A method for improving the initial coulomb efficiency and energy density of a sodium-ion battery, a positive electrode slurry, a positive electrode sheet, and a sodium-ion battery
By using sodium bicarbonate as a sodium supplement additive in the positive electrode of sodium-ion batteries, the problems of low initial coulombic efficiency and slurry gelation are solved, thereby improving the battery's energy density and stability, making it suitable for the industrial production of sodium-ion batteries.
Patent Information
- Application Number
- CN202310758275.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-26
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-06-26
AI Technical Summary
Sodium-ion batteries have a low initial coulombic efficiency, which limits the improvement of energy density. Existing cathode pre-sodiumification technology has stability problems and processing difficulties, especially the sodium carbonate additive is unstable and easily causes slurry gelation.
Sodium bicarbonate is used as a sodium supplement additive in the positive electrode. During the coating process, it decomposes upon heating to generate sodium carbonate, which in situ generates sodium-rich chemicals to supplement Na⁺ in the battery system, improves the initial coulombic efficiency and energy density, and avoids the problem of slurry gelation.
It improves the initial coulombic efficiency and energy density of sodium-ion batteries, avoids slurry gelation, is suitable for industrial production, and enhances battery performance.
Smart Images

Figure BDA0004303686360000061
Abstract
Description
Technical Field
[0001] This invention relates to the field of sodium-ion secondary battery technology, specifically to a method for improving the initial coulombic efficiency and energy density of sodium-ion batteries, a positive electrode slurry, a positive electrode sheet, and a sodium-ion battery. Background Technology
[0002] Compared to lithium-ion batteries, sodium-ion batteries have significant cost advantages and a sustainable resource supply, making them an ideal alternative. However, the low initial coulombic efficiency of sodium-ion battery anode materials restricts further improvements in energy density and the industrialization of sodium-ion batteries. The low initial coulombic efficiency is mainly due to the fact that sodium ions released from the positive electrode during the first charge react at the negative electrode, forming an SEI film or undergoing other side reactions, resulting in the loss of active sodium ions. Consequently, during discharge, an equal number of sodium ions cannot be released from the negative electrode back to the positive electrode, leading to lower cell capacity.
[0003] To improve the initial coulombic efficiency and energy density of sodium-ion batteries, pre-sodiuming technology is commonly used in existing technologies. The principle of pre-sodiuming is to add extra active sodium to the negative or positive electrode materials beforehand to compensate for the irreversible capacity loss during the first charge-discharge cycle, thereby significantly improving the overall battery energy density and cycle life. The main methods of pre-sodiuming include negative electrode pre-sodiuming and positive electrode pre-sodiuming. Negative electrode pre-sodiuming includes physical pre-sodiuming (physically combining sodium powder or sodium foil with the electrode active material to be treated) and chemical reaction pre-sodiuming (using a highly reducing chemical sodium-adding reagent to chemically supplement sodium in the sodium-ion battery electrode materials). While negative electrode pre-sodiuming can supplement sodium to some extent, sodium metal has high reactivity and readily reacts with water and oxygen, thus requiring strict anhydrous and oxygen-free environments, which is not conducive to industrialization. Furthermore, treatment with chemical sodium-adding reagents can leave residual reagents that are difficult to remove completely. Positive electrode pre-sodiuming refers to adding sodium-adding additives to the positive electrode slurry, causing irreversible decomposition during the first charging cycle to release sufficient active sodium. This method is simpler, more practical, and beneficial for industrial production. There are many types of sodium-replenishing additives, mainly inorganic compounds, including Na₂CO₃, NaN₃, Na₃P, NaCrO₂, and Na₂C₄O₄. However, these cathode sodium-replenishing additives have some drawbacks. For example, NaN₃ and Na₃P are extremely unstable in air, and residual phosphorus may react with active materials or electrolytes, reducing battery energy density. Na₂CO₃ is strongly alkaline, and high residual alkali on the surface of sodium battery cathode materials can easily cause cathode slurry gelation. Adding Na₂CO₃ will further deteriorate the cathode slurry state, increasing the risk of cathode slurry processing failure. Therefore, it is necessary to find inexpensive, safe, efficient, and industrially suitable sodium-rich compounds as cathode sodium-replenishing additives that can improve the initial coulombic efficiency of sodium-ion batteries, have minimal impact on cathode slurry stability, and avoid causing cathode slurry gelation and processing difficulties. Summary of the Invention
[0004] To address the shortcomings of existing technologies, this invention provides a method for improving the initial coulombic efficiency and energy density of sodium-ion batteries. This method effectively solves the problem of low initial coulombic efficiency of sodium storage anode materials, which restricts the development of high-energy-density sodium-ion batteries, while avoiding the problem of positive electrode slurry gelation.
[0005] The objective of this invention is achieved through the following technical solutions.
[0006] A method for improving the initial coulombic efficiency and energy density of sodium-ion batteries includes the following steps:
[0007] The adhesive and organic solvent are first mixed to obtain an adhesive solution;
[0008] The positive electrode active material, conductive agent and sodium bicarbonate are mixed a second time to obtain a mixture;
[0009] A portion of the binder solution is first added to the mixture, kneaded, and then the remaining binder solution is added. After a third mixing, a positive electrode slurry is obtained.
[0010] The sodium bicarbonate comprises 1.5% to 4.5% of the total weight of the binder, organic solvent, positive electrode active material, and conductive agent.
[0011] The sodium bicarbonate (NaHCO3) additive used in this invention is a weakly alkaline compound, which has minimal impact on the stability of the positive electrode slurry and will not cause problems such as slurry gelation or processing difficulties. During the coating process, sodium bicarbonate decomposes upon heating (2NaHCO3→Na2CO3+H2O↑+CO2↑), generating sodium-rich sodium carbonate (Na2CO3) in situ. The remaining products evaporate with the solvent. At this point, the electrode coating has dried and formed on the current collector, and there is no problem with slurry gelation. When the battery is first charged to 4.0V, sodium carbonate (Na2CO3) decomposes (2Na2CO3→2CO2↑+O2↑+4Na + +4e - Based on the sodium bicarbonate (NaHCO3) additive, the theoretical sodium supplementation capacity can reach 319 mAh / g, and the generated Na + It enters the electrolyte to directly replenish the Na consumed by the negative electrode material during the formation of SEI in the first charge. + This improves the initial coulombic efficiency of sodium-ion secondary batteries. The decomposition products, CO2 and O2 gases, are removed during the battery degassing process, which further increases the battery energy density.
[0012] This invention uses sodium bicarbonate as a sodium supplement, ultimately resulting in only sodium in the battery. + The byproducts are all in gaseous form and leave the battery during the sodium-ion battery manufacturing process, thus achieving sodium replenishment without affecting the battery formulation ratio or increasing battery weight. Furthermore, compared to the direct addition of sodium carbonate in existing technologies, this invention generates sodium carbonate in situ during the slurry coating process. At this point, the electrode coating has already dried and formed on the current collector, avoiding the problem of slurry gelation. Using sodium bicarbonate as a sodium replenishment additive in this invention can improve the initial coulombic efficiency of sodium-ion batteries while effectively avoiding the slurry gelation problem associated with using sodium carbonate.
[0013] The method of the present invention first adds a portion of binder solution to the positive electrode active material, conductive agent and sodium bicarbonate, which can increase the viscosity of the slurry and increase the "collision" and "tearing" effect of particles within and between the above components during the dispersion process, thereby making the slurry more uniformly dispersed.
[0014] Preferably, by weight, the binder comprises 0.6 to 2.4 parts, the organic solvent comprises 20 to 40 parts, the positive electrode active material comprises 49.8 to 78.4 parts, and the conductive agent comprises 0.6 to 3.2 parts.
[0015] Preferably, the weight of the sodium bicarbonate is 1.5% to 4.5% of the total weight of the binder, organic solvent, positive electrode active material, and conductive agent.
[0016] Preferably, the initial charge cutoff potential of the sodium-ion battery is greater than the decomposition potential of sodium carbonate.
[0017] Preferably, the specific operation of the first mixing is as follows: first, stir at a revolution speed of 5-20 rpm and a rotation speed of 400-1000 rpm for 5-10 minutes, and then stir at a revolution speed of 15-30 rpm and a rotation speed of 1200-2000 rpm for 30-120 minutes.
[0018] Preferably, the second mixing operation is as follows: stirring at a revolution speed of 10-25 rpm and a rotation speed of 400-1000 rpm for 5-10 minutes.
[0019] Preferably, 60% to 90% of the adhesive solution is added first, and kneaded for 30 to 90 minutes at a revolution speed of 5 to 20 rpm and a rotation speed of 0 rpm, and then 10% to 40% of the adhesive solution is added.
[0020] Preferably, the third mixing operation is as follows: stirring at a revolution speed of 15-30 rpm and a rotation speed of 1200-2000 rpm for 30-120 minutes.
[0021] This invention first adds 60%–90% of a binder solution to the positive electrode active material, conductive agent, and sodium bicarbonate to increase the consistency of the slurry. High-consistency, low-speed stirring is then performed to disperse and coat the positive electrode active material, conductive agent, and binder, achieving uniform coating of the positive electrode active material by the conductive agent and binder. Then, the remaining 10%–40% of the binder solution is added, and low-consistency, high-speed stirring is performed to further disperse the phase components evenly and stabilize the solid-liquid suspension system, resulting in a positive electrode slurry with excellent coating and processing performance.
[0022] Preferably, the positive electrode active material includes at least one of layered oxide, sodium vanadium phosphate, sodium vanadium fluorophosphate, sodium cobaltate, sodium manganate, sodium nickelate, and Prussian blue.
[0023] The present invention also provides a positive electrode slurry, which is prepared by the method described above.
[0024] The present invention also provides a positive electrode sheet, comprising a positive current collector and a positive active material layer disposed on at least one surface of the positive current collector, wherein the positive active material layer comprises the positive slurry prepared by the method.
[0025] The present invention also provides a sodium-ion secondary battery, including the positive electrode plate.
[0026] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0027] (1) In this invention, sodium bicarbonate is used as a sodium-replenishing additive for the positive electrode. Sodium bicarbonate decomposes in situ during the coating process to produce sodium-rich sodium carbonate. Sodium carbonate decomposes during the first charge of the battery to produce Na. + Replenish Na consumed in the battery system + This improves the initial coulombic efficiency and battery energy density, while the byproducts CO2 and O2 gases are removed during the battery degassing process, ultimately leaving only Na in the battery. + The byproducts are all in gaseous form and leave the battery during the sodium-ion battery manufacturing process, thus achieving sodium replenishment without affecting the battery formula ratio.
[0028] (2) The present invention uses sodium bicarbonate as a sodium supplement additive, which can effectively replenish the Na consumed in the battery system. + This also effectively avoids the problem of slurry gelation caused by directly using sodium carbonate as a sodium supplement. Detailed Implementation
[0029] The applicant will now provide a detailed description of the method of the present invention in conjunction with specific embodiments, with the aim of enabling those skilled in the art to clearly understand the present invention.
[0030] The following embodiments are merely illustrative examples of specific implementations of the present invention. The described embodiments are only a part of the embodiments of the present invention, but the following embodiments should not be construed in any way as limiting the scope of protection claimed in the claims of the present invention.
[0031] The preferred method of the present invention for improving the initial coulombic efficiency and energy density of sodium-ion batteries includes the following steps:
[0032] S1. Mix 0.6 to 2.4 parts of binder and 20 to 40 parts of organic solvent in a first mixing to obtain binder solution; mix 49.8 to 78.4 parts of positive electrode active material, 0.6 to 3.2 parts of conductive agent and 1.5 to 4.5 parts of sodium bicarbonate in a second mixing to obtain mixture;
[0033] S2. First, add 60% to 90% of the binder solution to the mixture, knead it, and then add the remaining binder solution. After a third mixing, the positive electrode slurry is obtained.
[0034] S3. The positive electrode slurry is coated onto the current collector to obtain a positive electrode sheet, and then assembled into a sodium-ion battery.
[0035] As an optional embodiment, the positive electrode active material of the sodium-ion battery of the present invention may be selected from at least one of layered oxides, sodium vanadium phosphate, sodium vanadium fluorophosphate, sodium cobaltate, sodium manganate, sodium nickelate, and Prussian blue; the binder may be selected from at least one of polytetrafluoroethylene, polyvinylidene fluoride (PVDF), sodium carboxymethyl cellulose, and styrene-butadiene rubber; the organic solvent may be selected from at least one of N-methylpyrrolidone (NMP), dimethyl sulfoxide, tetrahydrofuran, ketones, and lactones; and the conductive agent may be selected from at least one of conductive carbon black (Super P), graphene, carbon nanotubes, Ketjen black, acetylene black, and carbon nanofibers.
[0036] Example 1
[0037] This embodiment provides a method for improving the initial coulombic efficiency and energy density of sodium-ion batteries, including the following steps:
[0038] S1. Add 2.0 parts of PVDF adhesive and 25 parts of NMP organic solvent to a mixing tank. First, stir for 10 min at a revolution speed of 10 rpm and a rotation speed of 600 rpm to premix. Then, stir for 90 min at a revolution speed of 25 rpm and a rotation speed of 1800 rpm to obtain the adhesive solution for later use.
[0039] S2. Add 70.5 parts of the positive electrode active material nickel-iron-manganese ternary layered oxide, 2.5 parts of the conductive agent Super P, and 1.5 parts of the sodium supplement additive sodium bicarbonate to the mixing tank, and stir for 10 minutes at a revolution speed of 20 rpm and a rotation speed of 800 rpm; then add 70% of the binder solution obtained in step S1, and knead for 60 minutes at a revolution speed of 15 rpm and a rotation speed of 0 rpm to make the binder, conductive agent, and positive electrode active material evenly dispersed and coated; then add the remaining 30% of the binder solution, and stir for 90 minutes at a revolution speed of 25 rpm and a rotation speed of 1800 rpm to make the components of each phase evenly dispersed, the solid-liquid suspension system stable, and the homogenization completed to obtain the positive electrode slurry;
[0040] S3. After homogenization, the positive electrode is obtained by coating, drying and forming; then, the positive electrode is obtained by stacking, encapsulation, liquid injection, activation, formation, volume determination, Degas evacuation encapsulation, edge folding and adhesive application.
[0041] The manufacturing process in step S3 is a conventional method for producing batteries known to those skilled in the art. The negative electrode material can be selected from hard carbon, soft carbon, titanium-based materials (Na2Ti3O7), organic polymer-based materials (disodium terephthalate), metal compound-based materials (molybdenum disulfide), etc.
[0042] Example 2
[0043] The method in this embodiment is basically the same as that in embodiment 1, except that the sodium bicarbonate additive is 3.0 parts by weight.
[0044] Example 3
[0045] The method in this embodiment is basically the same as that in embodiment 1, except that the sodium bicarbonate additive is used in 4.5 parts by weight.
[0046] Example 4
[0047] This embodiment provides a method for improving the initial coulombic efficiency and energy density of sodium-ion batteries, including the following steps:
[0048] S1. Add 2.2 parts of PVDF adhesive and 28.0 parts of NMP organic solvent to a mixing tank. First, stir for 10 minutes at a revolution speed of 20 rpm and a rotation speed of 400 rpm to premix. Then, stir for 60 minutes at a revolution speed of 15 rpm and a rotation speed of 2000 rpm to obtain the adhesive solution for later use.
[0049] S2. Add 67.0 parts of the positive electrode active material nickel-iron-manganese ternary layered oxide, 3.0 parts of the conductive agent Super P, and 1.4 parts of the sodium supplement additive sodium bicarbonate to the mixing tank, and stir for 10 min at a revolution speed of 10 rpm and a rotation speed of 1000 rpm; then add 60% of the binder solution obtained in step S1, and knead for 90 min at a revolution speed of 10 rpm and a rotation speed of 0 rpm to make the binder, conductive agent, and positive electrode active material evenly dispersed and coated; then add the remaining 40% of the binder solution, and stir for 90 min at a revolution speed of 15 rpm and a rotation speed of 2000 rpm to make the components of each phase evenly dispersed, the solid-liquid suspension system stable, and the homogenization completed to obtain the positive electrode slurry;
[0050] S3. After homogenization, the positive electrode is obtained by coating, drying and forming; then, the positive electrode is obtained by stacking, encapsulation, liquid injection, activation, formation, volume determination, Degas evacuation encapsulation, edge folding and adhesive application.
[0051] Example 5
[0052] This embodiment provides a method for improving the initial coulombic efficiency and energy density of sodium-ion batteries, including the following steps:
[0053] S1. Add 1.8 parts of PVDF adhesive and 21.5 parts of NMP organic solvent to a mixing tank. First, stir at 5 rpm and 800 rpm for 10 min to premix. Then, stir at 30 rpm and 2000 rpm for 60 min to obtain the adhesive solution for later use.
[0054] S2. Add 74.0 parts of the positive electrode active material nickel-iron-manganese ternary layered oxide, 2.8 parts of the conductive agent Super P, and 1.6 parts of the sodium supplement additive sodium bicarbonate to the mixing tank, and stir for 10 min at a revolution speed of 25 rpm and a rotation speed of 500 rpm; then add 90% of the binder solution obtained in step S1, and knead for 60 min at a revolution speed of 20 rpm and a rotation speed of 0 rpm to make the binder, conductive agent, and positive electrode active material evenly dispersed and coated; then add the remaining 10% of the binder solution, and stir for 90 min at a revolution speed of 30 rpm and a rotation speed of 1200 rpm to make the components of each phase evenly dispersed, the solid-liquid suspension system stable, and the homogenization completed to obtain the positive electrode slurry;
[0055] S3. After homogenization, the positive electrode is obtained by coating, drying and forming; then, the positive electrode is obtained by stacking, encapsulation, liquid injection, activation, formation, volume determination, Degas evacuation encapsulation, edge folding and adhesive application.
[0056] Comparative Example 1
[0057] The method in this embodiment is basically the same as that in embodiment 1, except that sodium bicarbonate additive is not added in step S2, and the weight proportions of other components are the same as in embodiment 1.
[0058] Comparative Example 2
[0059] The method in this embodiment is basically the same as that in embodiment 1, except that sodium carbonate is used instead of sodium bicarbonate in step S2, and the weight of sodium carbonate is 1.5 parts.
[0060] The results of the initial coulombic efficiency, battery energy density, and fully charged negative electrode state of the sodium-ion secondary batteries of Examples 1-5 and Comparative Examples 1-2 are shown in Table 1.
[0061] Table 1. Initial coulombic efficiency, battery energy density, and fully charged negative electrode state of sodium-ion secondary batteries.
[0062]
[0063] As shown in Table 1, compared with Comparative Example 1 without sodium bicarbonate, Examples 1-3, with the addition of sodium bicarbonate as a sodium-replenishing additive for the positive electrode, significantly improved the initial coulombic efficiency and energy density of the sodium-ion secondary batteries. In particular, when the weight percentage of sodium bicarbonate was 3.0 parts, the initial coulombic efficiency increased from 85% to 95%, completely replenishing the Na+ consumed by the negative electrode material during the first charge to form the SEI film. + Meanwhile, the battery's energy density increased from 150Wh / kg to 168Wh / kg, an increase of 12%. However, when the amount added increased to 4.5 parts, due to the presence of Na in the system... + The amount of Na has exceeded the receiving capacity of the positive electrode, therefore, during discharge, the excess Na... + Unable to return to the positive electrode, the initial coulombic efficiency and battery energy density did not improve further, and sodium deposition occurred at the negative electrode. Compared with Example 1, Examples 4 and 5 adjusted the component dosages and stirring speed while keeping the relative amounts of positive electrode active material and sodium bicarbonate additive unchanged. The improvement in the initial coulombic efficiency and battery energy density of the sodium-ion secondary battery was not significantly different from that of Example 1.
[0064] Comparing Example 1 and Comparative Example 2 reveals that using sodium carbonate as a sodium supplement for the positive electrode causes gelation of the positive electrode slurry, thus affecting its stability. In contrast, using sodium bicarbonate as a sodium supplement for the positive electrode has minimal impact on the stability of the positive electrode slurry, does not cause gelation, and yields a positive electrode slurry with excellent stability.
[0065] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a positive electrode slurry to improve the initial coulombic efficiency and energy density of a sodium-ion battery, characterized in that, Includes the following steps: The adhesive and organic solvent are first mixed to obtain an adhesive solution; the adhesive is selected from at least one of polytetrafluoroethylene, polyvinylidene fluoride, sodium carboxymethyl cellulose, and styrene-butadiene rubber. The positive electrode active material, conductive agent, and sodium bicarbonate are mixed in a second process to obtain a mixture; the positive electrode active material includes at least one of sodium vanadium phosphate, sodium vanadium fluorophosphate, sodium cobaltate, sodium manganate, sodium nickelate, and Prussian blue. A portion of the binder solution is first added to the mixture, kneaded, and then the remaining binder solution is added. After a third mixing, a positive electrode slurry is obtained. Specifically, 60% to 90% of the binder solution is first added, kneaded at a revolution speed of 5 to 20 rpm and a rotation speed of 0 rpm for 30 to 90 minutes, and then 10% to 40% of the binder solution is added. The sodium bicarbonate comprises 1.5% to 4.5% of the total weight of the binder, organic solvent, positive electrode active material, and conductive agent. By weight, the binder comprises 0.6 to 2.4 parts, the organic solvent comprises 20 to 40 parts, the positive electrode active material comprises 49.8 to 78.4 parts, and the conductive agent comprises 0.6 to 3.2 parts.
2. The method for preparing a positive electrode slurry to improve the initial coulombic efficiency and energy density of a sodium-ion battery according to claim 1, characterized in that, The specific operation for the first mixing is as follows: first stir at a revolution speed of 5-20 rpm and a rotation speed of 400-1000 rpm for 5-10 minutes, and then stir at a revolution speed of 15-30 rpm and a rotation speed of 1200-2000 rpm for 30-120 minutes.
3. The method for preparing a positive electrode slurry to improve the initial coulombic efficiency and energy density of a sodium-ion battery according to claim 1, characterized in that, The specific operation for the second mixing is as follows: stir for 5 to 10 minutes at a revolution speed of 10 to 25 rpm and a rotation speed of 400 to 1000 rpm.
4. The method for preparing a positive electrode slurry to improve the initial coulombic efficiency and energy density of a sodium-ion battery according to claim 1, characterized in that, The specific operation for the third mixing is as follows: stir for 30 to 120 minutes at a revolution speed of 15 to 30 rpm and a rotation speed of 1200 to 2000 rpm.
5. A positive electrode slurry, characterized in that, It is prepared by the method described in any one of claims 1 to 4.
6. A positive electrode sheet, characterized in that, It includes a positive current collector and a positive active material layer disposed on at least one surface of the positive current collector, wherein the positive active material layer includes the positive slurry as described in claim 5.
7. A sodium-ion secondary battery, characterized in that, Including the positive electrode sheet as described in claim 6.
Citation Information
Patent Citations
Manufacturing method of high-specific-energy positive pole piece
CN109428056A
Positive electrode sheet and preparation method thereof, and lithium ion battery containing positive electrode sheet and preparation method thereof
CN111599984A
Sodium-ion battery positive plate, preparation method thereof and sodium-ion battery
CN112768699A
Positive electrode material for sodium ion battery and sodium ion battery comprising positive electrode material
CN113130896A
Positive electrode slurry, preparation method thereof and positive electrode plate