A negative temperature coefficient thermistor ceramic material and preparation method thereof

Through the solid-phase sintering method of materials composed of 0.69(Bi1-xMgx)FeO3-0.31BaTiO3, the problem of insufficient use of traditional thermistor materials in high-temperature environments has been solved, and a wide-temperature range high-temperature thermometer with good compactness and thermal-sensitive properties has been prepared. Thermistor material, suitable for applications in the range of 0 to 700°C.

CN116655367BActive Publication Date: 2024-10-18SOUTH CHINA UNIV OF TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310361976.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-07
Publication Date
2024-10-18
Estimated Expiration
2043-04-07

Smart Images

  • Figure CN116655367B_ABST
    Figure CN116655367B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of electronic ceramic materials, and specifically relates to a negative temperature coefficient thermistor ceramic material and a preparation method thereof. The composition of the ceramic material includes 0.69 (Bi 1‑x Mg x )FeO3‑0.31BaTiO3, wherein x=0.1% to 5.0%. The formula raw materials of the ceramic material include oxides, inorganic salts or organic salts containing the following elements: Bi, Fe, Ba, Ti, Mg metal elements; for example, including Bi2O3, Fe2O3, BaCO3, TiO2 and MgO powders. The wide temperature range high temperature thermistor material of the present invention has good compactness and excellent thermal sensitivity, and has obvious negative temperature coefficient characteristics in the range of 0 to 700°C, and is suitable for preparing wide temperature range high temperature thermistors.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of semiconductor thermistors, in particular to a negative temperature coefficient thermistor ceramic material and a preparation method thereof. Background Art

[0002] Sensitive components and sensors are one of the pillars of the electronic information industry, with broad development prospects and a pivotal role in the development of the electronics industry. Negative Temperature Coefficient (NTC) thermistor is a resistor whose resistance decreases as the temperature increases. It has the advantages of simple structure, small size, high sensitivity and low cost. It is widely used in temperature measurement and control, overcurrent protection of electronic products and temperature compensation. It has become one of the indispensable electronic components in many household and industrial fields such as medical appliances, automotive industry, household appliances and even aerospace. However, traditional spinel thermistor ceramics composed of transition metal oxides can usually only be used below 300°C and cannot meet the use in high temperature environments. This poses new challenges to the development of new high-temperature NTC thermistor ceramic materials.

[0003] High-temperature NTC thermistors refer to NTC thermistors that can be used in situations above 300°C. In current research, two methods are generally used to achieve use in high-temperature environments: one is to mix NTC thermistors with high-resistance ceramics to improve the high-temperature stability of the material; the other is to modify the perovskite thermistors with high-temperature stability, usually by replacing the A and B elements in the perovskite structure through doping, changing its electrical properties, so that it can be stably used in high-temperature areas and has suitable NTC performance. Bismuth ferrite-barium titanate ceramic material belongs to perovskite ceramics, which has the characteristics of good high-temperature stability and is widely studied in the field of high-temperature electronic ceramics. At present, there are few reports on the preparation of NTC thermistors based on bismuth ferrite-barium titanate ceramics, so its potential as an NTC thermistor remains to be studied. Summary of the invention

[0004] In order to solve the problems existing in the prior art, the present invention provides a high-temperature NTC thermistor ceramic material and a preparation method thereof, wherein the prepared 0.69 (B i1-x Mg x )FeO3-0.31BaTiO3 wide temperature range high temperature thermistor material has good compactness and excellent thermal sensitivity. It has obvious negative temperature coefficient characteristics in the range of 0 to 700°C and is suitable for the preparation of wide temperature range high temperature thermistors.

[0005] The negative temperature coefficient thermistor ceramic material of the present invention comprises 0.69 (Bi 1-x Mg x)FeO3-0.31BaTiO3, where x=0.1%~5.0%.

[0006] Preferably, the value of x is: x=0.5%, or x=1.0%, or x=1.5%, or x=2.0%.

[0007] Preferably, the raw materials of the ceramic material include oxides, inorganic salts or organic salts containing the following elements: Bi, Fe, Ba, Ti, Mg metal elements.

[0008] Further preferably, the formula raw materials of the ceramic material include Bi2O3, Fe2O3, BaCO3, TiO2 and MgO powder.

[0009] The method for preparing the negative temperature coefficient thermistor ceramic material of the present invention comprises the following steps:

[0010] Step (1), weigh the raw materials according to the formula;

[0011] Step (2), mixing the formula raw materials weighed in step (1), using deionized water as a mixing medium, mixing and grinding the raw materials for several hours, and drying;

[0012] Step (3), pre-calcining the powder obtained after drying in step (2) to obtain powder;

[0013] Step (4), grinding the powder obtained by pre-calcining in step (3), grinding again with deionized water as the medium for several hours and drying;

[0014] Step (5), granulating the powder obtained after drying in step (4);

[0015] Step (6), sieving the powder granulated in step (5);

[0016] Step (7), placing the powder screened in step (6) into a mold, applying high pressure, and pressing into shape;

[0017] Step (8), placing the green body pressed out in step (7) into a high temperature furnace for debinding;

[0018] Step (9), placing the green body after debinding in step (8) in a crucible, and then sintering and cooling.

[0019] Compared with the prior art, the technical effects achieved by the present invention include:

[0020] 1. The present invention uses Bi2O3, Fe2O3, BaCO3, TiO2, and MgO powders as raw materials, and obtains bismuth ferrite-barium titanate-based high-temperature NTC thermistor ceramic materials by solid phase sintering, that is, 0.69 (B i1-x Mg x)FeO3-0.31BaTiO3 ceramic material has good compactness and excellent thermal sensitivity. At a sintering temperature of 1020℃, the resistivity is ρ at 100℃. 100 2.2×10 6 Ω·cm~4.7×10 4 Ω·cm, thermal constant B from 100℃ to 600℃ 100 / 600 The value is 4430K~6421K; it has obvious negative temperature coefficient characteristics in the range of 0~700℃, and is suitable for the preparation of high-temperature thermistors with a wide temperature range.

[0021] The present invention can prepare 0.69 (B i1- x Mg x )FeO3-0.31BaTiO3 wide temperature range high temperature thermistor material.

[0022] 2. The thermosensitive ceramic material of the present invention has simple composition and preparation process, and by adjusting the element content, the resistance value of the thermistor element can be adjusted in a wide range, and a relatively high thermal constant B of the material can be maintained.

[0023] 3. The composition formula of the thermistor material of the present invention can adjust the production process according to the needs in the actual application process, and has a certain flexibility. For example, the raw materials can be selected from oxides, inorganic salts or organic salts containing key elements. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 X-ray diffraction patterns of high temperature NTC ceramics prepared in Examples 1, 2, 3, and 4 of the present invention.

[0025] Figure 2 This is a surface SEM image of the high-temperature NTC thermistor ceramic prepared in Example 2 of the present invention.

[0026] Figure 3 The resistance-temperature characteristic diagram of the high-temperature NTC ceramics obtained in Examples 1, 2, 3, and 4 of the present invention is shown to indicate that the examples have typical NTC characteristics. DETAILED DESCRIPTION

[0027] The present invention provides a NTC thermistor ceramic material suitable for high temperature and a preparation method thereof. The present invention is further described below in conjunction with the accompanying drawings and embodiments, but the embodiments of the present invention are not limited thereto.

[0028] The present invention is a NTC thermistor ceramic material suitable for high temperature. The composition of the NTC thermistor includes 0.69 (B i1-x Mg x)FeO3-0.31BaTiO3, wherein x=0.1%~5.0%; that is, the formula contains Bi, Fe, Ba, Ti, Mg elements, and the raw materials can be oxides, inorganic salts or organic salts containing these elements.

[0029] The solid phase sintering process adopted by the present invention comprises the following steps:

[0030] Step (1), according to the formula calculation, weigh the formula raw materials, such as Bi2O3, Fe2O3, BaCO3, TiO2, MgO powder;

[0031] Step (2), mixing the raw materials weighed in step (1), using deionized water as a mixing medium, using a planetary ball mill to mix the raw materials for 12 hours, and drying;

[0032] Step (3), the powder obtained after drying in step (2) is placed in a corundum crucible, placed in a muffle furnace and pre-sintered at 800° C. to obtain a powder, and kept warm for 4 hours;

[0033] Step (4), grinding the powder obtained by pre-calcining in step (3), again using deionized water as a medium, ball milling in a planetary ball mill for 12 hours, and drying;

[0034] Step (5), granulating the powder obtained after drying in step (4); using polyvinyl alcohol (PVA) as a binder during granulation, and the amount of the binder added is 10% of the mass of the powder;

[0035] Step (6), sieving the powder after granulation in step (5), using a 100-mesh sieve;

[0036] Step (7), placing the powder screened in step (6) into a special mold, applying a high pressure of 5 MPa, and pressing into shape;

[0037] Step (8), placing the green body pressed out in step (7) into a high-temperature electric furnace for debinding at a temperature of 600° C. for 2 hours;

[0038] Step (9), placing the green body after debinding in step (8) in a crucible, and placing it in a muffle furnace for sintering; the heating rate is 3°C / min, the sintering temperature is 1020°C, and the temperature is kept for 3 hours, and the green body is cooled with the furnace after sintering;

[0039] Step (10), using 1000 mesh sandpaper for polishing, the ceramic surface obtained by sintering step (9) is polished and cleaned using ultrasound, and then electrodes are printed on both sides of the material using screen printing.

[0040] The technical solution of the present invention is further described in detail below with several embodiments taking different values ​​of x.

[0041] Example 1

[0042] In this embodiment, bismuth ferrite-barium titanate NTC thermistor ceramic resistor material with x=0.5% is prepared.

[0043] Select Bi2O3, Fe2O3, BaCO3, TiO2, MgO powders with purity higher than 99% as the raw materials of the formula, according to the chemical formula 0.69 (B i0.995 Mg 0.005 )The raw materials are weighed in the stoichiometric ratio of FeO3-0.31BaTiO3. Deionized water is used as the ball milling medium, zirconium oxide balls are used as grinding balls, and the ball milling jar is made of polytetrafluoroethylene. The raw materials, grinding balls, and deionized water are placed in a planetary ball mill in a mass ratio of 1:1:1, and the mixture is ball milled for 12 hours. After the material is discharged, it is placed in an oven and dried at 110°C. The dried powder is pre-fired at a heating rate of 3°C / min from room temperature to 800°C and kept warm for 4 hours. After the pre-fired intermediate is ground, it is ball milled for a second time for 12 hours with deionized water as the ball milling medium, dried, and a polyvinyl alcohol aqueous solution with a mass concentration of 10% is added as a binder for granulation, and passed through a 100 mesh sieve. Under a pressure of 5MPa, it is pressed into a disc with a diameter of 12mm and a thickness of 1.0mm in a mold. Subsequently, the ceramic sheet is heated from room temperature to 600°C for 5h in a sintering furnace, and kept warm for 2h for debinding to remove PVA. The ceramic green sheet after debinding is heated to 1020°C at a heating rate of 3°C / min for sintering, kept warm for 3 hours, and naturally cooled to room temperature with the furnace. The surface of the sintered ceramic sheet is polished flat with 1000-mesh sandpaper, and silver is coated on both sides of the ceramic sheet using a screen printing process. The silver is sintered at 800°C and kept warm for 20 minutes to form an electrode. Finally, the electrical performance is tested. After testing, the embodiment has a perovskite structure, no impurities are generated, the ceramic is dense, and there are no pores. In terms of electrical properties, the resistivity is ρ at 100°C. 100 2.2×10 6 Ω·cm, thermal constant B from 100℃ to 600℃ 100 / 600 It is 6421K.

[0044] Example 2

[0045] In this embodiment, bismuth ferrite-barium titanate NTC thermistor ceramic resistor material with x=1.0% is prepared.

[0046] Select Bi2O3, Fe2O3, BaCO3, TiO2, MgO powders with purity higher than 99% as the raw materials of the formula, according to the chemical formula 0.69 (B i0.99 Mg 0.01)The raw materials are weighed in the stoichiometric ratio of FeO3-0.31BaTiO3. Deionized water is used as the ball milling medium, zirconium oxide balls are used as grinding balls, and the ball milling jar is made of polytetrafluoroethylene. The raw materials, grinding balls, and deionized water are placed in a planetary ball mill in a mass ratio of 1:1:1, and the mixture is ball milled for 12 hours. After the material is discharged, it is placed in an oven and dried at 110°C. The dried powder is pre-fired at a heating rate of 3°C / min from room temperature to 800°C and kept warm for 4 hours. After the pre-fired intermediate is ground, it is ball milled for a second time for 12 hours with deionized water as the ball milling medium, dried, and a polyvinyl alcohol aqueous solution with a mass concentration of 10% is added as a binder for granulation, and passed through a 100 mesh sieve. Under a pressure of 5MPa, it is pressed into a disc with a diameter of 12mm and a thickness of 1.0mm in a mold. Subsequently, the ceramic sheet is heated from room temperature to 600°C for 5h in a sintering furnace, and kept warm for 2h for debinding to remove PVA. The ceramic green sheet after debinding is heated to 1020°C at a heating rate of 3°C / min for sintering, kept warm for 3 hours, and naturally cooled to room temperature with the furnace. The surface of the sintered ceramic sheet is polished flat with 1000-mesh sandpaper, and silver is coated on both sides of the ceramic sheet using a screen printing process. The silver is sintered at 800°C and kept warm for 20 minutes to form an electrode. Finally, the electrical performance is tested. After testing, the embodiment has a perovskite structure, no impurities are generated, the ceramic is dense, and there are no pores. In terms of electrical properties, the resistivity is ρ at 100°C. 100 4.0×10 5 Ω·cm, thermal constant B from 100℃ to 600℃ 100 / 600 It is 5502K.

[0047] Example 3

[0048] In this embodiment, bismuth ferrite-barium titanate NTC thermistor ceramic resistor material with x=1.5% is prepared.

[0049] Select Bi2O3, Fe2O3, BaCO3, TiO2, MgO powders with purity higher than 99% as the raw materials of the formula, according to the chemical formula 0.69 (B i0.985 Mg 0.015)The raw materials are weighed in the stoichiometric ratio of FeO3-0.31BaTiO3. Deionized water is used as the ball milling medium, zirconium oxide balls are used as grinding balls, and the ball milling jar is made of polytetrafluoroethylene. The raw materials, grinding balls, and deionized water are placed in a planetary ball mill in a mass ratio of 1:1:1, and the mixture is ball milled for 12 hours. After the material is discharged, it is placed in an oven and dried at 110°C. The dried powder is pre-fired at a heating rate of 3°C / min from room temperature to 800°C and kept warm for 4 hours. After the pre-fired intermediate is ground, it is ball milled for a second time for 12 hours with deionized water as the ball milling medium, dried, and a polyvinyl alcohol aqueous solution with a mass concentration of 10% is added as a binder for granulation, and passed through a 100 mesh sieve. Under a pressure of 5MPa, it is pressed into a disc with a diameter of 12mm and a thickness of 1.0mm in a mold. Subsequently, the ceramic sheet is heated from room temperature to 600°C for 5h in a sintering furnace, and kept warm for 2h for debinding to remove PVA. The ceramic green sheet after debinding is heated to 1020°C at a heating rate of 3°C / min for sintering, kept warm for 3 hours, and naturally cooled to room temperature with the furnace. The surface of the sintered ceramic sheet is polished flat with 1000-mesh sandpaper, and silver is coated on both sides of the ceramic sheet using a screen printing process. The silver is sintered at 800°C and kept warm for 20 minutes to form an electrode. Finally, the electrical performance is tested. After testing, the embodiment has a perovskite structure, no impurities are generated, the ceramic is dense, and there are no pores. In terms of electrical properties, the resistivity is ρ at 100°C. 100 7.6×10 4 Ω·cm, thermal constant B from 100℃ to 600℃ 100 / 600 It is 4592K.

[0050] Example 4

[0051] In this embodiment, bismuth ferrite-barium titanate NTC thermistor ceramic resistor material with x=2.0% is prepared.

[0052] Select Bi2O3, Fe2O3, BaCO3, TiO2, MgO powders with purity higher than 99% as the raw materials of the formula, according to the chemical formula 0.69 (B i0.985 Mg 0.015)The raw materials are weighed in the stoichiometric ratio of FeO3-0.31BaTiO3. Deionized water is used as the ball milling medium, zirconium oxide balls are used as grinding balls, and the ball milling jar is made of polytetrafluoroethylene. The raw materials, grinding balls, and deionized water are placed in a planetary ball mill in a mass ratio of 1:1:1, and the mixture is ball milled for 12 hours. After the material is discharged, it is placed in an oven and dried at 110°C. The dried powder is pre-fired at a heating rate of 3°C / min from room temperature to 800°C and kept warm for 4 hours. After the pre-fired intermediate is ground, it is ball milled for a second time for 12 hours with deionized water as the ball milling medium, dried, and a polyvinyl alcohol aqueous solution with a mass concentration of 10% is added as a binder for granulation, and passed through a 100 mesh sieve. Under a pressure of 5MPa, it is pressed into a disc with a diameter of 12mm and a thickness of 1.0mm in a mold. Subsequently, the ceramic sheet is heated from room temperature to 600°C for 5h in a sintering furnace, and kept warm for 2h for debinding to remove PVA. The ceramic green sheet after debinding is heated to 1020°C at a heating rate of 3°C / min for sintering, kept warm for 3 hours, and naturally cooled to room temperature with the furnace. The surface of the sintered ceramic sheet is polished flat with 1000-mesh sandpaper, and silver is coated on both sides of the ceramic sheet using a screen printing process. The silver is then fired at 800°C and kept warm for 20 minutes to form an electrode. Finally, the electrical properties are tested. After testing, the embodiment has a perovskite structure, no impurities are generated, the ceramic is dense, and there are no pores. In terms of electrical properties, the resistivity is ρ at 100°C. 100 4.7×10 4 Ω·cm, thermal constant B from 100℃ to 600℃ 100 / 600 It is 4430K.

[0053] The NTC thermistor material suitable for high temperature prepared by the present invention has good NTC thermistor performance on the basis of ensuring basic density. At a sintering temperature of 1020°C, the resistivity ρ at 100°C 100 2.2×10 6 Ω·cm~4.7×10 4 Ω·cm, thermal constant B from 100℃ to 600℃ 100 / 600 The value is 4430K~6421K. It has obvious negative temperature coefficient characteristics in the range of 0~700℃, and is suitable for preparing high-temperature thermistors with a wide temperature range. The X-ray diffraction patterns of the high-temperature NTC ceramics prepared in the above Examples 1-4 are as follows: Figure 1 The surface SEM image of the high temperature NTC thermistor ceramic prepared in Example 2 is as shown in Figure 2 As shown; the resistance-temperature characteristic diagram of high temperature NTC ceramics obtained in Examples 1-4 is as follows Figure 3 As shown, it is shown that the embodiment has typical NTC characteristics.

[0054] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A negative temperature coefficient thermistor ceramic material, characterized in that: The composition of the ceramic material includes 0.69 (Bi 1- x Mg x )FeO3-0.31BaTiO3, where x = 0.1%~5.0%; The ceramic material comprises Bi2O3, Fe2O3, BaCO3, TiO2 and MgO powders. The bismuth ferrite-barium titanate-based high-temperature NTC thermistor ceramic material is obtained by solid phase sintering. The resistivity at 100°C is ρ 100 2.2×10 6 Ω·cm ~ 4.7×10 4 Ω·cm, thermal constant B from 100℃ to 600℃ 100 / 600 The value is 4430K ~ 6421K.

2. The negative temperature coefficient thermistor ceramic material according to claim 1, characterized in that: The value of x is: x = 0.5%, or x = 1.0%, or x = 1.5%, or x = 2.0%.

3. A method for preparing the negative temperature coefficient thermistor ceramic material according to claim 1 or 2, characterized in that: The steps include: Step (1), weigh the raw materials according to the formula; Step (2), mixing the formula raw materials weighed in step (1), using deionized water as the mixing medium, mixing and grinding the raw materials for several hours, and drying; Step (3), pre-calcining the powder obtained after drying in step (2) to obtain powder; Step (4), grinding the powder obtained by pre-calcining in step (3), grinding again with deionized water as the medium for several hours and drying; Step (5), granulating the powder obtained after drying in step (4); Step (6), sieving the powder granulated in step (5); Step (7), placing the powder screened in step (6) into a mold, applying high pressure, and pressing into shape; Step (8), placing the green body pressed in step (7) into a high-temperature furnace for debinding; Step (9), placing the green body after debinding in step (8) in a crucible, and then sintering and cooling.

4. The preparation method according to claim 3, characterized in that: Also includes: Step (10), grinding the ceramic surface obtained by sintering step (9) to make it smooth, and ultrasonically cleaning it, and then printing electrodes on both sides of the material.

Citation Information

Patent Citations

  • Novel NTC thermistor material based on nickel oxide

    CN105967656A