Negative electrode material for nonaqueous electrolyte secondary battery and nonaqueous electrolyte secondary battery

By using composite particles containing lithium aluminate phase and dispersed silicon phase as the negative electrode active material, the problem of low alkali resistance of lithium silicate phase is solved, achieving high-efficiency charging and discharging and improved stability of lithium-ion secondary batteries, and promoting the high energy density of batteries.

CN116636036BActive Publication Date: 2026-11-24PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202180078909.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-11-30
Filing Date
2021-09-22
Publication Date
2026-11-24
Estimated Expiration
2041-09-22

AI Technical Summary

Technical Problem

In existing lithium-ion secondary batteries, the lithium silicate phase has low alkali resistance, resulting in low initial charge and discharge efficiency and frequent side reactions, which affects the process of achieving high energy density in batteries.

Method used

Composite particles are used as the negative electrode active material. The composite particles contain a lithium aluminate phase and a silicon phase dispersed therein. By controlling the composition and structure of the lithium aluminate phase, the alkali resistance is improved and the side reactions are suppressed. The island structure is formed to mitigate the expansion and contraction of the silicon phase.

Benefits of technology

It effectively suppressed the decrease in initial charge and discharge efficiency, improved the battery's cycle characteristics and increased capacity, and enhanced the battery's stability and ion conductivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116636036B_ABST
    Figure CN116636036B_ABST
Patent Text Reader

Abstract

The negative electrode active material for non-aqueous electrolyte secondary batteries comprises composite particles, wherein the composite particles include a lithium aluminate phase and a silicon phase dispersed within the lithium aluminate phase.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure mainly relates to improvement of a negative electrode for a non-aqueous electrolyte secondary battery. Background Art

[0002] Non-aqueous electrolyte secondary batteries, particularly lithium ion secondary batteries, have high voltage and high energy density, and therefore are expected as power sources for small civilian applications, power storage devices, and electric vehicles. In the process of increasing the energy density of batteries, utilization of a silicon (Si)-containing material that can be alloyed with lithium is expected as a negative electrode active material having high theoretical capacity density.

[0003] Patent Literature 1 proposes a negative electrode active material (hereinafter also referred to as LSX) including Li 2z SiO 2+z a lithium silicate phase represented by (0<z<2), and silicon particles dispersed in the lithium silicate phase.

[0004] Prior Art Literature

[0005] Patent Literature

[0006] Patent Literature 1: International Publication No. 2016 / 35290 pamphlet Summary of Invention

[0007] LSX has a smaller irreversible capacity and a higher initial charge / discharge efficiency than SiOx in which silicon particles are dispersed in a SiO2 phase.

[0008] However, the lithium silicate phase in LSX has low alkali resistance (stability to Li), and may still cause a side reaction with Li ions during initial charging, so further improvement of the initial charge / discharge efficiency is required.

[0009] In view of the above, one aspect of the present disclosure relates to a negative electrode active material for a non-aqueous electrolyte secondary battery, including composite particles, the composite particles including: a lithium aluminate phase, and a silicon phase dispersed in the lithium aluminate phase.

[0010] Another aspect of the present disclosure relates to a non-aqueous electrolyte secondary battery including: a positive electrode, a negative electrode, and a non-aqueous electrolyte, wherein the negative electrode includes the above negative electrode active material for a non-aqueous electrolyte secondary battery.

[0011] According to the present disclosure, it is possible to suppress a decrease in initial charge / discharge efficiency of a non-aqueous electrolyte secondary battery. Brief Description of Drawings

[0012] Figure 1 FIG. 1 is a diagram showing an example of an XRD spectrum of a negative electrode active material (composite particles) according to an embodiment of the present disclosure.

[0013] Figure 2 A cross-sectional view of a negative electrode active material (composite particles) according to one embodiment of the present disclosure is shown for illustrative purposes.

[0014] Figure 3 A simplified perspective view of a non-aqueous electrolyte secondary battery according to one embodiment of this disclosure, with a portion cut off. Detailed Implementation

[0015] [Negative electrode active material for non-aqueous electrolyte secondary batteries]

[0016] The negative electrode active material for a non-aqueous electrolyte secondary battery according to embodiments of this disclosure comprises composite particles (hereinafter also referred to as LAX particles), the composite particles comprising: a lithium aluminate phase and a silicon phase dispersed within the lithium aluminate phase.

[0017] Compared to the lithium silicate phase dispersed within the lithium silicate phase in LSX particles, the lithium aluminate phase in LAX particles exhibits superior alkali resistance. Consequently, the initial charging side reactions with Li ions are further suppressed in LAX particles compared to LSX particles, thus inhibiting the degradation of the negative electrode active material associated with these side reactions and the resulting reduction in initial capacity. In other words, the initial reduction in charge-discharge efficiency is highly suppressed.

[0018] LAX particles may be substantially free of lithium silicate and SiO2. LAX particles may contain lithium silicate and SiO2, but preferably in small amounts. The content of lithium silicate and SiO2 in added LAX particles may, for example, be less than 3% by mass.

[0019] In the LAX particles, the aluminum content (MAl) relative to the total amount of elements other than oxygen (excluding oxygen) is preferably 10% by mass or more and 47% by mass or less, and the lithium content (MLi) relative to the total amount of elements other than oxygen (excluding oxygen) is 0.7% by mass or more and 13.5% by mass or less. When the aluminum content (MAl) and lithium content (MLi) are within the above ranges, an aluminate phase with excellent stability and ionic conductivity is readily obtained. It should be noted that the above stability includes both chemical stability (alkali resistance) and thermal stability. The aluminum content (MAl) is more preferably 11.5% by mass or more and 45.5% by mass or less. The lithium content (MLi) is more preferably 1.0% by mass or more and 9.5% by mass or less.

[0020] Furthermore, from the viewpoint of easily obtaining lithium aluminate phases with excellent stability and ionic conductivity, the ratio of aluminum (MAl) to lithium (MLi) is preferably 2 or more and 20 or less. More preferably, the ratio is 4 or more and 12 or less.

[0021] From the viewpoint of balancing high capacity and improved cycle performance, the silicon content (MSi) in LAX particles, relative to the total amount of elements other than oxygen, is preferably 40% by mass or more and 90% by mass or less, more preferably 50.8% by mass or more and 85.5% by mass or less. The aforementioned silicon content (MSi) refers to the amount of Si constituting the silicon phase in the LAX particles.

[0022] In the XRD pattern of the composite particles obtained by X-ray diffraction (XRD), a peak originating from the lithium aluminate phase can be observed near 2θ = x°. x° is selected from at least one of the group consisting of 19.4°, 22.3°, 31.9°, 34.3°, and 37.5°. Cu Kα rays are used in the XRD measurements. It should be noted that, in this specification, "near x°" refers to, for example, a range of x ± 1°.

[0023] The lithium aluminate phase can contain dispersed Al₂O₃ phase. Highly crystalline, finely textured Al₂O₃ phases can be distributed in island-like patterns within the aluminate matrix. In this case, the expansion and cracking of the aluminate phase, accompanied by the expansion and contraction of the silicon phase, is easily suppressed, and the cycling characteristics are easily improved. In this case, a peak originating from the Al₂O₃ phase can be observed near 2θ = 25.4° in the X-ray diffraction pattern of the composite particles obtained by X-ray diffraction. The Al₂O₃ phase content in the LAX particles is, for example, 0% by mass or more and 10% by mass or less.

[0024] Here, Figure 1 An example of an XRD pattern of a negative electrode active material (composite particles) according to an embodiment of the present disclosure is shown. Figure 1 The solid line in the image represents the XRD pattern of the large Al-rich composite particles (LAX2) of MAl / MLi. Figure 1 The dashed line in the figure represents the XRD pattern of small Li-rich composite particles (LAX4) of MaI / MLi. LAX2 corresponds to Example 2 (battery A2) described later, and LAX4 corresponds to Example 4 (battery A4) described later.

[0025] Both LAX2 and 4 show peaks originating from the Si(111) plane of the silicon phase around 2θ = 28°. In Al-rich LAX2, a peak originating from the Al2O3 phase is observed around 2θ = 25.4°.

[0026] Figure 1 In LAX2, peaks (i) to (v) represent those originating from the lithium aluminate phase. Peaks of Li₂Al₄O₇ and LiAlO₂ originating from the lithium aluminate phase are observed near 2θ = 19.4° and 2θ = 31.9°, respectively. Figure 1Peaks (i) and (ii) in LAX2 were observed near 2θ = 37.5°, representing Li2Al4O7 and LiAl5O8 originating from the lithium aluminate phase. Figure 1 (peak (iii) in the middle).

[0027] In LAX4, peaks originating from the lithium aluminate phase, namely LiAlO2 and Li5AlO4, were observed near 2θ = 22.3° and 2θ = 34.3°. Figure 1 Peaks (iv) and (v) in the middle.

[0028] The composite particles possess an island structure, with a lithium aluminate phase forming the sea and fine silicon phases dispersed within it as islands. The lithium aluminate phase exhibits excellent ionic conductivity, facilitating the absorption, storage, and release of lithium ions between the lithium aluminate and silicon phases. High capacity can be achieved by controlling the amount of silicon phase dispersed within the lithium aluminate phase. The lithium aluminate phase mitigates the expansion and contraction of the silicon phase. Therefore, it is easy to achieve a balance between high battery capacity and improved cycle performance. From the perspective of mitigating silicon phase expansion and contraction, the lithium aluminate phase can be amorphous.

[0029] In composite particles, multiple primary particles comprising lithium aluminate and silicon phases are combined to form secondary particles. The average particle size of the composite particles (secondary particles) is, for example, 1 μm or more and 25 μm or less, or 4 μm or more and 15 μm or less. Within the above particle size range, the stress caused by the volume change of the composite particles during charging and discharging is easily mitigated, making it easier to obtain good cycling characteristics. The surface area of ​​the composite particles is also of an appropriate size, and the capacity reduction caused by side reactions with non-aqueous electrolytes is also suppressed. The average particle size of the composite particles refers to the particle size in the particle size distribution measured by laser diffraction scattering method, where the volume cumulative value is 50% (volume average particle size). For example, the "LA-750" manufactured by Horiba Corporation can be used in the measuring apparatus. When the surface of the composite particles is covered by a conductive layer, the thickness of the conductive layer is so small that it does not substantially affect the average particle size of the composite particles; therefore, the average particle size of the composite particles with the conductive layer can also be regarded as the average particle size of the composite particles.

[0030] The composite particles can be removed from the battery using the following method. First, the battery in a fully discharged state is disassembled, and the negative electrode is removed. The negative electrode is then cleaned with anhydrous methyl ethyl carbonate or dimethyl carbonate to remove non-aqueous electrolyte components. As described later, the negative electrode has a negative current collector and a negative electrode additive layer loaded on its surface. Therefore, the negative electrode additive layer is peeled off from the copper foil and pulverized in a mortar to obtain sample powder. Next, the sample powder is dried in a dry atmosphere for 1 hour and immersed in slightly boiling 6M hydrochloric acid for 10 minutes to remove elements other than those from the composite particles. Then, the sample powder is washed with deionized water, filtered, and dried at 200°C for 1 hour. Afterward, the conductive layer is removed by heating to 900°C in an oxygen atmosphere, thereby separating only the composite particles. It should be noted that a fully discharged state refers to a depth of discharge (DOD) of 90% or more (state of charge (SOC) of 10% or less).

[0031] (Lithium aluminate phase)

[0032] Lithium aluminates contain lithium (Li), aluminum (Al), and oxygen (O). The atomic ratio of O to Al in lithium aluminates is, for example, 1.6 or more and 4 or less. Furthermore, the atomic ratio of Li to Al in lithium aluminates is, for example, 1 / 5 or more and 5 or less. When the atomic ratios of O / Al and Li / Al are within the above ranges, it is advantageous in terms of the stability and ionic conductivity of the lithium aluminate phase.

[0033] The composition of lithium aluminate can be expressed by the formula: Li u AlO (3+u) / 2 The expression is used to indicate the presence of a component. From the viewpoint of ease of manufacture, stability, and ionic conductivity, u in the formula can be greater than 0 and less than 5, or greater than 0 and less than 1. For example, if u = 1 / 5, it can be represented by LiAl5O8; if u = 1 / 2, it can be represented by Li2Al4O7; if u = 1, it can be represented by LiAlO2; and if u = 5, it can be represented by Li5AlO4. From the viewpoint of ease of manufacture, stability, and ionic conductivity, the lithium aluminate phase preferably includes at least one component selected from the group consisting of LiAl5O8, Li2Al4O7, LiAlO2, and Li5AlO4. More preferably, the lithium aluminate phase includes LiAlO2 as the main component. Here, "main component" refers to a component that accounts for 50% or more by mass of the total mass of the lithium aluminate phase, or 70% or more by mass.

[0034] In addition to Li, Al, and O, the lithium aluminate phase may also contain other elements M. Element M is selected from at least one element chosen from the group consisting of sodium (Na), potassium (K), calcium (Ca), magnesium (Mg), zirconium (Zr), iron (Fe), boron (B), phosphorus (P), and lanthanum (La). The inclusion of element M further improves the stability and ionic conductivity of the aluminate phase. Furthermore, side reactions arising from contact between the aluminate phase and non-aqueous electrolytes are suppressed. From the viewpoint of resistance to non-aqueous electrolytes and structural stability of the aluminate phase, element M is preferably selected from at least one element chosen from the group consisting of Zr, Fe, P, and B. La can further improve the initial charge-discharge efficiency.

[0035] Element M can form compounds. Depending on the type of element M, these compounds can be, for example, oxides or aluminates of element M. In the lithium aluminate phase, the content of element M relative to the total amount of elements other than oxygen is, for example, 0.3 mol% or more and 3 mol% or less.

[0036] The lithium aluminate phase may also contain trace amounts of elements such as chromium (Cr), nickel (Ni), manganese (Mn), copper (Cu), and molybdenum (Mo).

[0037] The contents of Li, Al, and element M in the lithium aluminate phase can be determined, for example, by analyzing the cross-section of the negative electrode binder layer.

[0038] First, the fully discharged battery was disassembled, and the negative electrode was removed. The negative electrode was then cleaned with anhydrous methyl ethyl carbonate or dimethyl carbonate to remove the non-aqueous electrolyte components. After drying, a cross-section polishing (CP) machine was used to obtain the cross-section of the negative electrode flux layer. Next, the cross-section of the negative electrode flux layer was observed using a scanning electron microscope (SEM).

[0039] Then, the content of each element can be determined using any of the following methods. Furthermore, the composition of the lithium aluminate phase can be calculated from the content of each element.

[0040] <EDX>

[0041] Ten composite particles with a maximum diameter of 5 μm or more were randomly selected from the cross-sectional image of the reflected electron image of the negative electrode mixture layer. For each particle, elemental mapping analysis based on energy-dispersive X-ray (EDX) was performed. The area containing the target element was calculated using image analysis software. The ideal magnification was 2000–20000x. The measured areas containing the specified element in the ten particles were averaged. The content of the target element was calculated from the average value.

[0042] The following shows the ideal measurement conditions for cross-sectional SEM-EDX analysis.

[0043] <SEM-EDX measurement conditions>

[0044] Processing apparatus: JEOL SM-09010 (Cross Section Polisher)

[0045] Processing conditions: acceleration voltage 6kV

[0046] Current value: 140μA

[0047] Degree of vacuum: 1×10 -3 to 2×10 -3 Pa

[0048] Measurement apparatus: electron microscope HITACHI SU-70

[0049] Acceleration voltage during analysis: 10kV

[0050] Field: free mode

[0051] Probe current mode: medium

[0052] Probe current range: high

[0053] Anode Ap.: 3

[0054] OBJ Ap.: 2

[0055] Analysis area: 1 μm square

[0056] Analysis software: EDAX Genesis

[0057] CPS: 20500

[0058] Lsec: 50

[0059] Time constant: 3.2

[0060] <AES>

[0061] From cross-sectional images of the negative electrode mixture layer captured via reflected electron imaging, 10 composite particles with a maximum diameter of 5 μm or larger are randomly selected. Each selected particle is subjected to qualitative and quantitative elemental analysis using an Auger electron spectroscopy (AES) analyzer (for example, JAMP-9510F manufactured by JEOL Ltd.). Measurement conditions may be set to, for example, an acceleration voltage of 10 kV, a beam current of 10 nA, and an analysis area The content of a specified element contained in the 10 particles is averaged to calculate the content.

[0062] Note that the EDX analysis and AES analysis are performed on a region that is 1 μm or more inward from the peripheral edge of the cross-section of the composite particle.

[0063] <ICP>

[0064] A sample of the composite particles is completely dissolved in a heated acid solution (a mixed acid of hydrofluoric acid, nitric acid, and sulfuric acid), and the carbon in the solution residue is filtered and removed. Thereafter, the obtained filtrate is analyzed by inductively coupled plasma atomic emission spectrometry (ICP) to measure the spectral intensity of each element. Then, a calibration curve is prepared using commercially available standard solutions of each element to calculate the content of each element contained in the composite particles.

[0065] In addition, the quantification of each element can also be performed using an electron probe microanalyzer (EPMA), laser ablation ICP mass spectrometry (LA-ICP-MS), X-ray photoelectron spectroscopy (XPS), or the like.

[0066] Furthermore, the contents of B, Na, K, and Al contained in the composite particles can also be quantitatively analyzed in accordance with JIS R3105 (1995) (Analytical Methods for Borosilicate Glass).

[0067] The content of Ca contained in the composite particles can also be quantitatively analyzed in accordance with JIS R3101 (1995) (Analytical Methods for Soda Lime Glass).

[0068] The carbon content contained in the composite particles can be measured using a carbon / sulfur analyzer (for example, model EMIA-520 manufactured by HORIBA, Ltd.). A sample is weighed on a magnetic plate, a combustion aid is added, and the mixture is inserted into a combustion furnace heated to 1350°C (carrier gas: oxygen). The amount of carbon dioxide gas generated during combustion is detected by infrared absorption. For example, a calibration curve is prepared using a carbon steel (carbon content 0.49%) manufactured by Bureau of Analysed Samples, Ltd., to calculate the carbon content of the sample (high-frequency induction furnace combustion-infrared absorption method).

[0069] The oxygen content contained in the composite particles can be measured using an oxygen / nitrogen / hydrogen analyzer (for example, model EGMA-830 manufactured by HORIBA, Ltd.). A sample is placed in a Ni capsule and introduced into a carbon crucible heated at a power of 5.75 kW together with Sn pellets and Ni pellets serving as a flux, and the released carbon monoxide gas is detected. A calibration curve is prepared using the standard sample Y₂O₃ to calculate the oxygen content of the sample (inert gas fusion-nondispersive infrared absorption method).

[0070] The amount of Si constituting the silicon phase in the composite particles can be quantified by Si-NMR.

[0071] Preferred measurement conditions for Si-NMR are shown below.

[0072] <Si-NMR Measurement Conditions>

[0073] Measurement Apparatus: Varian Solid-State Nuclear Magnetic Resonance Spectrometer (INOVA-400)

[0074] Probe: Varian 7mm CPMAS-2

[0075] MAS: 4.2kHz

[0076] MAS speed: 4kHz

[0077] Pulse: DD (45° pulse + 1H signal collection time for decoupling)

[0078] Repeat time: 1200 seconds to 3000 seconds

[0079] Observation amplitude: 100kHz

[0080] Observation center: around -100ppm

[0081] Signal acquisition time: 0.05 seconds

[0082] Total number of times: 560

[0083] Sample volume: 207.6 mg

[0084] (Silicon phase)

[0085] The silicon phase is the elemental silicon (Si) phase that repeatedly absorbs and releases lithium ions during battery charging and discharging. The capacity is determined by the Faraday reaction involving the silicon phase. Because the silicon phase has a large capacity, it also expands and contracts significantly during charging and discharging. However, since the silicon phase is dispersed within the lithium aluminate phase, the stress generated by the expansion and contraction of the silicon phase is mitigated.

[0086] The silicon phase can be composed of multiple crystallites. The crystallite size of the silicon phase is preferably below 30 nm. When the crystallite size of the silicon phase is below 30 nm, the volume change caused by the expansion and contraction of the silicon phase during charging and discharging can be reduced, further improving cycle characteristics. For example, the isolation of the silicon phase caused by the formation of pores around the silicon phase during contraction is suppressed, thus suppressing the decrease in charge and discharge efficiency. There is no particular limitation on the lower limit of the silicon phase crystallite size; for example, it can be above 1 nm.

[0087] The crystallite size of the silicon phase is more preferably 10 nm or more and 30 nm or less, and even more preferably 15 nm or more and 25 nm or less. When the crystallite size of the silicon phase is 10 nm or more, the surface area of ​​the silicon phase can be suppressed less, and therefore, the degradation of the silicon phase accompanied by irreversible capacity formation is less likely to occur. When the crystallite size of the silicon particles is 30 nm or less, the expansion and contraction of the silicon phase is more easily homogenized, the stress generated in the composite particles is more easily mitigated, and the cyclic properties can be improved. The crystallite size of the silicon phase is calculated from the half-width of the diffraction peaks of the (111) plane belonging to the silicon phase (elemental Si) in the X-ray diffraction pattern according to the Scherer formula.

[0088] Before the first charge, the silicon phase of the composite particles contained in the battery is, for example, granular. The average particle size of the granular silicon phase is preferably 500 nm or less, more preferably 200 nm or less, and even more preferably 50 nm or less. After the first charge, the average particle size of the silicon phase is preferably 400 nm or less, more preferably 100 nm or less. By miniaturizing the silicon phase, the volume change of the composite particles during charging and discharging is reduced, and the structural stability of the composite particles is further improved. The average particle size of the silicon phase is determined using a cross-sectional image of the composite particles obtained by SEM. Specifically, the average particle size of the silicon phase is calculated by averaging the maximum diameters of any 100 silicon phases.

[0089] From the viewpoint of high capacity, the silicon phase content in the composite particles is preferably 30% by mass or more, more preferably 35% by mass or more, and even more preferably 55% by mass or more. In this case, lithium ion diffusion is good, resulting in excellent loading characteristics. On the other hand, from the viewpoint of improving cycle characteristics, the silicon phase content in the composite particles is preferably 95% by mass or less, more preferably 75% by mass or less, and even more preferably 70% by mass or less. In this case, the surface area of ​​the silicon phase exposed without being covered by the silicate phase is reduced, and side reactions between the non-aqueous electrolyte and the silicon phase are easily suppressed.

[0090] (Conductive layer)

[0091] A conductive layer comprising a conductive material can be formed on at least a portion of the surface of the composite particles (secondary particles). This improves the conductivity of the composite particles. The thickness of the conductive layer is preferably substantially thin enough not to affect the average particle size of the composite particles. Considering both ensuring conductivity and lithium-ion diffusion, the thickness of the conductive layer is preferably 1–200 nm, more preferably 5–100 nm. The thickness of the conductive layer can be measured by observing a cross-section of the composite particles using SEM or TEM.

[0092] Conductive carbon materials are preferred as conductive materials. Amorphous carbon, graphite, easily graphitized carbon (soft carbon), and difficult-to-graphitize carbon (hard carbon) can be used as conductive carbon materials. Among these, amorphous carbon is preferred in terms of easily forming a thin conductive layer covering the surface of the composite particles. Examples of amorphous carbon include carbon black, calcined pitch, coke, and activated carbon. Examples of graphite include natural graphite, artificial graphite, and graphitized mesophase carbon.

[0093] [Manufacturing method of composite particles]

[0094] Composite particles can be manufactured, for example, by a manufacturing method including the following steps 1 to 4.

[0095] (Step 1) The process of obtaining lithium aluminate (hereinafter also referred to as raw material aluminate) as raw material.

[0096] (Step 2) The process of combining raw aluminate and raw silicon to disperse the silicon phase within the silicate phase and obtain a composite intermediate.

[0097] (Step 3) The composite intermediate is subjected to heat treatment to obtain a sintered body containing an aluminate phase and a silicon phase dispersed in the aluminate phase.

[0098] (Step 4) The process of crushing the sintered body to obtain composite particles containing an aluminate phase and a silicon phase dispersed within the aluminate phase.

[0099] (Step 1)

[0100] The first step includes, for example, the following steps: step 1a, mixing an aluminum compound, a lithium compound, and a compound containing element M as needed to obtain a mixture; and step 1b, calcining the mixture to obtain a raw aluminate. The calcination of step 1b is, for example, carried out in an oxidizing atmosphere. The calcination temperature of step 1b is preferably 400°C or higher and 1200°C or lower, more preferably 800°C or higher and 1100°C or lower.

[0101] Examples of aluminum compounds include aluminum oxide (Al₂O₃), aluminum hydroxide, and aluminum carbonate. Aluminum compounds can be used alone or in combination of two or more.

[0102] Examples of lithium compounds include lithium carbonate, lithium oxide, lithium hydroxide, and lithium hydride. A single lithium compound can be used alone, or in combination of two or more compounds.

[0103] As compounds containing element M, oxides, hydroxides, hydrides, halides, carbonates, oxalates, nitrates, sulfates, etc., of element M can be used. A single compound containing element M can be used alone, or in combination of two or more.

[0104] In the first step, aluminum compounds that did not react with lithium compounds during the preparation of the raw aluminate may remain in the raw aluminate. When the amount of aluminum compound used is large compared to lithium compounds, aluminum compounds are more likely to remain. If the aluminum compound remaining in the raw aluminate is Al2O3, an Al2O3 phase dispersed within the lithium aluminate phase can be formed in the final composite particles.

[0105] (Step 2)

[0106] The second step includes, for example, the following step: pulverizing a mixture of raw aluminate and raw silicon while applying shear force to the mixture to obtain a micronized composite intermediate. Here, for example, the raw aluminate and raw silicon can be mixed at a predetermined mass ratio, and the mixture can be micronized while stirring using a pulverizing device such as a ball mill.

[0107] The raw silicon can be coarse particles with an average particle size of a few μm to tens of μm. The final silicon particles are preferably controlled by the half-width of the diffraction peaks attributable to the Si(111) plane in the X-ray diffraction pattern and the crystallite size calculated according to the Scherer formula to be 10 nm or more.

[0108] It should be noted that the second step is not limited to the above. For example, silicon nanoparticles and aluminate nanoparticles can be synthesized and mixed without using a pulverizing device.

[0109] (Step 3)

[0110] The third step includes, for example, the following step: while applying pressure to the micronized composite intermediate by hot pressing or the like, the composite intermediate is sintered to obtain a sintered body. The sintering of the composite intermediate is carried out, for example, in an inactive atmosphere (e.g., argon, nitrogen, etc.). The sintering temperature is preferably 50°C or higher and 1000°C or lower. Within this temperature range, it is easy to disperse small silicon particles within the low-crystallinity aluminate phase. The raw material aluminate is stable within the above temperature range and hardly reacts with silicon. The sintering temperature is preferably 550°C or higher and 900°C or lower, more preferably 650°C or higher and 850°C or lower. The sintering time is, for example, 1 hour or higher and 10 hours or lower.

[0111] (Step 4)

[0112] The fourth step is to pulverize the sintered body to obtain composite particles containing an aluminate phase and a silicon phase dispersed within the aluminate phase, in a manner that achieves the desired particle size distribution. The composite particles are pulverized, for example, with an average particle size of 1 to 25 μm.

[0113] (Step 5)

[0114] The method for manufacturing composite particles may further include a fifth step of forming a conductive layer by covering at least a portion of the surface of the composite particles with a conductive material. The conductive material is preferably electrochemically stable, and preferably a conductive carbon material. Examples of methods for covering the surface of the composite particles with a conductive carbon material include CVD methods using hydrocarbon gases such as acetylene or methane as raw materials, and methods of mixing composite particles with coal tar pitch, petroleum tar pitch, phenolic resin, etc., and then heating and carbonizing them. Alternatively, carbon black can be deposited on the surface of the composite particles. In the fifth step, for example, the mixture of composite particles and conductive carbon material is heated in, for example, an inactive atmosphere (e.g., argon, nitrogen, etc.) at a temperature of 700°C or higher and 950°C or lower, thereby forming a conductive layer on the surface of the composite particles.

[0115] Here, Figure 2 This is a schematic cross-sectional view of a negative electrode active material (composite particles) according to an embodiment of the present disclosure.

[0116] The composite particle 20 has a base particle 23 composed of secondary particles formed by the aggregation of multiple primary particles 24. The base particle 23 (primary particles 24) has a lithium aluminate phase 21 and a silicon phase 22 dispersed within the lithium aluminate phase 21. The base particle 23 has an island structure in which a fine silicon phase is dispersed in the matrix of the lithium aluminate phase 21.

[0117] Furthermore, fine Al₂O₃ phase 28 can be dispersed within lithium aluminate phase 21. At least a portion of the surface of the base particles 23 can be covered by conductive layer 26. Lithium aluminate phase 21 may also contain element M. With repeated charging and discharging, adjacent particulate silicon phases 22 connect with each other, forming a network of silicon phases.

[0118] [Non-aqueous electrolyte secondary battery]

[0119] The non-aqueous electrolyte secondary battery of the present disclosure includes a positive electrode, a negative electrode, and a non-aqueous electrolyte, wherein the negative electrode comprises the aforementioned negative electrode active material for a non-aqueous electrolyte secondary battery.

[0120] The following is a detailed explanation of non-aqueous electrolyte secondary batteries.

[0121] [negative electrode]

[0122] The negative electrode may include a negative current collector and a negative electrode additive layer loaded on the surface of the negative current collector. The negative electrode additive layer can be formed by coating a negative electrode slurry containing a negative electrode additive dispersed in a dispersion medium onto the surface of the negative current collector and drying it. The dried coating can be calendered as needed. The negative electrode additive layer can be formed on one surface of the negative current collector or on both surfaces.

[0123] The negative electrode mixture contains a negative electrode active material as an essential component, and may contain binders, conductive agents, thickeners, etc. as optional components. The negative electrode active material must contain at least the aforementioned composite particles.

[0124] The negative electrode active material preferably also includes carbon materials that electrochemically absorb and release lithium ions. Since the composite particles expand and contract in volume during charging and discharging, a higher proportion of these particles in the negative electrode active material can easily lead to poor contact between the negative electrode active material and the negative electrode current collector during charging and discharging. On the other hand, by combining composite particles with carbon materials, it is possible to impart high capacity to the negative electrode from silicon particles while achieving excellent cycle characteristics. From the viewpoint of high capacity and improved cycle characteristics, the proportion of carbon materials in the total composite particles and carbon materials is preferably 98% by mass or less, more preferably 70% by mass or more and 98% by mass or less, and even more preferably 75% by mass or more and 95% by mass or less.

[0125] Examples of carbon materials include graphite, easily graphitized carbon (soft carbon), and difficult-to-graphitize carbon (hard carbon). Among these, graphite is preferred due to its excellent charge-discharge stability and low irreversible capacity. Graphite refers to materials with a graphitic crystal structure, such as natural graphite, artificial graphite, and graphitized mesophase carbon particles. Carbon materials can be used alone or in combination of two or more types.

[0126] As the negative current collector, a non-porous conductive substrate (such as metal foil) or a porous conductive substrate (such as a sieve, mesh, or perforated plate) can be used. Examples of materials for the negative current collector include stainless steel, nickel, nickel alloys, copper, and copper alloys. The thickness of the negative current collector is not particularly limited; however, from the viewpoint of balancing strength and lightweight, 1–50 μm is preferred, and 5–20 μm is even more ideal.

[0127] Examples of adhesives include resin materials such as fluoropolymers like polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVDF); polyolefin resins like polyethylene and polypropylene; polyamide resins like aromatic polyamide resins; polyimide resins like polyimide and polyamide-imide; acrylic resins like polyacrylic acid, polymethyl acrylate, and ethylene-acrylic acid copolymers; vinyl resins like polyacrylonitrile and polyvinyl acetate; polyvinylpyrrolidone; polyethersulfone; and rubber-like materials like styrene-butadiene copolymer rubber (SBR). An adhesive can be used alone or in combination of two or more types.

[0128] Examples of conductive agents include carbon-based conductive agents such as acetylene black; conductive fibers such as carbon fibers and metal fibers; fluorinated hydrocarbons; metal powders such as aluminum; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and organic conductive materials such as phenylene derivatives. A single conductive agent can be used, or two or more can be used in combination.

[0129] Examples of thickeners include carboxymethyl cellulose (CMC) and its modified forms (including salts such as Na salts), cellulose derivatives such as methyl cellulose (cellulose ethers, etc.); saponifications of polymers containing vinyl acetate units such as polyvinyl alcohol; and polyethers (polyethylene oxide, polyoxyethylene, etc.). Thickeners can be used alone or in combination of two or more.

[0130] There are no particular limitations on the dispersion medium; for example, water, alcohols such as ethanol, ethers such as tetrahydrofuran, amides such as dimethylformamide, N-methyl-2-pyrrolidone (NMP), or mixtures thereof can be used.

[0131] [positive electrode]

[0132] The positive electrode may include a positive current collector and a positive electrode additive layer loaded on the surface of the positive current collector. The positive electrode additive layer can be formed by coating a positive electrode slurry containing a positive electrode additive dispersed in a dispersion medium onto the surface of the positive current collector and drying it. The dried coating can be calendered as needed. The positive electrode additive layer can be formed on one surface of the positive current collector or on both surfaces. The positive electrode additive contains essential components for the positive electrode active material and may include binders, conductive agents, etc., as arbitrary components. NMP or similar materials are used as the dispersion medium for the positive electrode slurry.

[0133] As a positive electrode active material, lithium-containing composite oxides can be used, for example. Li can be cited as an example. a CoO2, Li a NiO2, Li a MnO2, Li a Co b Ni 1-b O2, Li a Co b Me 1-b O c Li a Ni 1-b Me b O c Li a Mn2O4, Li a Mn 2-b Me b O4, LiMePO4, Li2MePO4F (Me is selected from at least one element chosen from the group consisting of Na, Mg, Sc, Y, Mn, Fe, Co, Ni, Cu, Zn, Al, Cr, Pb, Sb, and B). Here, a = 0–1.2, b = 0–0.9, and c = 2.0–2.3. It should be noted that the value of a, representing the molar ratio of lithium, increases or decreases depending on the charge and discharge cycle.

[0134] Among them, preferred is Li a Ni b Me 1-b O2 (Me is at least one selected from the group consisting of Mn, Co, and Al, 0<a≤1.2, 0.3≤b≤1.) The lithium nickel composite oxide represented by the formula. From the viewpoint of increasing capacity, it is more preferable to satisfy 0.85≤b<1. From the viewpoint of crystal structure stability, further preferred is Li containing Co and Al as Me a Ni b Co c Al d O2 (0<a≤1.2, 0.85≤b<1, 0<c<0.15, 0<d≤0.1, b+c+d=1).

[0135] As the binder and conductive agent, the same substances as those exemplified for the negative electrode can be used. As the conductive agent, graphite such as natural graphite and artificial graphite can also be used.

[0136] The shape and thickness of the positive electrode current collector can be selected from those conforming to the shape and range of the negative electrode current collector, respectively. Examples of the material of the positive electrode current collector include stainless steel, aluminum, aluminum alloys, and titanium.

[0137] [Non-aqueous electrolyte]

[0138] The non-aqueous electrolyte contains a non-aqueous solvent and a lithium salt dissolved in the non-aqueous solvent. The concentration of the lithium salt in the non-aqueous electrolyte is, for example, preferably 0.5 mol / L or more and 2 mol / L or less. By setting the lithium salt concentration within the above range, a non-aqueous electrolyte with excellent ionic conductivity and moderate viscosity can be obtained. However, the lithium salt concentration is not limited to the above.

[0139] As the non-aqueous solvent, for example, cyclic carbonates, chain carbonates, cyclic carboxylic acid esters, chain carboxylic acid esters, and the like are used. Examples of the cyclic carbonate include propylene carbonate (PC), ethylene carbonate (EC), and the like. Examples of the chain carbonate include diethyl carbonate (DEC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), and the like. Examples of the cyclic carboxylic acid ester include γ-butyrolactone (GBL), γ-valerolactone (GVL), and the like. Examples of the chain carboxylic acid ester include methyl formate, ethyl formate, propyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, and the like. The non-aqueous solvent may be used alone or in combination of two or more.

[0140] Examples of the lithium salt include LiClO4, LiBF4, LiPF6, LiAlCl4, LiSbF6, LiSCN, LiCF3SO3, LiCF3CO2, LiAsF6, LiB 10 Cl10 Examples of borates include lower aliphatic carboxylic acids such as lithium, LiCl, LiBr, LiI, borates, and imide salts. Examples of borates include lithium bis(1,2-phenylene glycol 2-O,O')borate, lithium bis(2,3-naphthalene glycol 2-O,O')borate, lithium bis(2,2'-biphenylene glycol 2-O,O')borate, and lithium bis(5-fluoro-2-ol 1-benzenesulfonic acid 2-O,O')borate. Examples of lithium bis(fluorosulfonyl)imide (LiN(FSO2)2), lithium bis(trifluoromethanesulfonyl)imide (LiN(CF3SO2)2), lithium trifluoromethanesulfonate nonafluorobutanesulfonylimide (LiN(CF3SO2)(C4F9SO2)), and lithium bis(pentafluoroethylsulfonyl)imino (LiN(C2F5SO2)2) are examples of lithium bis(fluoroethylsulfonyl)imino. LiPF6 is preferred. A single lithium salt can be used alone, or two or more can be used in combination.

[0141] [Separator]

[0142] Typically, it is desirable to sandwich the separator between the positive and negative electrodes. The separator should have high ion permeability, moderate mechanical strength, and insulation properties. Microporous membranes, woven fabrics, and non-woven fabrics can be used as separators. Polyolefins such as polypropylene and polyethylene are preferred materials for the separator.

[0143] As an example of the structure of a non-aqueous electrolyte secondary battery, one can exemplify a structure in which an electrode assembly consisting of a positive and a negative electrode wound together with a separator and housed together with a non-aqueous electrolyte in a casing. However, this is not a limitation, and other forms of electrode assemblies can also be used. For example, a stacked electrode assembly consisting of a positive and a negative electrode layered together with a separator can be used. The shape of the non-aqueous electrolyte secondary battery is also not limited; for example, it can be cylindrical, square, coin-shaped, button-shaped, laminated, etc.

[0144] The following is a reference. Figure 3 The structure of a square non-aqueous electrolyte secondary battery, which is an example of a non-aqueous electrolyte secondary battery disclosed herein, will be described.

[0145] The battery comprises: a square-shaped battery casing 4, and an electrode assembly 1 and a non-aqueous electrolyte housed within the battery casing 4. The electrode assembly 1 has a long strip-shaped negative electrode, a long strip-shaped positive electrode, and a separator sandwiched between them. The negative electrode current collector is electrically connected to a negative terminal 6 located on a sealing plate 5 via a negative electrode lead 3. The negative terminal 6 is insulated from the sealing plate 5 by a resin gasket 7. The positive electrode current collector is electrically connected to the back of the sealing plate 5 via a positive electrode lead 2. That is, the positive electrode is electrically connected to the battery casing 4, which also has a positive terminal. The periphery of the sealing plate 5 is fitted into the open end of the battery casing 4, and the fitting is laser-welded. The sealing plate 5 has an injection hole for the non-aqueous electrolyte, which is blocked by a sealing plug 8 after electrolyte injection.

[0146] The present disclosure will now be described in detail based on embodiments and comparative examples, but the present invention is not limited to the following embodiments.

[0147] <Examples 1-10>

[0148] [Preparation of composite particles (LAX particles)]

[0149] (Step 1)

[0150] Al₂O₃ and Li₂CO₃ were mixed and calcined in air at 950°C for 10 hours to obtain the raw aluminate. The molar ratio of Al₂O₃ to Li₂CO₃ in the mixture was set as shown in Table 1. The raw aluminate was pulverized to achieve an average particle size of 10 μm.

[0151] (Step 2)

[0152] Next, the aluminate (average particle size 10 μm) and silicon (3N, average particle size 10 μm) were mixed. The mass ratio of the aluminate to the silicon in the mixture was set as shown in Table 1.

[0153] Fill the mixture into the jar (SUS, volume: 500mL) of a planetary ball mill (Fritsch P-5), place 24 SUS balls (20mm in diameter) into the jar, close the lid, and pulverize the mixture at 200rpm for 50 hours in an inactive atmosphere.

[0154] (Step 3)

[0155] Next, in an inactive atmosphere, the powdered mixture is taken out and sintered at 800°C for 4 hours in an inactive atmosphere using a hot press while applying pressure, to obtain a sintered body of the mixture.

[0156] (Step 4)

[0157] The obtained sintered body was crushed and passed through a 40μm sieve to obtain composite particles.

[0158] (Step 5)

[0159] The composite particles were mixed with coal tar pitch (manufactured by JFE Chemical Co., Ltd., MCP250). The mixture was calcined at 800°C for 5 hours in an inert atmosphere to form a conductive layer containing conductive carbon material on the surface of the composite particles. The coverage of the conductive layer was set to 5% by mass relative to the total mass of the composite particles and the conductive layer. Then, using a sieve, composite particles (LAX particles with a silicon phase dispersed within the lithium aluminate phase) with an average particle size of 5 μm and a conductive layer were obtained.

[0160] The XRD patterns of the LAX particles obtained by XRD analysis confirmed peaks originating from the silicon phase and the lithium aluminate phase. Peaks originating from the Al₂O₃ phase were also confirmed in particles LAX1–LAX3 and LAX6–LAX8. The crystallite size of the silicon phase in the LAX particles, determined by the method described, is 15 nm.

[0161] Based on the composition of the lithium aluminate phase obtained by the method described above and the amount of Si constituting the silicon phase in the LAX particles, the Li content ratio (MLi), Si content ratio (MSi), and Al content ratio (MAl) in the LAX particles were determined. The values ​​of each content ratio are shown in Table 1.

[0162] [Making the negative electrode]

[0163] Composite particles with a conductive layer were mixed with graphite at a mass ratio of 5:95 to serve as the negative electrode active material. A negative electrode slurry was prepared by adding water and stirring to a negative electrode mixture containing the negative electrode active material, Na salt of CMC, and SBR at a mass ratio of 97.5:1:1.5. Next, the negative electrode slurry was coated onto the surface of copper foil, and after the coating dried, it was calendered to form a layer with a density of 1.5 g / cm³ on both sides of the copper foil. 3 The negative electrode of the negative electrode compound layer.

[0164] [The production of the positive electrode]

[0165] NMP was added to a cathode mixture containing lithium cobalt oxide, acetylene, and PVDF in a mass ratio of 95:2.5:2.5, and the mixture was stirred to prepare a cathode slurry. Next, the cathode slurry was coated onto the surface of aluminum foil, and after the coating dried, it was calendered to form a cathode with a density of 3.6 g / cm³ on both sides of the aluminum foil. 3 The positive electrode of the positive electrode layer.

[0166] [Preparation of non-aqueous electrolytes]

[0167] A non-aqueous electrolyte was prepared by dissolving LiPF6 at a concentration of 1.0 mol / L in a mixed solvent containing EC and DEC in a volume ratio of 3:7.

[0168] [Construction of a non-aqueous electrolyte secondary battery]

[0169] A positive and negative electrode assembly, each equipped with tabs, is wound together with a separator to create an electrode assembly with the tabs located at the outermost periphery. The electrode assembly is inserted into a casing made of aluminum laminated film, and after vacuum drying at 105°C for 2 hours, a non-aqueous electrolyte is injected. The opening of the casing is then sealed to obtain a non-aqueous electrolyte secondary battery. In Table 1, LAX1-10 and A1-A10 represent the composite particles and batteries of Examples 1-10.

[0170] <Comparative Example 1>

[0171] In the second step, silicate is used instead of aluminate. Silicate (average particle size 10 μm) and silicon (3N, average particle size 10 μm) are mixed at a mass ratio of 25:75. The silicate is mixed with SiO2 at a molar ratio of SiO2:Li2CO3 = 70:30. The mixture is then calcined in air at 950°C for 10 hours to obtain the final product. The silicate is then pulverized to achieve an average particle size of 10 μm.

[0172] In addition to the above, composite particles with a conductive layer (LSX particles with silicon phase dispersed in lithium silicate phase) were obtained by the same method as in Example 1.

[0173] The XRD patterns of LSX particles obtained by XRD analysis confirmed peaks originating from the lithium silicate phase (Li2Si2O5 and Li2SiO3) and the silicon phase. The crystallite size of the silicon phase in the LSX particles was 15 nm.

[0174] Battery B1 was fabricated using LSX particles with conductive layers instead of LAX1 particles with conductive layers, except that the battery was fabricated using the same method as in Example 1.

[0175] For each battery obtained above, the initial charge-discharge efficiency is calculated using the following method.

[0176] [Initial charge / discharge efficiency]

[0177] <Charging>

[0178] At 25°C, a constant current of 1It (800mA) is applied until the voltage reaches 4.2V, and then a constant voltage of 4.2V is applied until the current reaches 1 / 20It (40mA).

[0179] <Discharge>

[0180] After a 10-minute pause, a constant current discharge of 1 It (800 mA) was applied at 25°C until the voltage reached 2.75V.

[0181] For each battery, the charging capacity and discharging capacity were calculated based on the above charging and discharging methods. The ratio of the discharging capacity to the charging capacity was then used as the initial charge-discharge efficiency. In Table 1, the initial charge-discharge efficiency value obtained from battery B1 of Comparative Example 1 was set to 100, and the initial charge-discharge efficiency value of each battery was expressed as a relative value. The evaluation results are shown in Table 1.

[0182] [Table 1]

[0183]

[0184] Batteries A1 to A10, which use LAX particles, exhibit higher initial charge-discharge efficiency compared to battery B1, which uses LSX particles. In particular, batteries A2 to A4 and A7 to A9 show even higher initial charge-discharge efficiency.

[0185] Industrial availability

[0186] The non-aqueous electrolyte secondary battery disclosed herein is useful as a main power source for mobile communication devices, portable electronic devices, and the like.

[0187] Explanation of reference numerals in the attached figures

[0188] Electrode group 1

[0189] 2 Positive leads

[0190] 3 negative leads

[0191] 4 Battery casing

[0192] 5 sealing boards

[0193] 6 negative extremes

[0194] 7 gaskets

[0195] 8 sealing plugs

[0196] 20 composite particles

[0197] 21 Lithium Aluminate Phase

[0198] 22 silicon phase

[0199] 23 basic particles

[0200] 24 granules

[0201] 26 conductive layers

[0202] 28Al2O3 phase

Claims

1. A negative electrode active material for a non-aqueous electrolyte secondary battery, comprising composite particles, said composite particles comprising: a lithium aluminate phase and a silicon phase dispersed within said lithium aluminate phase, The content of the silicon phase in the composite particles is more than 55% by mass and less than 75% by mass. In the composite particles, the aluminum content (MAl) relative to the total amount of elements other than oxygen is 11.50% by mass or more and 45.5% by mass or less. The lithium content (MLi) relative to the total amount of elements other than oxygen is 1.0% by mass or more and 9.5% by mass or less.

2. The negative electrode active material for a nonaqueous electrolyte secondary battery according to claim 1, wherein The ratio of aluminum (MAl) to lithium (MLi) is: MAl / MLi is 2 or more and 20 or less.

3. The negative electrode active material for a non-aqueous electrolyte secondary battery according to claim 1 or 2, wherein, The lithium aluminate phase comprises at least one selected from the group consisting of LiAl5O8, Li2Al4O7, LiAlO2, and Li5AlO4.

4. The negative electrode active material for a non-aqueous electrolyte secondary battery according to claim 1 or 2, wherein, The X-ray diffraction pattern of the composite particles obtained by X-ray diffraction measurement. The peak originating from the lithium aluminate phase appears near 2θ=x°. The x° is selected from at least one of the groups consisting of 19.4°, 22.3°, 31.9°, 34.3° and 37.5°.

5. The negative electrode active material for a non-aqueous electrolyte secondary battery according to claim 1 or 2, wherein, The lithium aluminate phase contains an Al2O3 phase.

6. The negative electrode active material for a non-aqueous electrolyte secondary battery according to claim 5, wherein, In the X-ray diffraction pattern of the composite particles obtained by X-ray diffraction, the peak originating from the Al2O3 phase appears near 2θ=25.4°.

7. The negative electrode active material for a non-aqueous electrolyte secondary battery according to claim 1 or 2, wherein, The lithium aluminate phase comprises at least one element selected from the group consisting of sodium, potassium, calcium, magnesium, zirconium, iron, boron, phosphorus and lanthanum.

8. A non-aqueous electrolyte secondary battery, comprising: a positive electrode, a negative electrode, and a non-aqueous electrolyte. The negative electrode comprises the negative electrode active material for a non-aqueous electrolyte secondary battery as described in any one of claims 1 to 7.

Citation Information

Patent Citations

  • Negative electrode active material for nonaqueous electrolyte secondary batteries, and nonaqueous electrolyte secondary battery

    WO2016035290A1

  • Negative active material for lithium secondary battery and manufacturing method thereof

    JP2007500421A