A duplex stainless steel and method of additive manufacturing thereof

By using laser selective melting 3D printing technology and special raw material ratios, and adjusting process parameters, high-efficiency and dense duplex stainless steel can be directly prepared, solving the problems of high energy consumption and long cycle in existing technologies, and achieving simplified production process and high-efficiency preparation.

CN116652170BActive Publication Date: 2026-11-20TAIYUAN UNIVERSITY OF TECHNOLOGY
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310837803.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-10
Publication Date
2026-11-20
Estimated Expiration
2043-07-10

AI Technical Summary

Technical Problem

Existing duplex stainless steel production processes are energy-intensive and have long production cycles, requiring repeated heat treatment and/or plastic deformation treatments to obtain the desired microstructure.

Method used

Using duplex stainless steel powder with a special raw material ratio, and through selective laser melting 3D printing technology, the additive manufacturing process parameters are adjusted to print layer by layer austenitic and ferritic duplex stainless steel with a suitable ratio.

Benefits of technology

It simplifies the preparation process of duplex stainless steel, improves production efficiency, reduces energy consumption, and directly obtains dense metal parts without the need for complex subsequent heat treatment and plastic deformation processing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116652170B_ABST
    Figure CN116652170B_ABST
Patent Text Reader

Abstract

The application belongs to the technical field of metal material manufacturing, and particularly relates to a duplex stainless steel and an additive manufacturing method thereof. The additive manufacturing method of the duplex stainless steel comprises the following steps: S1, preparation of duplex stainless steel metal powder: 430 ferrite stainless steel and 316L austenite stainless steel metal powder are uniformly mixed by using a ball mill, and the duplex stainless steel mixed powder is obtained by ball milling and powder mixing, S2, pretreatment of the duplex stainless steel mixed powder before printing; S3, additive manufacturing of the duplex stainless steel mixed powder, the dry duplex stainless steel mixed powder of S2 is used as raw material, and the duplex stainless steel is prepared by using laser selective melting 3D printing, the scanning power is 210W+ / -10W, and the scanning speed is 800-1200mm / s. The duplex stainless steel containing ferrite and austenite is prepared by adjusting the scanning speed of additive manufacturing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of metal material manufacturing technology, specifically relating to a duplex stainless steel and its additive manufacturing method. Background Technology

[0002] Duplex stainless steel refers to steel whose microstructure at room temperature contains both ferrite and austenitic phases, with both phases present in relatively high volume fractions, typically between 30% and 70%. Due to its unique microstructure, duplex stainless steel combines the advantages of both austenitic and ferritic stainless steels. It possesses the excellent toughness and weldability of austenitic stainless steel, as well as the high strength and chlorine resistance of ferritic stainless steel, resulting in excellent corrosion resistance, high strength, and ease of processing and manufacturing. Therefore, duplex stainless steel is widely used in many fields, including marine oil and gas, shipbuilding, chemical industry, and military industry.

[0003] The development and application of duplex stainless steel began in the 1930s. The earliest research report on duplex stainless steel dates back to 1927, when E.C. Bain and W.Griffiths first studied the ferrite and austenitic duplex structure of the steel. Subsequently, through the tireless efforts of generations of researchers, the smelting process for duplex stainless steel has continuously matured. By the 1980s, a third generation of duplex stainless steel with a higher degree of alloying had been developed to adapt to more demanding service environments; this is known as super duplex stainless steel. The elemental content (mass percentage) of this type of steel is approximately: Cr: 25%, Ni: 6%–7%, Mo: 3%–4%, N: 0.2%–0.3%, Cu: 0.1%–2%, W: 0.1%–2%. Almost simultaneously with super duplex stainless steel, cost-saving duplex stainless steel was also developed. Although cost-saving duplex stainless steel reduces the content of alloying elements (especially Mo), it still possesses mechanical properties and corrosion resistance comparable to 304L and 316L.

[0004] To obtain duplex stainless steel with a suitable microstructure, it is essential to correctly control the alloy's chemical composition and rationally design its heat treatment process. Currently, the conventional preparation process involves solution treatment followed by cold deformation, and then superplastic forming. Existing duplex stainless steel production requires repeated heat treatment and / or plastic deformation to achieve the desired microstructure. This production method is not only energy-intensive but also has a long production cycle, impacting the production efficiency of duplex stainless steel. Therefore, a simple and effective preparation process for duplex stainless steel is of practical significance for improving its applications. Summary of the Invention

[0005] The purpose of this invention is to provide an additive manufacturing method for duplex stainless steel. This method achieves additive manufacturing of duplex stainless steel by using a special raw material ratio, and can obtain austenitic and ferritic duplex stainless steel with appropriate proportions by adjusting the additive manufacturing process parameters and printing layer by layer.

[0006] The technical solution adopted by this invention to solve its technical problem is:

[0007] An additive manufacturing method for duplex stainless steel, the method comprising the following steps:

[0008] S1. Preparation of duplex stainless steel metal powder:

[0009] A ball mill was used to uniformly mix 430 ferritic stainless steel and 316L austenitic stainless steel powders. The resulting duplex stainless steel powder was obtained by ball milling. The mass ratio of 430 ferritic stainless steel to 316L austenitic stainless steel powders was 1:1.49 to 1.51.

[0010] S2, Pre-treatment of duplex stainless steel mixed powder for printing:

[0011] The duplex stainless steel mixed powder obtained in S1 was placed in a forced-air drying oven and dried at 80±5℃ for 4-6 hours for later use to remove moisture from the powder.

[0012] S3, additive manufacturing of duplex stainless steel mixed powder

[0013] The duplex stainless steel was prepared by laser selective melting 3D printing using S2 dry duplex stainless steel mixed powder as raw material. The scanning power was 210W±10W and the scanning rate was 800~1200mm / s.

[0014] Preferably, in the duplex stainless steel mixed powder, the chemical composition of the 430 ferritic stainless steel powder includes the following elements by mass fraction: Cr 16.85%, Mn 0.97%, Si 0.66%, with the balance being Fe and unavoidable impurities. The 430 ferritic stainless steel powder is in the form of regular spheres, and the powder particle size distribution is in the range of 15 to 53 μm.

[0015] Preferably, in the duplex stainless steel mixed powder, the chemical composition of the 316L austenitic stainless steel powder includes the following elements by mass fraction: Cr: 17.94%, Ni: 12.01%, Mo: 2.15%, Si: 0.39%, Mn: 0.006%, with the balance being Fe and unavoidable impurities. The 316L austenitic stainless steel powder is in the form of regular spheres, and the powder particle size distribution is in the range of 15 to 53 μm.

[0016] As a preferred option, the process parameters for laser selective melting are: a checkerboard scanning strategy, a scanning interval of 0.1 mm, a powder thickness of 30 μm, a rotation angle between layers of 67°, and a laser beam diameter of 100 μm.

[0017] Preferably, during the additive manufacturing process of the duplex stainless steel, the preheating temperature of the substrate in the laser selective melting equipment is 80±5℃, the protective atmosphere is argon, and the oxygen content is not higher than 0.8 Vol.%.

[0018] Preferably, the scanning rate of laser selective melting is 900-1200 mm / s, and the volume fraction of austenite in duplex stainless steel is above 30%.

[0019] Preferably, the scanning rate of laser selective melting is 900, 1000, or 1200 mm / s.

[0020] As a preferred option, the scanning rate of laser selective melting is 1000 mm / s ± 50 mm / s, and the ratio of the two phases in duplex stainless steel is close to 1:1, which is the optimal phase ratio.

[0021] A duplex stainless steel, which is manufactured by the additive manufacturing method of duplex stainless steel described in this invention.

[0022] Preferably, the elemental content of the duplex stainless steel, calculated as 100% by mass, is approximately: Cr 16.9–17.5%, Ni 6.9–7.21%, Mo 0.98–1.29%, Mn 0.25–0.39%, Si 0.3–0.498%, with the balance being Fe and unavoidable impurities.

[0023] The beneficial effects of this invention are:

[0024] 1. This invention prepares duplex stainless steel containing ferrite and austenite by adjusting the scanning rate of additive manufacturing, and the austenite phase, which has a relatively small content, has a volume fraction of more than 30%, and the prepared metal parts have high density and few defects.

[0025] 2. The additive manufacturing method for duplex stainless steel provided by this invention uses selective laser melting to prepare dense metal parts directly. This process is simple, requiring only adjustment of the additive manufacturing process parameters to print layer by layer to obtain a suitable ratio of austenitic and ferritic duplex stainless steel. It does not require repeated heat treatment and / or plastic deformation processing, consumes less energy, and takes less time, which is beneficial to improving production efficiency. Attached Figure Description

[0026] Figure 1 This is an EBSD phase distribution diagram of austenite and ferrite in Example 1 of the present invention;

[0027] Figure 2 This is an EBSD phase distribution diagram of austenite and ferrite in Embodiment 2 of the present invention;

[0028] Figure 3 This is an EBSD phase distribution diagram of austenite and ferrite in Example 3 of the present invention;

[0029] Figure 4 This is an EBSD phase distribution diagram of austenite and ferrite in Example 4 of the present invention;

[0030] Figure 5 This is an EBSD phase distribution diagram of austenite and ferrite in Example 5 of the present invention;

[0031] Figure 6 This is an EBSD phase distribution diagram of austenite and ferrite in Comparative Example 1 of the present invention;

[0032] Figure 7 This is an EBSD phase distribution diagram of austenite and ferrite in Comparative Example 2 of the present invention;

[0033] Figure 8 This is a diagram showing the EBSD phase distribution of austenite and ferrite in Comparative Example 3 of the present invention. Detailed Implementation

[0034] It should be noted that the following detailed descriptions are illustrative and intended to provide further explanation of this application. Unless otherwise specified, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application pertains.

[0035] It should be noted that the terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the exemplary embodiments according to this application. As used herein, the singular form is intended to include the plural form as well, unless the context clearly indicates otherwise. Furthermore, it should be understood that when the terms "comprising" and / or "including" are used in this specification, they indicate the presence of features, steps, operations, devices, components, and / or combinations thereof.

[0036] The present invention will now be further illustrated with specific examples. The following embodiments are only for explaining the present invention and do not constitute a limitation thereof. The test samples and test procedures used in the following embodiments include the following (if the specific experimental conditions are not specified in the embodiments, they are usually performed according to conventional conditions or the conditions recommended by the reagent company; the reagents, consumables, etc. used in the following embodiments can be obtained commercially unless otherwise specified).

[0037] Example

[0038] An additive manufacturing method for duplex stainless steel, wherein the specific steps of the additive manufacturing method for duplex stainless steel are as follows:

[0039] (1) Preparation of duplex stainless steel metal powder:

[0040] 430 (ferritic steel) and 316L (austenitic steel) stainless steel powders were uniformly mixed using a ball mill to obtain a mixed powder of duplex stainless steel (fully mixed for more than 4 hours). The mass ratio of 430 to 316L stainless steel powders was 1:1.49 to 1:1.51.

[0041] In the duplex stainless steel mixed powder, the chemical composition of the 430 ferritic stainless steel powder is: Cr: 16.85%, Mn: 0.97%, Si: 0.66%, with the balance being Fe and unavoidable impurities. The 430 ferritic stainless steel powder is in the form of regular spheres, and the powder particle size distribution is in the range of 15 to 53 μm.

[0042] In the duplex stainless steel mixed powder, the chemical composition of the 316L austenitic stainless steel powder is: Cr: 17.94%, Ni: 12.01%, Mo: 2.15%, Si: 0.39%, Mn: 0.006%, with the balance being Fe and unavoidable impurities. The 316L austenitic stainless steel powder is in the form of regular spheres, and the powder particle size distribution is in the range of 15 to 53 μm.

[0043] The elemental content of the duplex stainless steel, calculated as 100% by mass, is approximately: Cr: 17.5%, Ni: 7.21%, Mo: 1.29%, Mn: 0.391%, Si: 0.498%, with the balance being Fe and unavoidable impurities.

[0044] (2) Pre-treatment of duplex stainless steel mixed powder for printing:

[0045] The prepared duplex stainless steel mixed powder was placed in a forced-air drying oven and dried at 80°C for 4 hours for later use.

[0046] (3) Additive manufacturing of duplex stainless steel mixed powder

[0047] The duplex stainless steel was prepared by selective laser melting 3D printing. The additive manufacturing process parameters were as follows: the scanning strategy was a checkerboard pattern, the scanning power was 210W, the scanning rate was 800-1200mm / s, the scanning spacing was 0.1mm, the powder thickness was 30μm, the rotation angle between layers was 67°, and the laser beam diameter was 100μm.

[0048] During the additive manufacturing process of the duplex stainless steel, the substrate is preheated to 80°C, the protective atmosphere is argon, and the oxygen content cannot exceed 0.8 vol.%.

[0049] Comparative Example 1

[0050] 430 (ferritic steel) and 316L (austenitic steel) stainless steel powders were uniformly mixed using a ball mill to obtain a mixed powder of duplex stainless steel (fully mixed for more than 4 hours). The mass ratio of 430 to 316L stainless steel powders was 1:0.99 to 1:1.1.

[0051] The material was prepared using selective laser melting (SLM) additive manufacturing. The scanning strategy of SLM additive manufacturing was a checkerboard pattern. The laser power of SLM additive manufacturing was 210W. The scanning speed of SLM additive manufacturing was 1000mm / s. The scanning interval of SLM additive manufacturing was 0.1mm. The powder thickness of SLM additive manufacturing was 30μm.

[0052] In this comparative example, the microstructure of the duplex stainless steel consists of ferrite and austenite, with an austenite volume fraction of 2.3%.

[0053] Alloy powders for laser selective melting additive manufacturing were prepared by mixing 430 and 316L stainless steel metal powders in mass ratios of 1:1, 1:1.5, 1:2, and 1:4, respectively.

[0054] Comparative Example 2

[0055] 430 (ferritic steel) and 316L (austenitic steel) stainless steel powders were uniformly mixed using a ball mill to obtain a mixed powder of duplex stainless steel (mixed thoroughly for more than 4 hours). The mass ratio of 430 to 316L stainless steel powders was 1:1.98 to 1:2.11.

[0056] The material was prepared using selective laser melting (SLM) additive manufacturing. The scanning strategy of SLM additive manufacturing was a checkerboard pattern. The laser power of SLM additive manufacturing was 210W. The scanning speed of SLM additive manufacturing was 1000mm / s. The scanning interval of SLM additive manufacturing was 0.1mm. The powder thickness of SLM additive manufacturing was 30μm.

[0057] In this comparative example, the microstructure of the duplex stainless steel consists of ferrite and austenite, with an austenite volume fraction of 80.1%.

[0058] Comparative Example 3

[0059] 430 (ferritic steel) and 316L (austenitic steel) stainless steel powders were uniformly mixed using a ball mill to obtain a mixed powder of duplex stainless steel (mixed thoroughly for more than 4 hours). The mass ratio of 430 to 316L stainless steel powders was 1:3.99 to 1:4.1.

[0060] The material was prepared using selective laser melting (SLM) additive manufacturing. The scanning strategy of SLM additive manufacturing was a checkerboard pattern. The laser power of SLM additive manufacturing was 210W. The scanning speed of SLM additive manufacturing was 1000mm / s. The scanning interval of SLM additive manufacturing was 0.1mm. The powder thickness of SLM additive manufacturing was 30μm.

[0061] In this comparative example, the microstructure of the duplex stainless steel consists of ferrite and austenite, with an austenite volume fraction of 99.2%.

[0062] Table 2 shows the mass ratio of 430 to 316L stainless steel powders and the additive manufacturing process parameters, as well as the volume fractions of austenite and ferrite in the alloys in Comparative Examples 1-3. Some EBSDs are shown in Table 2. Figures 6 to 8 As shown.

[0063] Example 1

[0064] The specific method is the same as in the aforementioned embodiments. In this embodiment, the additive manufacturing is selective laser melting (SLM). The scanning strategy of SLM is a checkerboard pattern, the laser power is 210W, the scanning speed is 900mm / s, the scanning interval is 0.1mm, and the powder thickness is 30μm.

[0065] In this embodiment, the microstructure of the duplex stainless steel consists of ferrite and austenite, with the volume fraction of austenite being 34.5%.

[0066] Example 2

[0067] The specific method is the same as in the aforementioned embodiments. In this embodiment, the additive manufacturing is selective laser melting (SLM). The scanning strategy of SLM is a checkerboard pattern, the laser power is 210W, the scanning speed is 1200mm / s, the scanning interval is 0.1mm, and the powder thickness is 30μm.

[0068] In this embodiment, the microstructure of the duplex stainless steel consists of ferrite and austenite, with the volume fraction of austenite being 38.6%.

[0069] Example 3

[0070] The specific method is the same as in the aforementioned embodiments. In this embodiment, the additive manufacturing is selective laser melting (SLM). The scanning strategy of SLM is a checkerboard pattern, the laser power is 210W, the scanning speed is 1000mm / s, the scanning interval is 0.1mm, and the powder thickness is 30μm.

[0071] In this embodiment, the microstructure of the duplex stainless steel consists of ferrite and austenite, with the volume fraction of austenite being 48.8%.

[0072] Examples 4-5

[0073] The specific method is the same as the aforementioned embodiments, but the laser selective melting additive manufacturing parameters differ from those in Embodiment 1. The specific parameters are shown in Table 1.

[0074] The additive manufacturing process parameters and the volume fractions of austenite and ferrite in the alloys of Examples 1-5 are shown in Table 1. Some EBSDs are shown below. Figures 1 to 5 As shown.

[0075] Table 1

[0076]

[0077] Table 2 shows the additive manufacturing process parameters and the volume fractions of austenite and ferrite in the alloys of Comparative Examples 1 to 3.

[0078] Table 2

[0079]

[0080] Conclusion: This invention utilizes a laser selective melting additive manufacturing method to prepare duplex stainless steel. The raw material is a mixed powder of 430 and 316L. The laser power in the laser selective melting additive manufacturing process is 210W, the scanning interval is 0.1mm, and the powder layer thickness is 30μm. The phase ratio of ferrite to austenite is controlled by changing the scanning rate of the laser selective melting additive manufacturing process. The scanning rates are 800, 900, 1000, 1100, and 1200 mm / s. Figures 1-5 As shown in Table 1, when the scanning rate is 900, 1000, or 1200 mm / s, the volume fraction of austenite is above 30%. When the scanning rate is 1000 mm / s, the ratio of the two phases is close to 1:1, which is the optimal phase ratio.

[0081] According to the data from Comparative Examples 1-3 in Table 2, this invention uses a laser selective melting additive manufacturing method to prepare duplex stainless steel. The raw material is a mixture of 430 and 316L stainless steel powders. Duplex stainless steel powders with different mass ratios are obtained through ball milling. Figures 6-8 As shown in Table 2, when the mass ratio of 430 to 316L stainless steel powder is 1:1.5, duplex stainless steel with an austenite to ferrite ratio close to 1:1 can be directly obtained by selective laser melting additive manufacturing method without the need for complex subsequent heat treatment, which simplifies the preparation process of duplex stainless steel. Moreover, the powder preparation processes of 430 and 316L stainless steel are mature and can be purchased directly without the need for special powder preparation.

[0082] The various embodiments in this specification are described in a progressive manner, with each embodiment focusing on its differences from other embodiments. Similar or identical parts between embodiments can be referred to interchangeably. For the apparatus disclosed in the embodiments, since it corresponds to the method disclosed in the embodiments, the description is relatively simple; relevant parts can be referred to in the method section.

[0083] The present invention provides a detailed description of a duplex stainless steel and its additive manufacturing method. Specific examples have been used to illustrate the principles and implementation methods of the invention. These examples are merely illustrative to help understand the method and core concepts of the invention. It should be noted that those skilled in the art can make various improvements and modifications to the invention without departing from its principles, and these improvements and modifications also fall within the scope of protection of the claims.

Claims

1. A method for additive manufacturing of duplex stainless steel, characterized in that... The method includes the following steps: S1. Preparation of duplex stainless steel metal powder: A ball mill was used to uniformly mix 430 ferritic stainless steel and 316L austenitic stainless steel powders. The resulting duplex stainless steel powder was obtained by ball milling. The mass ratio of 430 ferritic stainless steel to 316L austenitic stainless steel powders was 1:1.49 ~ 1.

51. S2, Pre-treatment of duplex stainless steel mixed powder for printing: The duplex stainless steel mixed powder obtained in S1 was placed in a forced-air drying oven and dried at 80 ± 5℃ for 4 ~ 6 h to remove moisture from the powder. S3, additive manufacturing of duplex stainless steel mixed powder The duplex stainless steel was prepared by laser selective melting 3D printing using S2 dry duplex stainless steel mixed powder as raw material. The scanning power was 210 W ± 10 W and the scanning rate was 1000 mm / s ± 50 mm / s. The process parameters for laser selective melting are: a checkerboard scanning strategy, a scanning interval of 0.1 mm, a powder thickness of 30 μm, a rotation angle between layers of 67°, and a laser beam diameter of 100 μm. In the additive manufacturing process of the duplex stainless steel, the preheating temperature of the substrate in the laser selective melting equipment is 80±5℃, the protective atmosphere is argon, and the oxygen content is not higher than 0.8 Vol.%. The volume fraction of austenite in the duplex stainless steel is above 30%.

2. The additive manufacturing method for duplex stainless steel according to claim 1, characterized in that: In the duplex stainless steel mixed powder, the chemical composition of the 430 ferritic stainless steel powder includes the following elements by mass fraction: Cr 16.85%, Mn 0.97%, Si 0.66%, with the balance being Fe and unavoidable impurities. The 430 ferritic stainless steel powder is in the form of regular spheres, and the powder particle size distribution is in the range of 15 to 53 μm.

3. The additive manufacturing method for duplex stainless steel according to claim 1, characterized in that: In the duplex stainless steel mixed powder, the chemical composition of the 316L austenitic stainless steel powder includes the following elements by mass fraction: Cr: 17.94%, Ni: 12.01%, Mo: 2.15%, Si: 0.39%, Mn: 0.006%, with the balance being Fe and unavoidable impurities. The 316L austenitic stainless steel powder is in the form of regular spheres, and the powder particle size distribution is in the range of 15 ~ 53 μm.

4. The additive manufacturing method for duplex stainless steel according to claim 1, characterized in that: The scanning rates for laser selective melting are 900, 1000, and 1200 mm / s.

5. A duplex stainless steel, which is manufactured by the additive manufacturing method of the duplex stainless steel according to claim 1.

6. The duplex stainless steel according to claim 5, characterized in that: Based on a mass percentage of 100%, the elemental content of the duplex stainless steel is approximately: Cr 16.9 ~ 17.5%, Ni 6.9 ~ 7.21%, Mo 0.98 ~ 1.29%, Mn 0.25 ~ 0.39%, Si 0.3 ~ 0.498%, with the balance being Fe and unavoidable impurities.

Citation Information

Patent Citations

  • Method for improving plasticity of 3D printing duplex stainless steel

    CN116197412A

  • High-strength gradient stainless steel and additive manufacturing method thereof

    CN118577809A