum well layer and a second multi-quantum well layer sequentially stacked on the V-pit layer; The first multiple quantum well layer has a periodic structure with 2 to 8 periods. Each period of the first multiple quantum well layer includes sequentially stacked In... y Ga 1-y The N-layer and the second GaN-layer, where y is 0.25~0.4; The second multiple quantum well layer has a periodic structure with a period number of 1 to 5. Each period of the second multiple quantum well layer includes sequentially stacked In... z Ga 1-z The BGaN layer and the second AlGaN layer are co-doped with N and C and Mg, respectively, wherein z is 0.3~0.4. The V-pit layer forms multiple V-pits, and the second opening radius of the V-pit is 45nm~65nm larger than the first opening radius of the V-pit; Wherein, the first opening radius is the radius of the V-pit after the V-pit layer is grown, and the second opening radius is the radius of the V-pit after the multi-quantum-well layer is grown.
[0010] As an improvement to the above technical solution, the In y Ga 1-y The thickness of the N layer is 2nm~10nm, and the thickness of the second GaN layer is 5nm~15nm; The In z Ga1-z The thickness of the N layer is 2nm~10nm, the thickness of the C and Mg co-doped BGaN layer is 5nm~10nm, and the thickness of the second AlGaN layer is 5nm~10nm; The C doping concentration in the C and Mg co-doped BGaN layer is 1×10⁻⁶. 17 cm -3 ~5×10 17 cm -3 The Mg doping concentration is 2 × 10⁻⁶. 18 cm -3 ~5×10 19 cm -3 .
[0011] Accordingly, the present invention also discloses a method for preparing a light-emitting diode epitaxial wafer, which includes: A substrate is provided on which a buffer layer, an undoped GaN layer, an N-type GaN layer, a V-pit preparation layer, a V-pit layer, a multiple quantum well layer, an electron blocking layer and a P-type GaN layer are sequentially grown. The V-pit preparation layer includes a template layer, a GaN filler layer, and a first AlGaN layer stacked sequentially on the N-type GaN layer; the template layer includes multiple MoSe2 islands distributed in an array on the N-type GaN layer, and the thickness of the GaN filler layer is slightly greater than the height of the MoSe2 islands, so that after the GaN filler layer grows, a hole is formed on the top of the MoSe2 island; The V-pit layer has a periodic structure with 3 to 10 periods, and each period of the V-pit layer includes sequentially stacked In layers. x Ga 1-x The N-layer and the first GaN layer, where x is 0.22~0.3.
[0012] As an improvement to the above technical solution, the template layer is prepared by growing a MoO3 layer on the buffer layer, annealing it at 500℃~600℃ for 10min~30min in an oxygen-containing atmosphere, and then selenizing it at 600℃~700℃ for 30min~60min in an atmosphere containing a selenium source, thereby obtaining multiple MoSe2 islands. The MoO3 layer is grown by ALD, with Mo(CO)6 as the Mo source, O3 as the O source, Ar as the carrier gas, and the growth temperature being 150℃~200℃. The growth temperature of the GaN filler layer is 950℃~1100℃, the growth pressure is 50 torr~200 torr, and the V / III ratio is 2000~3000; The growth temperature of the first AlGaN layer is 1000℃~1100℃, the growth pressure is 50 torr~200 torr, and the V / Ⅲ ratio is 2000~3000; The In x Ga 1-x The growth temperature of the N layer is 620℃~750℃, and the growth pressure is 100 torr~300 torr; The growth temperature of the first GaN layer is 700℃~800℃, and the growth pressure is 100 torr~300 torr.
[0013] As an improvement to the above technical solution, the multi-quantum well layer includes a first multi-quantum well layer and a second multi-quantum well layer; the first multi-quantum well layer includes In... y Ga 1-y The N-layer and the second GaN layer; the second multiple quantum well layer includes In z Ga 1-z N-layer and C, Mg co-doped BGaN layer and second AlGaN layer; The In y Ga 1-y The growth temperature of the N layer is 750℃~800℃, and the growth pressure is 100 torr~500 torr; The growth temperature of the second GaN layer is 850℃~900℃, and the growth pressure is 100 torr~500 torr; The In z Ga 1-z The growth temperature of the N layer is 750℃~800℃, and the growth pressure is 100 torr~500 torr; The growth temperature of the C and Mg co-doped BGaN layer is 650℃~750℃, and the growth pressure is 10 torr~150 torr; The growth temperature of the second AlGaN layer is 900℃~1000℃, and the growth pressure is 100 torr~500 torr.
[0014] Accordingly, the present invention also discloses a light-emitting diode, which includes the above-mentioned light-emitting diode epitaxial wafer.
[0015] Implementing this invention has the following beneficial effects: 1. In the epitaxial wafer of the light-emitting diode of the present invention, a V-pit preparation layer and a V-pit layer are sequentially disposed between an N-type GaN layer and a multi-quantum-well layer. The V-pit preparation layer includes a template layer, a GaN filling layer, and a first AlGaN layer stacked sequentially. The template layer includes multiple MoSe2 islands arrayed on the N-type GaN layer. The thickness of the GaN filling layer is slightly greater than the height of the MoSe2 islands, so that after the GaN filling layer grows, holes are formed on the top of the MoSe2 islands. Based on the above configuration, firstly, the MoSe2 islands promote the lateral growth tendency of the GaN filling layer, effectively reducing the density of edge dislocations, screw dislocations, mixed dislocations, and point dislocations. Secondly, by introducing the first AlGaN layer with higher crystal quality, the density of point dislocations is effectively reduced. Therefore, based on the above structure, the number of screw dislocations, point dislocations, mixed dislocations, and edge dislocations extending from the substrate can be significantly reduced. Only a small number of edge dislocations pass through the hole, resulting in a limited distribution of edge dislocations at the top after the first AlGaN layer is grown. This allows subsequent V-pits to be distributed along these edge dislocations, effectively promoting the uniformity of V-pit distribution and improving luminous efficiency and wavelength uniformity. Furthermore, because the V-pit preparation layer relaxes a large number of dislocations, improving surface smoothness, it also allows the In in the subsequent V-pit layer to... x Ga 1-x The In component is more evenly distributed in the N layer, thus making In x Ga 1-x The N-layer can use a higher In content, which increases the opening size of the V-shaped pit, increases the probability of holes being injected from the sidewall of the V-shaped pit, and improves the luminous efficiency of the LED epitaxial wafer.
[0016] 2. In the epitaxial wafer of the light-emitting diode of the present invention, the multiple quantum well layer includes a first multiple quantum well layer and a second multiple quantum well layer stacked sequentially; the first multiple quantum well layer is a periodically stacked In... y Ga 1-y The N-layer and the second GaN layer, the second multi-quantum-well layer are periodically stacked In layers. z Ga 1-z The invention comprises an N-layer, a C / Mg co-doped BGaN layer, and a second AlGaN layer. The z-value is 0.3–0.4. The In-type of this invention... z Ga 1-z In the N-layer, the high proportion of In content leads to the formation of In droplets after growth. This causes C and B atoms from the C and Mg-doped BGaN layers to agglomerate around the growth, inhibiting the growth of nearby materials and further increasing the radius of the V-pits. This increases the probability of holes being injected from the V-pit sidewalls, improving the luminous efficiency of the LED epitaxial wafer. Furthermore, the high potential barrier of BGaN and AlGaN also promotes hole flow to the low potential barrier of the V-pit sidewalls, further enhancing luminous efficiency. Attached Figure Description
[0017] Figure 1 This is a schematic diagram of the structure of a light-emitting diode epitaxial wafer in one embodiment of the present invention; Figure 2 This is a schematic diagram of the V-pit layer structure in one embodiment of the present invention; Figure 3 This is a schematic diagram of the structure of a multi-quantum well layer in one embodiment of the present invention; Figure 4 This is a schematic diagram of the structure of the first multi-quantum well layer in one embodiment of the present invention; Figure 5 This is a schematic diagram of the structure of the second multi-quantum well layer in one embodiment of the present invention; Figure 6 This is a flowchart of a method for preparing an epitaxial wafer for a light-emitting diode according to an embodiment of the present invention. Detailed Implementation
[0018] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be described in further detail below.
[0019] refer to Figure 1 and Figure 2 This invention discloses a light-emitting diode epitaxial wafer, comprising a substrate 1, a buffer layer 2, an undoped GaN layer 3, an N-type GaN layer 4, a V-pit preparation layer 5, a V-pit layer 6, a multiple quantum well layer 7, an electron blocking layer 8, and a P-type GaN layer 9, sequentially stacked on the substrate 1. The V-pit preparation layer 5 comprises a template layer 51, a GaN filler layer 52, and a first AlGaN layer 53, sequentially stacked on the N-type GaN layer 4. The template layer 51 comprises multiple MoSe2 islands 51a arrayed on the N-type GaN layer 4. The thickness of the GaN filler layer 52 is slightly greater than the height of the MoSe2 islands 51a, so that after the GaN filler layer 52 grows, holes are formed on the top of the MoSe2 islands 51a. Subsequently, the first AlGaN layer 53 preferentially grows in the hole region. Based on this growth method, extended edge dislocations can be formed on the upper part of the first AlGaN layer 53, thereby optimizing the distribution of V-pits.
[0020] The height of the MoSe2 island 51a is 20nm to 150nm. When its height is less than 20nm, it is difficult to effectively buffer various dislocations and guide the growth of the subsequent GaN fill layer 52. When its height is greater than 150nm, the subsequent oxidation and selenization processes are difficult, selenization is incomplete, and the buffering effect on various dislocations is relatively poor. For example, the height of the MoSe2 island 51a is 25nm, 30nm, 50nm, 60nm, 70nm, 80nm, 90nm, 100nm, 120nm, or 130nm, but is not limited to these. Preferably, the height of the MoSe2 island 51a is 30nm to 80nm. The width of the MoSe2 island 51a is 30nm to 300nm, for example, 50nm, 120nm, 140nm, 180nm, 210nm, 240nm, or 270nm, but is not limited to these. Preferably, the width of the MoSe2 island 51a is 80nm~200nm.
[0021] The MoSe2 islands 51a can be formed by first growing a MoSe2 layer and then etching it, but are not limited to this method. Preferably, in one embodiment of the present invention, the template layer 51 is prepared by growing a MoO3 layer on an N-type GaN layer 4, annealing it in an oxygen-containing atmosphere at 500°C to 600°C for 10 to 30 minutes, and then selenizing it in an atmosphere containing a selenium source at 600°C to 700°C for 30 to 60 minutes, thereby obtaining multiple MoSe2 islands 51a. Based on the above process of forming a MoO3 layer—annealing—selenization, firstly, the process difficulty is greatly reduced, avoiding the use of complex etching processes; secondly, due to the relatively low temperature, less thermal stress is introduced, reducing the dislocation density introduced by thermal mismatch and improving the luminous efficiency of the LED epitaxial wafer.
[0022] The thickness of the GaN filler layer 52 is 30 nm to 180 nm. When its thickness is less than 30 nm, the pore size formed on the top of the MoSe2 island 51a is too large, making it difficult for various dislocations to relax and affecting the uniformity of the V-pit distribution. When its thickness is greater than 180 nm, the GaN filler layer 52 is almost merged, with no pores, making it difficult to effectively affect the distribution of V-pits. For example, the thickness of the GaN filler layer 52 is 40 nm, 50 nm, 80 nm, 110 nm, 140 nm, or 170 nm, but is not limited to these. Preferably, the thickness of the GaN filler layer 52 is 40 nm to 100 nm.
[0023] The thickness of the first AlGaN layer 53 is 20nm to 120nm, exemplarily 40nm, 60nm, 80nm, 100nm or 110nm, but not limited thereto. Preferably, the thickness of the first AlGaN layer 53 is 20nm to 100nm.
[0024] Among them, the V-pit layer 6 is a periodic structure with 3 to 10 periods. Each period of the V-pit layer 6 includes sequentially stacked In layers. x Ga 1-x The structure consists of an N-layer 61 (x = 0.22~0.3) and a first GaN layer 62. The V-pit layer 6 has a higher In content, resulting in a larger opening radius for the V-pit 6a.
[0025] Among them, In x Ga 1-x The thickness of the N layer 61 is 1nm to 8nm, with exemplary thicknesses of 2.5nm, 4nm, 5.5nm, 6nm, or 7nm, but not limited thereto. Preferably, it is 2nm to 5nm.
[0026] The thickness of the first GaN layer 62 is 5nm to 30nm, exemplarily 8nm, 12nm, 16nm, 20nm, 24nm or 28nm, but not limited thereto. Preferably, the thickness of the first GaN layer 62 is 10nm to 30nm.
[0027] Specifically, the distribution density of V-pits 6a obtained by the opening based on the above technical solution is 5×10⁻⁶. 6 cm -2 ~6×10 7 cm -2 Furthermore, the first opening radius of V-pit 6a is 60nm~120nm, and the second opening radius is 100nm~160nm; where the first opening radius is the radius of V-pit 6a after the growth of V-pit layer 6 (i.e., Figure 1 (d) The second opening radius is the radius of the V pit 6a after the growth of the multi-quantum well layer 7 (i.e. Figure 1 (D).
[0028] The multiple quantum well layer 7 can be a common InGaN / GaN or InGaN / AlGaN type multiple quantum well layer in the art. Furthermore, the In content of InGaN (i.e., the molar ratio of InN) is 0.25~0.4. Based on the V-pit preparation layer 5 and V-pit layer 6 of this application, dislocations can be significantly shielded, thereby increasing the In content in the multiple quantum well layer 7, enabling the LED epitaxial wafer of this invention to better adapt to yellow-green LEDs.
[0029] Preferably, in one embodiment of the present invention, reference is made to... Figures 3-5 The multiple quantum well layer 7 includes a first multiple quantum well layer 71 and a second multiple quantum well layer 72 sequentially stacked on the V-pit layer 6; the first multiple quantum well layer 71 has a periodic structure with a period number of 2 to 8, and each period of the first multiple quantum well layer 71 includes sequentially stacked In... y Ga 1-yN layer 711 and second GaN layer 712, where y is 0.25~0.4.
[0030] Specifically, In y Ga 1-y The thickness of the N-layer 711 is 2nm to 10nm, with examples of 3nm, 4nm, 5nm, 7nm, or 9nm, but not limited thereto. The thickness of the second GaN layer 712 is 5nm to 15nm; with examples of 6nm, 8nm, 10nm, 12nm, or 14nm, but not limited thereto.
[0031] The second multiple quantum well layer 72 has a periodic structure with a period number of 1 to 5. Each period of the second multiple quantum well layer 72 includes sequentially stacked In... z Ga 1-z The N-layer 721 and the C / Mg co-doped BGaN layer 722 and the second AlGaN layer 723, wherein z is 0.3~0.4. In the second multiple quantum well layer 72 of the present invention, a composite layer of the C / Mg co-doped BGaN layer 722 and the second AlGaN layer 723 is used as the quantum barrier layer. This structure of the second multiple quantum well layer 72 can increase the opening size of the V-pit 6a and improve the luminous efficiency. Specifically, based on the above scheme, the second opening radius of the V-pit 6a is 45nm~65nm larger than the first opening radius of the V-pit 6a.
[0032] Among them, In z Ga 1-z The thickness of the N-layer 721 is 2nm to 10nm, with examples of 3nm, 4nm, 5nm, 7nm, or 9nm, but not limited thereto. The thickness of the second AlGaN layer 723 is 5nm to 10nm, with examples of 6nm, 7nm, 8nm, or 9nm, but not limited thereto.
[0033] The thickness of the C and Mg co-doped BGaN layer 722 is 5nm to 10nm, with exemplary thicknesses of 6nm, 7nm, 8nm, or 9nm, but not limited to these. The C doping concentration in the C and Mg co-doped BGaN layer 722 is 1×10⁻⁶. 17 cm -3 ~5×10 17 cm -3 An example is 1.5 × 10 17 cm -3 2×10 17 cm -3 3×10 17 cm -3 Or 4×10 17 cm -3 However, this is not the only factor. The doping concentration of Mg is 2 × 10⁻⁶. 18 cm -3~5×10 19 cm -3 An example is 4×10. 18 cm -3 8×10 18 cm -3 2×10 19 cm -3 Or 4×10 19 cm -3 However, it is not limited to this.
[0034] The substrate 1 is a sapphire substrate, a silicon substrate, a SiC substrate, a ZnO substrate, or a GaN substrate, but is not limited to these.
[0035] The buffer layer 2 is an AlN layer or an AlGaN layer, but is not limited to these. Preferably, it is an AlN layer. The thickness of the buffer layer 2 is 30nm to 80nm, with exemplary thicknesses of 35nm, 40nm, 45nm, 55nm, 60nm, or 75nm, but is not limited to these.
[0036] The thickness of the undoped GaN layer 3 is 0.8 μm to 2.5 μm, with exemplary thicknesses of 0.9 μm, 1.2 μm, 1.5 μm, 1.8 μm, 2.1 μm or 2.4 μm, but not limited thereto.
[0037] The N-type dopant element in the N-type GaN layer 4 is Si, but it is not limited to Si. The N-type doping concentration of the N-type GaN layer 4 is 5 × 10⁻⁶. 18 cm -3 ~5×10 19 cm -3 An example is 6×10 18 cm -3 8×10 18 cm -3 1×10 19 cm -3 3×10 19 cm -3 Or 4×10 19 cm -3 However, it is not limited to this. The thickness of the N-type GaN layer 4 is 1μm to 3μm, with 1.5μm, 1.7μm, 2.3μm or 2.5μm being exemplary, but not limited to this.
[0038] The electron blocking layer 8 is an AlGaN layer or an InAlGaN layer, but is not limited thereto. Preferably, it is an AlGaN layer. The thickness of the electron blocking layer 8 is 30nm to 100nm, with exemplary thicknesses of 40nm, 50nm, 60nm, 70nm, 80nm, or 90nm, but is not limited thereto.
[0039] The P-type dopant in the P-type GaN layer 9 is Mg, but it is not limited to this. The P-type doping concentration in the P-type GaN layer 9 is 1×10⁻⁶. 19 cm -3 ~1×10 21 cm -3 The thickness of the p-type GaN layer 9 is 200nm~500nm, with examples of 220nm, 240nm, 300nm, 400nm or 450nm, but not limited to these.
[0040] Accordingly, refer to Figure 6 The present invention also provides a method for preparing a light-emitting diode epitaxial wafer, which specifically includes the following steps: S1: Provides a substrate; S2: A buffer layer, an undoped GaN layer, an N-type GaN layer, a V-pit preparation layer, a V-pit layer, a multiple quantum well layer, an electron blocking layer, and a P-type GaN layer are grown sequentially on the substrate. Specifically, step S2 includes: S21: Growing a buffer layer on a silicon substrate; Specifically, the buffer layer can be grown using PVD or MOCVD, but is not limited to these methods.
[0041] S22: Growing an undoped GaN layer on the buffer layer; In one embodiment of the present invention, an undoped GaN layer is grown by MOCVD at a growth temperature of 1000℃~1100℃ and a growth pressure of 100 torr~500 torr.
[0042] S23: Growing an N-type GaN layer on an undoped GaN layer; In one embodiment of the present invention, an N-type GaN layer is grown by MOCVD at a growth temperature of 1100°C to 1150°C and a growth pressure of 100 torr to 500 torr.
[0043] S24: Growing V-pit preparation layer on N-type GaN layer; Specifically, step S24 includes: S241: Growing a MoO3 layer on an N-type GaN layer; The MoO3 layer can be grown by PVT, ALD, or PECVD, but is not limited to these methods. Preferably, in one embodiment of the present invention, the MoO3 layer is grown by ALD, using Mo(CO)6 as the Mo source, O3 as the O source, Ar as the carrier gas, and at a growth temperature of 150°C to 200°C.
[0044] S242: Anneal the substrate obtained in step S241 in an oxygen-containing atmosphere; The oxygen-containing atmosphere can be O3, O2, or air, but is not limited to these. The annealing temperature is 500℃~600℃, and the annealing time is 10min~30min.
[0045] Specifically, annealing can be performed in an ALD reaction chamber or an MOCVD reaction chamber, with MOCVD reaction chamber being the preferred option.
[0046] S243: Selenize the silicon substrate obtained in step S242 in a selenium-containing atmosphere to obtain a template layer; The selenium source is DMSe, which can be transported to the reaction chamber using N2 or Ar as the carrier gas for selenization treatment. The selenization treatment temperature is 600℃~700℃, and the selenization treatment time is 30min~60min, but not limited to these. Specifically, the selenization treatment can be carried out in an ALD reaction chamber or an MOCVD reaction chamber, preferably in an MOCVD reaction chamber.
[0047] S244: Growing a GaN filler layer on the template layer; In one embodiment of the present invention, GaN filler layers are grown by MOCVD at a growth temperature of 950°C to 1100°C, a growth pressure of 50 torr to 200 torr, and a V / III ratio of 2000 to 3000. The high-temperature, low-pressure, and high V / III ratio growth method can promote lateral, layered growth.
[0048] S245: The first AlGaN layer is grown on the GaN filler layer; In one embodiment of the present invention, the first AlGaN layer is grown by MOCVD. The growth temperature is 1000℃~1100℃, the growth pressure is 50 torr~200 torr, and the V / III ratio is 2000~3000. The growth temperature is relatively high, the crystal quality is good, and it can effectively block point dislocations.
[0049] S25: Growing a V-pit layer on the V-pit preparation layer; In one embodiment of the present invention, In is periodically grown by MOCVD. x Ga 1-x The process continues with N layers and the first GaN layer, until the V-pit layer is obtained. In... x Ga 1-x The growth temperature of the N layer is 620℃~750℃, and the growth pressure is 100 torr~300 torr; the growth temperature of the first GaN layer is 700℃~800℃, and the growth pressure is 100 torr~300 torr.
[0050] S26: Growth of multiple quantum well layers on V-pit layers; Among them, InGaN / GaN type multiple quantum well layers, or InGaN / AlGaN type multiple quantum well layers or AlGaN / AlGaN type multiple quantum well layers can be grown by MOCVD, but are not limited to these.
[0051] Preferably, in one embodiment of the present invention, S26 includes: S261: The first multi-quantum well layer is grown on the V-pit layer; In one embodiment of the present invention, In is periodically grown by MOCVD. y Ga 1-y The process continues with N-layers and second GaN layers until the first multi-quantum-well layer is obtained. In... y Ga 1-y The growth temperature of the N layer is 750℃~800℃, and the growth pressure is 100 torr~500 torr; the growth temperature of the second GaN layer is 850℃~900℃, and the growth pressure is 100 torr~500 torr.
[0052] S262: Growing a second quantum well layer on the first quantum well layer; In one embodiment of the present invention, In is periodically grown by MOCVD. z Ga 1-z N-layer, C and Mg co-doped BGaN layer, and second AlGaN layer, until a second quantum well layer is obtained. In z Ga 1-z The growth temperature of the N layer is 750℃~800℃, and the growth pressure is 100 torr~500 torr; the growth temperature of the second AlGaN layer is 900℃~1000℃, and the growth pressure is 100 torr~500 torr.
[0053] The growth temperature of the C and Mg co-doped BGaN layer is 650℃~750℃, and the growth pressure is 10 torr~150 torr. During growth, NH3 is introduced as the N source, N2 is introduced as the carrier gas, TEGa is introduced as the C source and Ga source, triethylboron is introduced as the B source, and CP2Mg is introduced as the Mg source in MOCVD.
[0054] S27: Growth of an electron blocking layer on a multi-quantum-well layer; In one embodiment of the present invention, an AlGaN layer is grown by MOCVD as an electron blocking layer at a growth temperature of 1000℃~1100℃ and a growth pressure of 100 torr~300 torr.
[0055] S28: A P-type GaN layer is grown on an electron blocking layer; In one embodiment of the present invention, a P-type GaN layer is grown by MOCVD at a growth temperature of 900°C to 1000°C and a growth pressure of 100 torr to 300 torr.
[0056] The present invention will be further described below with reference to specific embodiments: Example 1 refer to Figure 1 and Figure 2 This embodiment provides a light-emitting diode epitaxial wafer, which includes a substrate 1, and a buffer layer 2, an undoped GaN layer 3, an N-type GaN layer 4, a V-pit preparation layer 5, a V-pit layer 6, a multiple quantum well layer 7, an electron blocking layer 8, and a P-type GaN layer 9 sequentially stacked on the substrate 1.
[0057] In this design, substrate 1 is a sapphire substrate, buffer layer 2 is an AlN layer with a thickness of 50 nm, and undoped GaN layer 3 has a thickness of 1.3 μm. The N-type GaN layer 4 is doped with Si at a doping concentration of 8 × 10⁻⁶. 18 cm -3 Its thickness is 2.5μm.
[0058] The V-pit preparation layer 5 includes a template layer 51, a GaN filler layer 52, and a first AlGaN layer 53 sequentially stacked on an N-type GaN layer 4. The template layer 51 includes multiple MoSe2 islands 51a arrayed on the N-type GaN layer 4, each MoSe2 island 51a having a height of 25 nm and a width of 65 nm. The GaN filler layer 52 has a thickness of 40 nm, creating pores on the top of the MoSe2 islands after the GaN filler layer has grown. The first AlGaN layer has a thickness of 30 nm.
[0059] Among them, the V-pit layer 6 is a periodic structure with 5 periods. Each period of the V-pit layer 6 includes sequentially stacked In layers. x Ga 1-x Layer N 61 (x=0.23) and the first GaN layer 62. Wherein... x Ga 1-x The thickness of the N layer 61 is 1 nm, and the thickness of the first GaN layer 62 is 8 nm.
[0060] The distribution density of V-pit 6a obtained by opening V-pit layer 6 is 5.5 × 10⁻⁶. 7 cm -2 Its first opening radius d is 65nm~75nm, and its second opening radius D is 100nm~112nm.
[0061] Among them, the multi-quantum well layer 7 is a periodic structure with 10 periods. Each period of the multi-quantum well layer 7 includes an InGaN layer and a GaN layer. The InGaN layer has an In composition ratio of 0.3 and a thickness of 3nm, while the GaN layer has a thickness of 10nm.
[0062] Among them, electron blocking layer 8 is an AlGaN layer with a thickness of 65nm.
[0063] In this layer, the doping element of the p-type GaN layer 9 is Mg, with a doping concentration of 3 × 10⁹ / L. 20 cm -3 Its thickness is 220nm.
[0064] The method for fabricating the epitaxial wafer of the light-emitting diode in this embodiment includes the following steps: (1) Provide a substrate.
[0065] (2) A buffer layer is grown on the substrate; Among them, an AlN layer is grown by PVD as a buffer layer; (3) Growing an undoped GaN layer on the buffer layer; Undoped GaN layers were grown by MOCVD at a temperature of 1020℃ and a pressure of 120 torr.
[0066] (4) Growing an N-type GaN layer on an undoped GaN layer; Among them, the N-type GaN layer was grown by MOCVD at a growth temperature of 1150℃ and a growth pressure of 200 torr.
[0067] (5) A template layer is grown on the N-type GaN layer; The process involved growing a MoSe2 layer via MOCVD, followed by ICP etching to obtain multiple MoSe2 islands. The Mo source used was Mo(CO)6, the Se source was DMSe, and the carrier gas was Ar. The growth temperature was 800℃, and the growth pressure was 100 torr.
[0068] (6) Grow a GaN filler layer on the template layer; Among them, GaN filler layers were grown by MOCVD at a growth temperature of 980℃, a growth pressure of 70 torr, and a V / Ⅲ ratio of 2400.
[0069] (7) A first AlGaN layer is grown on the GaN filler layer; The first AlGaN layer was grown by MOCVD at a temperature of 1050℃, a growth pressure of 120 torr, and a V / Ⅲ ratio of 2500.
[0070] (8) A V-pit layer is grown on the first AlGaN layer; Among them, In is grown periodically through MOCVD. x Ga 1-x The process continues with N layers and the first GaN layer, until the V-pit layer is obtained. In... x Ga 1-x The growth temperature of the N layer is 650℃ and the growth pressure is 220 torr; the growth temperature of the first GaN layer is 750℃ and the growth pressure is 150 torr.
[0071] (9) Growing a multi-quantum-well layer on the V-pit layer; In this process, InGaN and GaN layers are periodically grown using MOCVD until a multi-quantum-well layer is obtained. The growth temperature of the InGaN layer is 760℃, the growth temperature of the GaN layer is 880℃, and the growth pressure of both is 300 torr.
[0072] (10) Growing an electron blocking layer on a multi-quantum-well layer; An AlGaN layer was grown using MOCVD as an electron blocking layer. The growth temperature of the electron blocking layer was 1050℃, and the growth pressure was 200 torr.
[0073] (11) A P-type GaN layer is grown on the electron blocking layer; P-type GaN layers were grown using MOCVD at a temperature of 950℃ and a growth pressure of 200 torr.
[0074] Example 2 This embodiment provides a light-emitting diode epitaxial wafer, which differs from Embodiment 1 in that: The MoSe2 island 51a has a height of 60 nm and a width of 130 nm; the GaN filler layer 52 has a thickness of 80 nm. x Ga 1-x The thickness of the N layer 61 is 4nm, and the thickness of the first GaN layer 62 is 11nm.
[0075] The distribution density of V-pit 6a obtained by opening V-pit layer 6 is 2.3 × 10⁻⁶. 7 cm -2 Its first opening radius d is 72nm~84nm, and its second opening radius D is 105nm~120nm.
[0076] Everything else is the same as in Example 1.
[0077] Example 3 This embodiment provides a light-emitting diode epitaxial wafer, which differs from Embodiment 2 in that the template layer 51 is prepared using the following method: (i) Growing a MoO3 layer on an N-type GaN layer; The MoO3 layer was grown using the ALD method, with Mo(CO)6 as the Mo source, O3 as the O source, Ar as the carrier gas, and a growth temperature of 160℃. The thickness of the MoO3 layer was 80 nm.
[0078] (ii) Annealing in an O2 atmosphere; Specifically, annealing is carried out in the MOCVD reaction chamber at a temperature of 550°C for 20 minutes.
[0079] (iii) Selenization is carried out in a selenium-containing atmosphere to obtain a template layer; Specifically, selenization is performed in the MOCVD reaction chamber using DMSe as the selenium source and Ar as the carrier gas. The selenization process is carried out at 650℃ for 55 minutes.
[0080] Specifically, in this embodiment, the height of the MoSe2 island 51a is 60nm~74nm and the width is 140nm~190nm.
[0081] The distribution density of V-pit 6a obtained by opening V-pit layer 6 is 8.5 × 10⁻⁶. 6 cm -2 Its first opening radius d is 70nm~85nm, and its second opening radius D is 98nm~120nm.
[0082] The rest are the same as in Example 2.
[0083] Example 4 This embodiment provides a light-emitting diode epitaxial wafer, which differs from Embodiment 3 in that: The multiple quantum well layer 7 includes a first multiple quantum well layer 71 and a second multiple quantum well layer 72 sequentially stacked on the V-pit layer 6; The first multiple quantum well layer has a periodic structure with 7 periods. Each period of the first multiple quantum well layer 71 includes sequentially stacked In... y Ga 1-y N-layer 711 (y=0.3) and the second GaN layer 712, In y Ga 1-y The thickness of the N-layer 711 is 3nm, and the thickness of the second GaN layer 712 is 10nm.
[0084] The second quantum well layer 72 has a periodic structure with 3 periods. Each period of the second quantum well layer 72 includes sequentially stacked In... z Ga 1-z The structure consists of an N-layer 721 (z=0.33), a C / Mg co-doped BGaN layer 722, and a second AlGaN layer 723. In... z Ga1-z The thickness of the N-layer 721 is 4 nm, the thickness of the C- and Mg co-doped BGaN layer 722 is 7 nm, and the thickness of the second AlGaN layer 723 is 7 nm. The C doping concentration in the C- and Mg co-doped BGaN layer 722 is 2.5 × 10⁻⁶. 17 cm -3 The Mg doping concentration is 5 × 10⁻⁶. 18 cm -3 .
[0085] The method for fabricating the multiple quantum well layer in this embodiment is as follows: (I) Growing the first multiple quantum well layer on the V-pit layer; Among them, In is grown periodically through MOCVD. y Ga 1-y The process continues with N-layers and second GaN layers until the first multi-quantum-well layer is obtained. In... y Ga 1-y The growth temperature of the N layer is 760℃ and the growth pressure is 300 torr; the growth temperature of the second GaN layer is 880℃ and the growth pressure is 300 torr.
[0086] (II) Growing a second multiple quantum well layer on the first multiple quantum well layer; Among them, In is grown periodically through MOCVD. z Ga 1-z The process continues with N-layers, C and Mg co-doped BGaN layers, and a second AlGaN layer, until a second multi-quantum-well layer is obtained. In... z Ga 1-z The growth temperature of the N-layer was 760℃, and the growth pressure was 300 torr; the growth temperature of the second AlGaN layer was 980℃, and the growth pressure was 300 torr. The growth temperature of the C and Mg co-doped BGaN layer was 730℃, and the growth pressure was 20 torr.
[0087] The first opening radius d of V pit 6a is 70nm~85nm, and the second opening radius D is 115nm~145nm.
[0088] Everything else is the same as in Example 3.
[0089] Comparative Example 1 This comparative example provides a light-emitting diode epitaxial wafer, which differs from Example 1 in that it does not include the V-pit preparation layer and the V-pit layer. Correspondingly, the preparation method does not include the preparation steps of these two layers. All other aspects are the same as in Example 1.
[0090] Comparative Example 2 This comparative example provides a light-emitting diode epitaxial wafer, which differs from Example 1 in that it does not include a V-pit preparation layer, and correspondingly, the fabrication method does not include the preparation step of this layer. Everything else is the same as in Example 1.
[0091] Comparative Example 3 This comparative example provides a light-emitting diode epitaxial wafer, which differs from Example 1 in that it does not include a V-pit layer, and correspondingly, the fabrication method does not include the fabrication step of this layer. Everything else is the same as in Example 1.
[0092] Comparative Example 4 This comparative example provides a light-emitting diode epitaxial wafer, which differs from Example 1 in that it does not include the V-pit preparation layer and the V-pit layer, and correspondingly, the fabrication method does not include the fabrication steps of these two layers. Furthermore, its multi-quantum-well layer structure and fabrication method are the same as those in Example 4.
[0093] Everything else is the same as in Example 1.
[0094] Comparative Example 5 This comparative example provides a light-emitting diode epitaxial wafer, which differs from Example 1 in that it does not include a V-pit preparation layer, and correspondingly, the fabrication method does not include the fabrication step of this layer. Furthermore, the structure and fabrication method of its multi-quantum-well layer are the same as those in Example 4.
[0095] Everything else is the same as in Example 1.
[0096] Comparative Example 6 This comparative example provides a light-emitting diode epitaxial wafer, which differs from Example 1 in that it does not include a V-pit layer, and correspondingly, the fabrication method does not include the fabrication step of this layer. Furthermore, its multi-quantum-well layer structure and fabrication method are the same as those in Example 4.
[0097] Everything else is the same as in Example 1.
[0098] Using the LED epitaxial wafers obtained in Examples 1-4 and Comparative Examples 1-6, a 10mil × 24mil vertical structure chip was fabricated. Testing was then performed. (1) Ten chips were taken from each embodiment and comparative example, and the luminous brightness at 20mA was measured. The luminous brightness improvement rate was calculated based on Comparative Example 1. (2) Take 10 chips for each example and comparative example, measure the emission wavelength at 20mA, and calculate the standard deviation as the emission wavelength uniformity.
[0099] The luminous intensity was tested; 20 samples were tested for each embodiment and comparative example, and the standard deviation of the test values was taken as the result. The specific test results are shown in the table below: As can be seen from the table, when the V-pit preparation layer and V-pit layer of the present invention are added to the conventional light-emitting diode epitaxial wafer (Comparative Example 1), the luminous brightness and wavelength uniformity of the light-emitting diode epitaxial wafer are effectively improved.
[0100] The above description is a preferred embodiment of the invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made without departing from the principle of the invention, and these improvements and modifications are also considered to be within the scope of protection of the invention.
Claims
1. A light-emitting diode epitaxial wafer, characterized in that, It includes a substrate, and a buffer layer, an undoped GaN layer, an N-type GaN layer, a V-pit preparation layer, a V-pit layer, a multiple quantum well layer, an electron blocking layer and a P-type GaN layer are sequentially stacked on the substrate. The V-pit preparation layer includes a template layer, a GaN filler layer, and a first AlGaN layer sequentially stacked on the N-type GaN layer; the template layer includes multiple MoSe2 islands arrayed on the N-type GaN layer, and the thickness of the GaN filler layer is slightly greater than the height of the MoSe2 islands, so that after the GaN filler layer grows, a hole is formed on the top of the MoSe2 island; the height of the MoSe2 island is 30nm~80nm, and the width of the MoSe2 island is 80nm~200nm; The V-pit layer has a periodic structure with 3 to 10 periods, and each period of the V-pit layer includes sequentially stacked In layers. x Ga 1-x The N-layer and the first GaN layer, where x is 0.22~0.
3.
2. The light-emitting diode epitaxial wafer as described in claim 1, characterized in that, The thickness of the GaN filler layer is 40nm~100nm, and the thickness of the first AlGaN layer is 20nm~100nm; The In x Ga 1-x The thickness of the N layer is 2nm~5nm, and the thickness of the first GaN layer is 10nm~30nm.
3. The light-emitting diode epitaxial wafer as described in claim 1, characterized in that, The template layer is prepared by growing a MoO3 layer on the N-type GaN layer, annealing it at 500℃~600℃ for 10min~30min in an oxygen-containing atmosphere, and then selenizing it at 600℃~700℃ for 30min~60min in an atmosphere containing a selenium source, thereby obtaining multiple MoSe2 islands.
4. The light-emitting diode epitaxial wafer as described in claim 1, characterized in that, The V-pit layer forms multiple V-pits, and the distribution density of the V-pits is 5 × 10⁻⁶. 6 cm -2 ~6×10 7 cm -2 The first opening radius of the V-shaped pit is 60nm~120nm, and the second opening radius is 100nm~160nm; Wherein, the first opening radius is the radius of the V-pit after the V-pit layer is grown, and the second opening radius is the radius of the V-pit after the multi-quantum-well layer is grown.
5. The light-emitting diode epitaxial wafer as described in any one of claims 1 to 4, characterized in that, The multi-quantum well layer includes a first multi-quantum well layer and a second multi-quantum well layer sequentially stacked on the V-pit layer; The first multiple quantum well layer has a periodic structure with 2 to 8 periods. Each period of the first multiple quantum well layer includes sequentially stacked In... y Ga 1-y The N-layer and the second GaN-layer, where y is 0.25~0.4; The second multiple quantum well layer has a periodic structure with a period number of 1 to 5. Each period of the second multiple quantum well layer includes sequentially stacked In... z Ga 1-z The BGaN layer and the second AlGaN layer are co-doped with N and C and Mg, respectively, wherein z is 0.3~0.
4. The V-pit layer forms multiple V-pits, and the second opening radius of the V-pit is 45nm~65nm larger than the first opening radius of the V-pit; Wherein, the first opening radius is the radius of the V-pit after the V-pit layer is grown, and the second opening radius is the radius of the V-pit after the multi-quantum-well layer is grown.
6. The light-emitting diode epitaxial wafer as described in claim 5, characterized in that, The In y Ga 1-y The thickness of the N layer is 2nm~10nm, and the thickness of the second GaN layer is 5nm~15nm; The In z Ga 1-z The thickness of the N layer is 2nm~10nm, the thickness of the C and Mg co-doped BGaN layer is 5nm~10nm, and the thickness of the second AlGaN layer is 5nm~10nm; The C doping concentration in the C and Mg co-doped BGaN layer is 1×10⁻⁶. 17 cm -3 ~5×10 17 cm -3 The Mg doping concentration is 2 × 10⁻⁶. 18 cm -3 ~5×10 19 cm -3 .
7. A method for fabricating a light-emitting diode epitaxial wafer, used to fabricate a light-emitting diode epitaxial wafer as described in any one of claims 1 to 6, characterized in that, include: A substrate is provided on which a buffer layer, an undoped GaN layer, an N-type GaN layer, a V-pit preparation layer, a V-pit layer, a multiple quantum well layer, an electron blocking layer and a P-type GaN layer are sequentially grown. The V-pit preparation layer includes a template layer, a GaN filler layer, and a first AlGaN layer sequentially stacked on the N-type GaN layer; the template layer includes multiple MoSe2 islands arrayed on the N-type GaN layer, and the thickness of the GaN filler layer is slightly greater than the height of the MoSe2 islands, so that after the GaN filler layer grows, a hole is formed on the top of the MoSe2 island; the height of the MoSe2 island is 30nm~80nm, and the width of the MoSe2 island is 80nm~200nm; The V-pit layer has a periodic structure with 3 to 10 periods, and each period of the V-pit layer includes sequentially stacked In layers. x Ga 1-x The N-layer and the first GaN layer, where x is 0.22~0.
3.
8. The method for fabricating a light-emitting diode epitaxial wafer as described in claim 7, characterized in that, The template layer is prepared by growing a MoO3 layer on the buffer layer, annealing it at 500℃~600℃ for 10min~30min in an oxygen-containing atmosphere, and then selenizing it at 600℃~700℃ for 30min~60min in an atmosphere containing a selenium source to obtain multiple MoSe2 islands. The MoO3 layer is grown by ALD, with Mo(CO)6 as the Mo source, O3 as the O source, Ar as the carrier gas, and the growth temperature being 150℃~200℃. The growth temperature of the GaN filler layer is 950℃~1100℃, the growth pressure is 50 torr~200 torr, and the V / III ratio is 2000~3000; The growth temperature of the first AlGaN layer is 1000℃~1100℃, the growth pressure is 50 torr~200 torr, and the V / Ⅲ ratio is 2000~3000; The In x Ga 1-x The growth temperature of the N layer is 620℃~750℃, and the growth pressure is 100 torr~300 torr; The growth temperature of the first GaN layer is 700℃~800℃, and the growth pressure is 100 torr~300 torr.
9. The method for fabricating a light-emitting diode epitaxial wafer as described in claim 7, characterized in that, The multi-quantum-well layer includes a first multi-quantum-well layer and a second multi-quantum-well layer; the first multi-quantum-well layer includes In... y Ga 1-y The N-layer and the second GaN layer; the second multiple quantum well layer includes In z Ga 1-z N-layer and C, Mg co-doped BGaN layer and second AlGaN layer; The In y Ga 1-y The growth temperature of the N layer is 750℃~800℃, and the growth pressure is 100 torr~500 torr; The growth temperature of the second GaN layer is 850℃~900℃, and the growth pressure is 100 torr~500 torr; The In z Ga 1-z The growth temperature of the N layer is 750℃~800℃, and the growth pressure is 100 torr~500 torr; The growth temperature of the C and Mg co-doped BGaN layer is 650℃~750℃, and the growth pressure is 10 torr~150 torr; The growth temperature of the second AlGaN layer is 900℃~1000℃, and the growth pressure is 100 torr~500 torr.
10. A light-emitting diode, characterized in that, Includes the light-emitting diode epitaxial wafer as described in any one of claims 1 to 6.
Citation Information
Patent Citations
Preparation method for semiconductor light-emitting device
CN104795472A
Semiconductor chip manufacturing condition setting method, and manufacturing method and manufacturing system of semiconductor chip
JP2016096321A