A GaN-based light emitting diode epitaxial wafer and a method of manufacturing the same

By introducing a periodically alternating InAlGaN and MgN layer structure into the epitaxial wafer of a GaN-based light-emitting diode, the hole concentration and mobility are optimized, the problem of imbalance between electron and hole distribution is solved, the luminous efficiency is improved and the operating voltage is reduced.

CN116666511BActive Publication Date: 2026-11-24JIANGXI ZHAO CHI SEMICON CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310796807.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-30
Publication Date
2026-11-24
Estimated Expiration
2043-06-30

AI Technical Summary

Technical Problem

In existing GaN-based light-emitting diode epitaxial wafers, the distribution of electrons and holes is unbalanced, resulting in low luminous efficiency and high operating voltage. Furthermore, the traditional multi-quantum-well layer and electron-blocking layer structure affects hole injection.

Method used

A hole optimization layer is formed by periodically alternating InAlGaN and MgN layers, located between a multi-quantum well layer and an electron blocking layer, to optimize hole concentration and mobility and reduce the doping concentration of the P-type GaN layer.

Benefits of technology

This improved the luminous efficiency of the light-emitting diode, reduced the operating voltage, enhanced the internal quantum efficiency, and stabilized the performance of the epitaxial wafer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116666511B_ABST
    Figure CN116666511B_ABST
Patent Text Reader

Abstract

This invention discloses a GaN-based light-emitting diode epitaxial wafer and its fabrication method. The GaN-based light-emitting diode epitaxial wafer includes a substrate and a nucleation layer, an intrinsic GaN layer, an N-type GaN layer, a first multiple quantum well layer, a first hole optimization layer, a second multiple quantum well layer, a second hole optimization layer, an electron blocking layer, a third hole optimization layer, and a P-type GaN layer sequentially stacked on the substrate. The first hole optimization layer, the second hole optimization layer, and the third hole optimization layer are all periodic structures formed by alternating InAlGaN layers and MgN layers. The doping concentration of the P-type GaN layer is 1×10⁻⁶. 16 -5×10 17 cm ‑3 The number of cycles in the first multi-quantum-well layer is greater than or equal to the number of cycles in the second multi-quantum-well layer. Implementing this invention can improve the luminous efficiency of a light-emitting diode (LED) while reducing its operating voltage.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of semiconductor technology, and in particular to a GaN-based light-emitting diode epitaxial wafer and its fabrication method. Background Technology

[0002] Epitaxial structure has a significant impact on the photoelectric performance of light-emitting diodes (LEDs). A traditional LED epitaxial wafer includes a substrate and, sequentially grown on the substrate, a nucleation layer, an intrinsic GaN layer, an N-type GaN layer, a multiple quantum well layer, an electron blocking layer, and a P-type GaN layer. Among these, the multiple quantum well layer, as the active region, is the core structure of the LED. The existing multi-quantum well layers have the following problems: (1) Due to the high electron mobility and low hole mobility, and the difficulty in activating holes themselves, the distribution of holes and electrons in the multi-quantum well layer is unbalanced. The hole concentration in the multi-quantum well region near the N-type GaN layer is too low, which affects the luminous efficiency; (2) The traditional electron blocking layer blocks holes while blocking electrons, making it difficult for holes generated by the P-type GaN layer to enter the multi-quantum well layer; (3) There is a potential barrier peak between the traditional multi-quantum well layer and the electron blocking layer, which affects hole injection. Therefore, it is usually necessary to set a high-concentration Mg-doped P-type GaN layer to improve hole injection. However, high-concentration Mg doping will cause the crystal quality of the P-type GaN layer to decrease, resulting in an increase in bulk resistance, which in turn leads to an increase in the operating voltage of the light-emitting diode. Summary of the Invention

[0003] The technical problem to be solved by the present invention is to provide a GaN-based light-emitting diode epitaxial wafer that can improve the luminous efficiency of the light-emitting diode while reducing the operating voltage of the light-emitting diode.

[0004] The technical problem to be solved by the present invention is to provide a method for preparing GaN-based light-emitting diode epitaxial wafers, which has a simple process and produces light-emitting diode epitaxial wafers with stable performance.

[0005] To achieve the above-mentioned technical effects, the present invention provides a GaN-based light-emitting diode epitaxial wafer, comprising a substrate, and a nucleation layer, an intrinsic GaN layer, an N-type GaN layer, a first multiple quantum well layer, a first hole optimization layer, a second multiple quantum well layer, a second hole optimization layer, an electron blocking layer, a third hole optimization layer and a P-type GaN layer sequentially stacked on the substrate.

[0006] The first hole optimization layer is a periodic structure formed by alternating layers of a first InAlGaN layer and a first MgN layer; the second hole optimization layer is a periodic structure formed by alternating layers of a second InAlGaN layer and a second MgN layer; the third hole optimization layer is a periodic structure formed by alternating layers of a third InAlGaN layer and a third MgN layer.

[0007] The doping concentration of the P-type GaN layer is 1×10⁻⁶. 16 -5×10 17 cm -3 ;

[0008] The number of cycles in the first multi-quantum well layer is greater than or equal to the number of cycles in the second multi-quantum well layer.

[0009] As an improvement to the above technical solution, the In component in the first InAlGaN layer is greater than the In component in the second InAlGaN layer, which is greater than the In component in the third InAlGaN layer; the Al component in the first InAlGaN layer is less than the Al component in the third InAlGaN layer, which is less than the Al component in the second InAlGaN layer.

[0010] As an improvement to the above technical solution, the In composition of the first InAlGaN layer is 0.1-0.15 and the Al composition is 0.01-0.05; the In composition of the second InAlGaN layer is 0.05-0.1 and the Al composition is 0.2-0.4; and the In composition of the third InAlGaN layer is 0-0.05 and the Al composition is 0.15-0.2.

[0011] As an improvement to the above technical solution, the number of cycles of the first hole optimization layer is 3-10, the thickness of the first InAlGaN layer is 0.5-3nm, and the thickness of the first MgN layer is 0.5-3nm.

[0012] The number of periods in the second hole optimization layer is 3-10, the thickness of the second InAlGaN layer is 0.5-3 nm, and the thickness of the second MgN layer is 0.5-3 nm.

[0013] The number of periods in the third hole optimization layer is 3-10, the thickness of the third InAlGaN layer is 0.5-3 nm, and the thickness of the third MgN layer is 0.5-3 nm.

[0014] As an improvement to the above technical solution, the number of cycles of the first multi-quantum well layer minus the number of cycles of the second multi-quantum well layer is ≤ 1.

[0015] Accordingly, the present invention also provides a method for preparing a GaN-based light-emitting diode epitaxial wafer, which includes the following steps:

[0016] A substrate is provided on which a nucleation layer, an intrinsic GaN layer, an N-type GaN layer, a first multiple quantum well layer, a first hole-optimized layer, a second multiple quantum well layer, a second hole-optimized layer, an electron-blocking layer, a third hole-optimized layer, and a P-type GaN layer are sequentially grown.

[0017] The first hole optimization layer is a periodic structure formed by alternating layers of a first InAlGaN layer and a first MgN layer; the second hole optimization layer is a periodic structure formed by alternating layers of a second InAlGaN layer and a second MgN layer; the third hole optimization layer is a periodic structure formed by alternating layers of a third InAlGaN layer and a third MgN layer.

[0018] The doping concentration of the P-type GaN layer is 1×10⁻⁶. 16 -5×10 17 cm -3 ;

[0019] The number of cycles in the first multi-quantum well layer is greater than or equal to the number of cycles in the second multi-quantum well layer.

[0020] As an improvement to the above technical solution, the V / II molar ratio of the first MgN layer is greater than that of the second MgN layer, which is greater than that of the third MgN layer.

[0021] As an improvement to the above technical solution, the V / II molar ratio of the first MgN layer is 800-1200; the V / II molar ratio of the second MgN layer is 500-900; and the V / II molar ratio of the third MgN layer is 100-500.

[0022] As an improvement to the above technical solution, the growth temperature of the first hole optimization layer is < the growth temperature of the second hole optimization layer < the growth temperature of the third hole optimization layer.

[0023] As an improvement to the above technical solution,

[0024] The growth temperature of the first hole optimization layer is 800-850℃, and the growth pressure is 100-300 Torr;

[0025] The growth temperature of the second hole optimization layer is 850-900℃, and the growth pressure is 100-300 Torr;

[0026] The growth temperature of the third hole optimization layer is 900-1000℃, and the growth pressure is 100-300 Torr.

[0027] Implementing the embodiments of the present invention has the following beneficial effects:

[0028] The LED epitaxial wafer provided by this invention comprises a first hole optimization layer, a second hole optimization layer, and a third hole optimization layer disposed between a first multiple quantum well layer and a second multiple quantum well layer, between the second multiple quantum well layer and an electron blocking layer, and between the electron blocking layer and a P-type GaN layer. The first hole optimization layer increases the hole concentration in the first multiple quantum well layer, solving the problem of insufficient hole concentration in the multiple quantum well layer near the N-type layer in traditional epitaxial structures. The second hole optimization layer increases the hole concentration entering the multiple quantum well region, improving hole mobility, and also acts as a barrier buffer between the electron blocking layer and the second multiple quantum well layer, preventing the formation of band spikes between the electron blocking layer and the multiple quantum well layer from affecting hole injection in traditional structures. The third hole optimization layer increases hole mobility, making it easier for holes in the P-type GaN layer to pass through the electron blocking layer into the multiple quantum well layer.

[0029] Furthermore, the first hole optimization layer, the second hole optimization layer, and the third hole optimization layer provided by this invention can reduce the doping concentration of the P-type GaN layer while increasing the hole concentration of the multi-quantum well layer, thereby reducing the bulk resistance and lowering the operating voltage. Attached Figure Description

[0030] Figure 1 This is a schematic diagram of the structure of the GaN-based light-emitting diode epitaxial wafer in Embodiment 1 of the present invention;

[0031] Figure 2 This is a flowchart of the method for fabricating a GaN-based light-emitting diode epitaxial wafer in Embodiment 1 of the present invention. Detailed Implementation

[0032] To make the objectives, technical solutions, and advantages of the present invention clearer, the present invention will be further described in detail below with reference to specific embodiments.

[0033] like Figure 1 As shown, an embodiment of the present invention provides a GaN-based light-emitting diode epitaxial wafer, including a substrate 1, and a nucleation layer 2, an intrinsic GaN layer 3, an N-type GaN layer 4, a first multiple quantum well layer 5, a first hole optimization layer 6, a second multiple quantum well layer 7, a second hole optimization layer 8, an electron blocking layer 9, a third hole optimization layer 10, and a P-type GaN layer 11 sequentially stacked on the substrate 1.

[0034] The first hole optimization layer 6 is a periodic structure formed by alternating layers of a first InAlGaN layer and a first MgN layer 62. A large lattice mismatch exists between InAlGaN and the heteromaterial, resulting in a polarization electric field that generates a two-dimensional hole gas. This two-dimensional hole gas helps accelerate hole mobility, thereby increasing the hole concentration of the first multi-quantum well layer 5. InGaN material can increase the matching between the first multi-quantum well layer 5 and the second multi-quantum well layer 7, reducing piezoelectric polarization. However, because In atoms are large, they easily form defects that trap holes. Therefore, smaller Al atoms are added to form an InAlGaN quaternary material. The smaller Al atoms can act as substitution atoms, reducing defect generation. Simultaneously, since Mg is p-type doped, MgN itself can also generate some holes, supplementing the holes in the first multi-quantum well layer 5. The first hole optimization layer 6 increases the hole concentration in the first multi-quantum well layer 5, solving the problem of insufficient hole concentration in multi-quantum well layers near the N-type layer in traditional epitaxial structures due to low hole mobility.

[0035] The second hole optimization layer 8 is a periodic structure formed by alternating layers of the second InAlGaN layer and the second MgN layer 82. The second hole optimization layer 8 can increase the hole concentration entering the multi-quantum well region and improve the hole mobility. The InAlGaN quaternary material can be used as a barrier buffer between the electron blocking layer 9 and the second multi-quantum well layer 7. The barrier height of the electron blocking layer 9 is greater than the barrier height of the second hole optimization layer 8, which is greater than the barrier height of the second multi-quantum well layer 7. The setting of the second hole optimization layer 8 can avoid the influence of the band spike formed between the electron blocking layer and the multi-quantum well layer on hole injection in the traditional structure.

[0036] The third hole optimization layer 10 is a periodic structure formed by alternating layers of a third InAlGaN layer and a third MgN layer 102. The third hole optimization layer 10 can increase the hole concentration and improve the hole mobility, making it easier for holes to pass through the electron blocking layer 9 into the multi-quantum well layer. At the same time, the InAlGaN quaternary material can act as a barrier buffer between the electron blocking layer 9 and the p-type GaN layer 11, avoiding the blocking of holes caused by the electron blocking layer of the traditional structure while blocking electrons.

[0037] The p-type GaN layer 11 is Mg-doped, with a Mg doping concentration of 1×10⁻⁶. 16 -5×10 17 cm -3 The thickness of the p-type GaN layer 11 is 5-60 nm. Because the structure of the first, second, and third hole-optimized layers increases the hole concentration in the entire multi-quantum-well layer, the Mg doping of the p-type GaN layer 11 can be reduced accordingly. The doping concentration of a conventional p-type GaN layer is typically 5 × 10⁻⁶ nm. 17 -1×1020 cm -3 Unlike traditional structures, the P-type GaN layer 11 in this application does not require high-concentration Mg doping to obtain holes. Therefore, the doping concentration can be reduced by 1-3 orders of magnitude, thereby reducing the bulk resistance and lowering the operating voltage.

[0038] The number of cycles in the first quantum well layer 5 is greater than or equal to the number of cycles in the second quantum well layer 7. The first quantum well layer 5, with its larger number of cycles, can alleviate the electron migration rate; the second quantum well layer 7, with its smaller number of cycles, facilitates hole injection, thereby improving the internal quantum efficiency of the LED.

[0039] In one embodiment, the In content of the first InAlGaN layer is greater than that of the second InAlGaN layer, which in turn is greater than that of the third InAlGaN layer. Since the first hole-optimized layer 6 has the highest In content, it improves its lattice matching with the first multiple quantum well layer 5 and the second multiple quantum well layer 7. The third hole-optimized layer 10 is located between the electron-blocking layer 9 and the p-type GaN layer 11, so its In content is relatively low, thereby increasing its energy level matching with the electron-blocking layer 9. Preferably, the In content of the first InAlGaN layer is 0.1-0.15, the In content of the second InAlGaN layer is 0.05-0.1, and the In content of the third InAlGaN layer is 0-0.05.

[0040] In one embodiment, the Al content in the first InAlGaN layer is less than the Al content in the third InAlGaN layer, which is less than the Al content in the second InAlGaN layer. Since the first hole-optimizing layer 6 is located between the first quantum well layer 5 and the second quantum well layer 7, its Al content is relatively minimal, thus improving its lattice matching with the first and second quantum well layers 5 and 7. The second hole-optimizing layer 8 is located between the second quantum well layer 7 and the electron-blocking layer 9, so its Al content is relatively high, enabling it to partially block electrons. Preferably, the Al content in the first InAlGaN layer is 0.01-0.05%, the Al content in the second InAlGaN layer is 0.2-0.4%, and the Al content in the third InAlGaN layer is 0.15-0.2%.

[0041] In one embodiment, the first hole optimization layer has 3-10 periods, the first InAlGaN layer has a thickness of 0.5-3 nm, and the first MgN layer has a thickness of 0.5-3 nm; the second hole optimization layer has 3-10 periods, the second InAlGaN layer has a thickness of 0.5-3 nm, and the second MgN layer has a thickness of 0.5-3 nm; the third hole optimization layer has 3-10 periods, the third InAlGaN layer has a thickness of 0.5-3 nm, and the third MgN layer has a thickness of 0.5-3 nm. If the InAlGaN and MgN layers are too thin, they cannot optimize holes; if the InAlGaN and MgN layers are too thick, they will affect the formation of two-dimensional holes.

[0042] In one embodiment, the number of cycles of the first quantum well layer 5 minus the number of cycles of the second quantum well layer 7 is less than or equal to 1. That is, the number of cycles of the first quantum well layer 5 is the same as the number of cycles of the second quantum well layer 7, or the first quantum well layer 5 has one more cycle than the second quantum well layer 7. By optimizing the number of cycles of the first quantum well layer 5 and the second quantum well layer 7, it is helpful to inject more holes into all well layers of the active layer.

[0043] In addition to the aforementioned composite interface layer, the other layered structures of the present invention have the following characteristics:

[0044] In one embodiment, the substrate 1 is one of a sapphire substrate, a silicon carbide substrate, or a silicon substrate. Preferably, the substrate 1 is a sapphire substrate.

[0045] In one embodiment, the nucleation layer 2 is an AlGaN nucleation layer or an AlN nucleation layer. Preferably, the nucleation layer 2 is an AlGaN nucleation layer. The thickness of the nucleation layer 2 is 20-100 nm. The nucleation layer 2 is mainly used to provide seed crystals, alleviate lattice mismatch between the substrate and the epitaxial layer, and improve the lattice quality of the epitaxial wafer.

[0046] In one embodiment, the thickness of the intrinsic GaN layer 3 is 300-800 nm.

[0047] In one embodiment, the N-type GaN layer 4 is Si-doped with a Si doping concentration of 5 × 10⁻⁶. 18 -1×10 19 cm -3 The thickness of the N-type GaN layer 4 is 1-3 μm. The N-type GaN layer 4 mainly provides electrons.

[0048] In one embodiment, both the first multiple quantum well layer 5 and the second multiple quantum well layer 7 include periodically stacked InGaN quantum well layers and GaN quantum barrier layers, with a period number of 2-8. The thickness of a single InGaN quantum well layer is 2-7 nm, and the thickness of a single GaN quantum barrier layer is 6-15 nm.

[0049] In one embodiment, the electron blocking layer 9 comprises periodically stacked AlGaN and InGaN layers with a period number of 3-15, and the thickness of the electron blocking layer 9 is 30-200 nm.

[0050] like Figure 2 As shown, this invention also discloses a method for fabricating a GaN-based light-emitting diode epitaxial wafer, comprising the following steps:

[0051] S100 provides a substrate:

[0052] The substrate is selected as a sapphire substrate. The reaction chamber temperature is controlled at 1000-1200℃ and the pressure at 200-600 Torr. The substrate is subjected to high-temperature annealing for 5-8 minutes in H2 atmosphere to clean the particles and oxides on the substrate surface.

[0053] S101 nucleation layer:

[0054] The reaction chamber temperature is controlled at 500-700℃ and the pressure at 200-400 Torr. NH3 is introduced to provide the N source, N2 and H2 are used as carrier gases, TMGa is introduced as the Ga source, and TMAl is introduced as the Al source.

[0055] S102 grows intrinsic GaN layers:

[0056] The reaction chamber temperature is controlled at 1100-1150℃, the pressure at 100-500 Torr, NH3 is introduced as the N source, N2 and H2 are used as carrier gases, and TMGa is introduced as the Ga source.

[0057] S103 grows N-type GaN layers:

[0058] The reaction chamber temperature is controlled at 1100-1150℃, the pressure at 100-500 Torr, NH3 is introduced as the N source, N2 and H2 are used as carrier gases, TMGa is introduced as the Ga source, and SiH4 is introduced as the N-type dopant.

[0059] First multi-quantum-well layer grown in S104:

[0060] The reaction chamber temperature was controlled at 700-800℃ and the pressure at 100-500 Torr. NH3 was introduced as the N source, N2 as the carrier gas, TEGa was introduced as the Ga source, and TMIn was introduced as the In source to grow an InGaN quantum well layer. The reaction chamber temperature was controlled at 800-900℃, the In source was turned off, N2 and H2 were used as carrier gases, and TEGa was introduced as the Ga source to grow a GaN quantum barrier layer. The InGaN quantum well layer and GaN quantum barrier layer were repeatedly stacked and periodically grown.

[0061] S105 Growth First Hole Optimization Layer:

[0062] The reaction chamber temperature is controlled at 800-850℃ and the pressure at 100-300 Torr. NH3 is introduced as the N source, N2 and H2 are used as carrier gases, TMIn is introduced as the In source, and TEGa is introduced as the Ga source to grow the first InAlGaN layer. The Ga, In, and Al sources are then turned off, and N2 and H2 are used as carrier gases. NH3 is introduced as the N source, and CP2Mg is introduced as the Mg source, with a V / II molar ratio of 800-1200, to grow the first MgN layer. The V / II molar ratio is the molar ratio of the introduced N source to the Mg source. The first InAlGaN layer and the first MgN layer are then periodically grown by repeated stacking.

[0063] S106 for growing a second multiple quantum well layer:

[0064] The reaction chamber temperature was controlled at 700-800℃ and the pressure at 100-500 Torr. NH3 was introduced as the N source, N2 as the carrier gas, TEGa was introduced as the Ga source, and TMIn was introduced as the In source to grow an InGaN quantum well layer. The reaction chamber temperature was controlled at 800-900℃, the In source was turned off, N2 and H2 were used as carrier gases, and TEGa was introduced as the Ga source to grow a GaN quantum barrier layer. The InGaN quantum well layer and GaN quantum barrier layer were repeatedly stacked and periodically grown.

[0065] S107 Growth of Second Hole Optimization Layer:

[0066] The reaction chamber temperature is controlled at 850-900℃ and the pressure at 100-300 Torr. NH3 is introduced as the N source, N2 and H2 are used as carrier gases, TMIn is introduced as the In source, and TEGa is introduced as the Ga source to grow the second InAlGaN layer. The Ga, In, and Al sources are turned off, N2 and H2 are used as carrier gases, NH3 is introduced as the N source, and CP2Mg is introduced as the Mg source, with a V / II molar ratio of 500-900, to grow the second MgN layer. The second InAlGaN layer and the second MgN layer are grown by repeated stacking and periodic growth.

[0067] S108 growth of electron blocking layer:

[0068] The reaction chamber temperature was controlled at 900-1000℃ and the pressure at 100-500 Torr. NH3 was introduced as the N source, N2 and H2 were used as carrier gases, TMAl was introduced as the Al source, and TEGa was introduced as the Ga source to grow the AlGaN layer. The Al source was then turned off, the Ga source was introduced again, and the In source was turned on to grow the InGaN layer. The AlGaN and InGaN layers were then stacked and grown periodically.

[0069] S109 Growth of Third Hole Optimization Layer:

[0070] The reaction chamber temperature was controlled at 900-1000℃ and the pressure at 100-300 Torr. NH3 was introduced as the N source, N2 and H2 were used as carrier gases, TMIn was introduced as the In source, and TEGa was introduced as the Ga source to grow the third InAlGaN layer. The Ga, In, and Al sources were turned off, N2 and H2 were used as carrier gases, NH3 was introduced as the N source, and CP2Mg was introduced as the Mg source, with a V / II molar ratio of 100-500, to grow the third MgN layer. The third InAlGaN layer and the third MgN layer were then repeatedly stacked and periodically grown.

[0071] By controlling the V / II molar ratio, the Mg content in different MgN layers is controlled, with the Mg content in the first MgN layer < the second MgN layer < the third MgN layer. The first hole-optimized layer 6 has the least Mg content, which facilitates better lattice matching with the first multiple quantum well layer 5 and the second multiple quantum well layer 7; the third hole-optimized layer 10 has the most Mg content, which better matches the P-type layer.

[0072] S110 growth of P-type GaN layers:

[0073] The reaction chamber temperature is controlled at 800-1000℃, the pressure at 100-300 Torr, NH3 is introduced as the N source, N2 and H2 are introduced as carrier gases, TEGa is introduced as the Ga source, and CP2Mg is introduced as the P-type dopant.

[0074] Specifically, an epitaxial wafer growth method is implemented using Veeco C4 MOCVD (Metal Organic Chemical Vapor Deposition) equipment. One of the following gases—high-purity H2, high-purity N2, or a mixture of high-purity H2 and high-purity N2—is used as the carrier gas; high-purity NH3 is used as the N-type source; trimethylgallium (TMGa) and / or triethylgallium (TEGa) are used as the gallium source; trimethylindium (TMIn) is used as the indium source; silane (SiH4) is used as the N-type dopant; trimethylaluminum (TMAl) is used as the aluminum source; and magnesium diacene (CP2Mg) is used as the P-type dopant. These selections are illustrative and not limited to the examples listed above.

[0075] The present invention will be further illustrated below with specific embodiments.

[0076] Example 1

[0077] This embodiment provides a light-emitting diode epitaxial wafer, including a substrate, and a nucleation layer, an intrinsic GaN layer, an N-type GaN layer, a first multiple quantum well layer, a first hole optimization layer, a second multiple quantum well layer, a second hole optimization layer, an electron blocking layer, a third hole optimization layer, and a P-type GaN layer sequentially stacked on the substrate.

[0078] The substrate is a sapphire substrate.

[0079] The nucleation layer is an AlGaN nucleation layer with a thickness of 30 nm.

[0080] The thickness of the intrinsic GaN layer is 400 nm.

[0081] The Si doping concentration in the N-type GaN layer is 7 × 10⁻⁶. 18 cm -3 The thickness is 2μm.

[0082] The first multiple quantum well layer comprises periodically alternating InGaN quantum well layers and GaN quantum barrier layers, with a period number of 5. The InGaN quantum well layer has a thickness of 3 nm, and the GaN quantum barrier layer has a thickness of 10 nm.

[0083] The first hole optimization layer includes a first In layer that grows periodically and alternately. 0.1 Al 0.1 Ga 0.8 The N layer and the first MgN layer have a period number of 5. The first In layer... 0.1 Al 0.1 Ga 0.8 The thickness of the N layer is 2 nm, and the thickness of the first MgN layer is 2 nm.

[0084] The second multiple quantum well layer consists of periodically alternating InGaN quantum well layers and GaN quantum barrier layers, with a period number of 5. The InGaN quantum well layer has a thickness of 3 nm, and the GaN quantum barrier layer has a thickness of 10 nm.

[0085] The second hole optimization layer includes a second In layer that grows periodically and alternately. 0.2 Al 0.1 Ga 0.7 The N layer and the second MgN layer have a period number of 5. Among them, the second In... 0.2 Al 0.1 Ga 0.7 The thickness of the N layer is 2 nm, and the thickness of the second MgN layer is 2 nm.

[0086] The electron blocking layer consists of periodically alternating AlGaN and InGaN layers, with a period of 8. The AlGaN layer has a thickness of 3 nm, and the InGaN layer has a thickness of 3 nm.

[0087] The third hole optimization layer includes a third In layer that grows periodically and alternately. 0.1 Al 0.05 Ga 0.85 The N layer and the third MgN layer have a period number of 5. The third In layer... 0.1 Al 0.05 Ga 0.85 The thickness of the N layer is 2 nm, and the thickness of the third MgN layer is 2 nm.

[0088] The Mg doping concentration in the p-type GaN layer is 1×10⁻⁶. 17 cm -3 The thickness is 10nm.

[0089] The above-mentioned method for fabricating an epitaxial wafer of a light-emitting diode includes the following steps:

[0090] S100 provides a substrate:

[0091] Sapphire substrate was selected. The reaction chamber temperature was controlled at 1000℃ and the pressure at 200 Torr. The substrate was subjected to high-temperature annealing for 6 minutes in an H2 atmosphere to clean the particles and oxides on the substrate surface.

[0092] S101 nucleation layer:

[0093] The reaction chamber temperature was controlled at 600℃ and the pressure at 200 Torr. NH3 was introduced to provide the N source, N2 and H2 were used as carrier gases, TMGa was introduced as the Ga source, and TMAl was introduced as the Al source.

[0094] S102 grows intrinsic GaN layers:

[0095] The reaction chamber temperature was controlled at 1120℃ and the pressure at 200 Torr. NH3 was introduced as the N source, N2 and H2 were used as carrier gases, and TMGa was introduced as the Ga source.

[0096] S103 grows N-type GaN layers:

[0097] The reaction chamber temperature was controlled at 1150℃ and the pressure at 220 Torr. NH3 was introduced as the N source, N2 and H2 were introduced as carrier gases, TMGa was introduced as the Ga source, and SiH4 was introduced as the N-type dopant.

[0098] First multi-quantum-well layer grown in S104:

[0099] The reaction chamber temperature was controlled at 750℃ and the pressure at 200 Torr. NH3 was introduced as the N source, N2 as the carrier gas, TEGa was introduced as the Ga source, and TMIn was introduced as the In source to grow an InGaN quantum well layer. The reaction chamber temperature was controlled at 850℃, the In source was turned off, N2 and H2 were used as carrier gases, and TEGa was introduced as the Ga source to grow a GaN quantum barrier layer. The InGaN quantum well layer and GaN quantum barrier layer were repeatedly stacked and periodically grown.

[0100] S105 Growth First Hole Optimization Layer:

[0101] The reaction chamber temperature was controlled at 820℃ and the pressure at 220 Torr. NH3 was introduced as the N source, N2 and H2 were used as carrier gases, TMIn was introduced as the In source, and TEGa was introduced as the Ga source to grow the first In. 0.1 Al 0.1 Ga 0.8 N layer; turn off Ga, In, and Al sources, use N2 and H2 as carrier gases, introduce NH3 as the N source, and introduce CP2Mg as the Mg source, with a V / II molar ratio of 1000, to grow the first MgN layer; repeat the stacking process to periodically grow the first In layer. 0.1 Al 0.1 Ga 0.8 N layer and first MgN layer.

[0102] S106 for growing a second multiple quantum well layer:

[0103] The reaction chamber temperature was controlled at 750℃ and the pressure at 200 Torr. NH3 was introduced as the N source, N2 as the carrier gas, TEGa was introduced as the Ga source, and TMIn was introduced as the In source to grow an InGaN quantum well layer. The reaction chamber temperature was controlled at 850℃, the In source was turned off, N2 and H2 were used as carrier gases, and TEGa was introduced as the Ga source to grow a GaN quantum barrier layer. The InGaN quantum well layer and GaN quantum barrier layer were repeatedly stacked and periodically grown.

[0104] S107 Growth of Second Hole Optimization Layer:

[0105] The reaction chamber temperature was controlled at 880℃ and the pressure at 200 Torr. NH3 was introduced as the N source, N2 and H2 were used as carrier gases, TMIn was introduced as the In source, and TEGa was introduced as the Ga source to grow the second In. 0.2 Al 0.1 Ga 0.7 N layer; turn off Ga, In, and Al sources, use N2 and H2 as carrier gases, introduce NH3 as the N source, and introduce CP2Mg as the Mg source, with a V / II molar ratio of 800, to grow the second MgN layer; repeat the stacking process to periodically grow the second In layer. 0.2 Al 0.1 Ga 0.7N layer and second MgN layer.

[0106] S108 growth of electron blocking layer:

[0107] The reaction chamber temperature was controlled at 950℃ and the pressure at 200 Torr. NH3 was introduced as the N source, N2 and H2 were used as carrier gases, TMAl was introduced as the Al source, and TEGa was introduced as the Ga source to grow an AlGaN layer. The Al source was then turned off, the Ga source was introduced again, and the In source was turned on to grow an InGaN layer. The AlGaN and InGaN layers were then stacked and grown periodically.

[0108] S109 Growth of Third Hole Optimization Layer:

[0109] The reaction chamber temperature was controlled at 950℃ and the pressure at 200 Torr. NH3 was introduced as the N source, N2 and H2 were used as carrier gases, TMIn was introduced as the In source, and TEGa was introduced as the Ga source to grow the third In. 0.1 Al 0.05 Ga 0.85 N layer; turn off Ga, In, and Al sources, use N2 and H2 as carrier gases, introduce NH3 as the N source, and introduce CP2Mg as the Mg source, with a V / II molar ratio of 400, to grow the third MgN layer; repeat the stacking process to periodically grow the third In layer. 0.1 Al 0.05 Ga 0.85 N layer and third MgN layer.

[0110] S110 growth of P-type GaN layers:

[0111] The reaction chamber temperature was controlled at 900℃ and the pressure at 200 Torr. NH3 was introduced as the N source, N2 and H2 were introduced as the carrier gas, TEGa was introduced as the Ga source, and CP2Mg was introduced as the P-type dopant.

[0112] Example 2

[0113] This embodiment provides a light-emitting diode epitaxial wafer, which differs from Embodiment 1 in that the compositions of the first InAlGaN layer, the second InAlGaN layer, and the third InAlGaN layer are different, while the rest are the same as in Embodiment 1.

[0114] Specifically, the first hole optimization layer includes a first In layer that grows in a periodically alternating manner. 0.12 Al 0.03 Ga 0.85 The N layer and the first MgN layer; the second hole-optimized layer includes a second In layer that grows in a periodically alternating manner. 0.07 Al 0.3 Ga 0.63 The N layer and the second MgN layer; the third hole optimization layer includes a third In layer that grows in a periodically alternating manner. 0.04Al 0.16 Ga 0.8 N layer and third MgN layer.

[0115] Example 3

[0116] This embodiment provides a light-emitting diode epitaxial wafer, which differs from Embodiment 1 in that the compositions of the first InAlGaN layer, the second InAlGaN layer, and the third InAlGaN layer are different, and the number of cycles of the first multi-quantum well layer minus the number of cycles of the second multi-quantum well layer is ≤1. The rest is the same as Embodiment 1.

[0117] Specifically, the first hole optimization layer includes a first In layer that grows in a periodically alternating manner. 0.12 Al 0.03 Ga 0.85 The N layer and the first MgN layer; the second hole-optimized layer includes a second In layer that grows in a periodically alternating manner. 0.07 Al 0.3 Ga 0.63 The N layer and the second MgN layer; the third hole optimization layer includes a third In layer that grows in a periodically alternating manner. 0.04 Al 0.16 Ga 0.8 The N-layer and the third MgN-layer. The first multi-quantum well layer has 6 periods, and the second multi-quantum well layer has 5 periods.

[0118] Comparative Example 1

[0119] This comparative example provides a light-emitting diode epitaxial wafer, which differs from Example 1 in that it does not have a first hole optimization layer, a second hole optimization layer, and a third hole optimization layer, and the Mg doping concentration in the P-type GaN layer is 1×10⁻⁶. 19 cm -3 The corresponding preparation method does not include the growth of the first hole optimization layer, the second hole optimization layer and the third hole optimization layer, but is otherwise the same as in Example 1.

[0120] Comparative Example 2

[0121] This comparative example provides a light-emitting diode epitaxial wafer, which differs from Example 1 in that it does not have a first hole optimization layer, and the corresponding preparation method does not include the growth of the first hole optimization layer; otherwise, it is the same as Example 1.

[0122] Comparative Example 3

[0123] This comparative example provides a light-emitting diode epitaxial wafer, which differs from Example 1 in that it does not have a second hole optimization layer, and the corresponding preparation method does not include the growth of the second hole optimization layer; otherwise, it is the same as Example 1.

[0124] Comparative Example 4

[0125] This comparative example provides a light-emitting diode epitaxial wafer, which differs from Example 1 in that it does not have a third hole optimization layer, and the corresponding preparation method does not include the growth of the third hole optimization layer; otherwise, it is the same as Example 1.

[0126] Performance testing:

[0127] LED chips with a vertical structure of 10mil × 24mil were fabricated from the epitaxial wafers of light-emitting diodes prepared in Examples 1-3 and Comparative Examples 1-4, and their luminous intensity (120mA) and operating voltage were tested. The test results are shown in Table 1.

[0128] Table 1. Photoelectric performance test results of LED epitaxial wafers

[0129] Brightness (mW) Operating voltage (V) Example 1 198.6 3.165 Example 2 199.1 3.163 Example 3 199.5 3.160 Comparative Example 1 194.7 3.210 Comparative Example 2 194.3 3.192 Comparative Example 3 194.1 3.190 Comparative Example 4 194.0 3.188

[0130] As can be seen from the comparison between Example 1 and Comparative Example 1, the chip made from the light-emitting diode epitaxial wafer provided in Example 1 of the present invention can reduce the operating voltage while improving the light-emitting brightness.

[0131] The above description represents the preferred embodiments of the present invention. It should be noted that those skilled in the art can make various improvements and modifications without departing from the principles of the present invention, and these improvements and modifications are also considered to be within the scope of protection of the present invention.

Claims

1. A GaN-based light-emitting diode epitaxial wafer, characterized in that, It includes a substrate, and a nucleation layer, an intrinsic GaN layer, an N-type GaN layer, a first multiple quantum well layer, a first hole optimization layer, a second multiple quantum well layer, a second hole optimization layer, an electron blocking layer, a third hole optimization layer and a P-type GaN layer sequentially stacked on the substrate; The first hole optimization layer is a periodic structure formed by alternating layers of a first InAlGaN layer and a first MgN layer; the second hole optimization layer is a periodic structure formed by alternating layers of a second InAlGaN layer and a second MgN layer; the third hole optimization layer is a periodic structure formed by alternating layers of a third InAlGaN layer and a third MgN layer. The doping concentration of the P-type GaN layer is 1×10⁻⁶. 16 -5×10 17 cm -3 ; The number of cycles in the first multi-quantum well layer is greater than or equal to the number of cycles in the second multi-quantum well layer.

2. The GaN-based light-emitting diode epitaxial wafer as described in claim 1, characterized in that, The In content of the first InAlGaN layer is greater than that of the second InAlGaN layer, which is greater than that of the third InAlGaN layer; the Al content of the first InAlGaN layer is less than that of the third InAlGaN layer, which is less than that of the second InAlGaN layer.

3. The GaN-based light-emitting diode epitaxial wafer as described in claim 2, characterized in that, The first InAlGaN layer has an In content of 0.1-0.15 and an Al content of 0.01-0.05; the second InAlGaN layer has an In content of 0.05-0.1 and an Al content of 0.2-0.4; and the third InAlGaN layer has an In content of 0-0.05 and an Al content of 0.15-0.

2.

4. The GaN-based light-emitting diode epitaxial wafer as described in claim 1, characterized in that, The number of periods in the first hole optimization layer is 3-10, the thickness of the first InAlGaN layer is 0.5-3 nm, and the thickness of the first MgN layer is 0.5-3 nm. The number of periods in the second hole optimization layer is 3-10, the thickness of the second InAlGaN layer is 0.5-3 nm, and the thickness of the second MgN layer is 0.5-3 nm. The number of periods in the third hole optimization layer is 3-10, the thickness of the third InAlGaN layer is 0.5-3 nm, and the thickness of the third MgN layer is 0.5-3 nm.

5. The GaN-based light-emitting diode epitaxial wafer as described in claim 1, characterized in that, The number of cycles in the first multi-quantum well layer minus the number of cycles in the second multi-quantum well layer is less than or equal to 1.

6. A method for fabricating a GaN-based light-emitting diode epitaxial wafer, used to fabricate the GaN-based light-emitting diode epitaxial wafer as described in any one of claims 1-5, characterized in that, Includes the following steps: A substrate is provided on which a nucleation layer, an intrinsic GaN layer, an N-type GaN layer, a first multiple quantum well layer, a first hole-optimized layer, a second multiple quantum well layer, a second hole-optimized layer, an electron-blocking layer, a third hole-optimized layer, and a P-type GaN layer are sequentially grown. The first hole optimization layer is a periodic structure formed by alternating layers of a first InAlGaN layer and a first MgN layer; the second hole optimization layer is a periodic structure formed by alternating layers of a second InAlGaN layer and a second MgN layer; the third hole optimization layer is a periodic structure formed by alternating layers of a third InAlGaN layer and a third MgN layer. The doping concentration of the P-type GaN layer is 1×10⁻⁶. 16 -5×10 17 cm -3 ; The number of cycles in the first multi-quantum well layer is greater than or equal to the number of cycles in the second multi-quantum well layer.

7. The method for fabricating a light-emitting diode epitaxial wafer as described in claim 6, characterized in that, The V / II molar ratio of the first MgN layer is greater than that of the second MgN layer, which is greater than that of the third MgN layer.

8. The method for fabricating a light-emitting diode epitaxial wafer as described in claim 7, characterized in that, The V / II molar ratio of the first MgN layer is 800-1200; the V / II molar ratio of the second MgN layer is 500-900; and the V / II molar ratio of the third MgN layer is 100-500.

9. The method for fabricating a light-emitting diode epitaxial wafer as described in claim 6, characterized in that, The growth temperature of the first hole optimization layer is < the growth temperature of the second hole optimization layer < the growth temperature of the third hole optimization layer.

10. The method for fabricating a light-emitting diode epitaxial wafer as described in claim 9, characterized in that, The growth temperature of the first hole optimization layer is 800-850℃, and the growth pressure is 100-300 Torr; The growth temperature of the second hole optimization layer is 850-900℃, and the growth pressure is 100-300 Torr; The growth temperature of the third hole optimization layer is 900-1000℃, and the growth pressure is 100-300 Torr.

Citation Information

Patent Citations

  • Preparation method for semiconductor light-emitting device

    CN104795472A

  • Nitride semiconductor element and its fabrication process

    JP2006313845A