Method for manufacturing a semiconductor structure and semiconductor structure

By forming gate oxide layers of varying thickness and length on the second sidewall of the active pillar, the problem of gate-induced drain leakage in semiconductor structures is solved, thereby improving the performance and yield of semiconductor structures.

CN116669419BActive Publication Date: 2026-11-20CHANGXIN MEMORY TECH INC +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310705736.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-30
Publication Date
2026-11-20
Estimated Expiration
2041-11-30

Smart Images

  • Figure CN116669419B_ABST
    Figure CN116669419B_ABST
Patent Text Reader

Abstract

The present disclosure provides a semiconductor structure manufacturing method and a semiconductor structure, and relates to the technical field of semiconductors. The semiconductor structure manufacturing method comprises the following steps: providing a substrate; forming an active pillar on the substrate, the active pillar comprising a first segment, a second segment and a third segment connected in sequence, forming a first gate oxide layer on the sidewall of the second segment, the top surface of the first segment and the bottom surface of the third segment along a first direction; forming a second gate oxide layer on the first gate oxide layer, the length of the second gate oxide layer being less than the length of the first gate oxide layer, the second gate oxide layer being arranged close to the third segment, and the thickness of the second gate oxide layer being greater than the thickness of the first gate oxide layer. The present disclosure forms two layers of gate oxide layers with different thicknesses at different positions on the second segment of the active pillar, thereby effectively reducing gate-induced drain leakage current, and further improving the performance and yield of the semiconductor structure.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of an earlier application (Invention title: Method for manufacturing semiconductor structure and semiconductor structure; Application date: November 30, 2021; Application number: 202111444498.7). Technical Field

[0002] This disclosure relates to the field of semiconductor technology, and in particular to a method for fabricating a semiconductor structure and the semiconductor structure itself. Background Technology

[0003] Dynamic random access memory (DRAM) is a semiconductor memory that allows for high-speed, random data writing and reading, and is widely used in data storage devices. DRAM consists of multiple repeatedly arranged memory cells, each including a transistor and a capacitor. The capacitor is connected to the source and drain of the transistor through capacitor contact areas and structures. As electronic products increasingly strive for lighter, thinner, shorter, and smaller designs, the design of DRAM components is also evolving towards higher integration, higher density, and miniaturization.

[0004] With the development of semiconductor technology, the size of semiconductor devices is getting smaller and smaller. Gate-induced drain leakage (GIDL) will have a significant adverse effect on the formation of semiconductor structures, reducing the performance and yield of semiconductor structures. Summary of the Invention

[0005] The following is an overview of the subject matter described in detail in this disclosure. This overview is not intended to limit the scope of the claims.

[0006] This disclosure provides a method for fabricating a semiconductor structure and the semiconductor structure itself.

[0007] The first aspect of this disclosure provides a method for fabricating a semiconductor structure, the method comprising:

[0008] Provide a base;

[0009] Multiple active pillars are formed on the substrate, and the multiple active pillars are arranged in an array. Along the first direction, each active pillar includes a first segment, a second segment, and a third segment connected in sequence, with a plane perpendicular to the first direction as its cross-section. The cross-sectional area of ​​the second segment is smaller than that of the first segment and the third segment.

[0010] A first gate oxide layer is formed on the sidewall of the second segment, the top surface of the first segment, and the bottom surface of the third segment;

[0011] A second gate oxide layer is formed on the sidewall of the first gate oxide layer. Along the first direction, the length of the second gate oxide layer is less than the length of the first gate oxide layer, and the second gate oxide layer is disposed close to the third segment. The thickness of the second gate oxide layer is greater than the thickness of the first gate oxide layer.

[0012] According to some embodiments of this disclosure, the thickness of the second gate oxide layer is 1 to 2 times the thickness of the first gate oxide layer.

[0013] According to some embodiments of this disclosure, forming a plurality of active pillars on the substrate includes:

[0014] Multiple bit line isolation structures are formed within the substrate, and the multiple bit line isolation structures are spaced apart along a second direction. The substrate between adjacent bit line isolation structures forms a strip.

[0015] The strip-shaped body is processed to form a silicon pillar structure, which includes a first part, a second part, and a third part along a first direction;

[0016] Multiple word line isolation structures are formed within the substrate, and the multiple word line isolation structures are spaced apart along a third direction. The second direction intersects the third direction on the same horizontal plane, wherein the silicon pillar structure between adjacent word line isolation structures forms a silicon pillar.

[0017] A portion of the silicon pillars undergoes a pre-processing step to form the active pillars.

[0018] According to some embodiments of this disclosure, forming a plurality of bit line isolation structures within the substrate, wherein the plurality of bit line isolation structures are spaced apart along a second direction, includes:

[0019] A plurality of bit line trenches spaced apart along a second direction are formed within the substrate;

[0020] A bit line isolation structure is formed within the bit line trench.

[0021] According to some embodiments of this disclosure, forming a plurality of word line isolation structures within the substrate, wherein the plurality of word line isolation structures are spaced apart along a third direction, includes:

[0022] A plurality of word line trenches are formed in the substrate at intervals along a third direction, wherein, along the first direction, the depth of the word line trenches is less than the depth of the bit line trenches;

[0023] A first dielectric layer is formed on the sidewall of the word line groove, and a first groove is formed between the first dielectric layers on the two sidewalls of the word line groove along the second direction;

[0024] A word line isolation structure is formed within the first trench;

[0025] A portion of the first dielectric layer is removed to expose the top surface of the silicon pillar structure.

[0026] According to some embodiments of this disclosure, the step of forming the word line isolation structure within the first trench further includes:

[0027] A bit line is formed at the bottom of the first trench, and there are multiple bit lines, which are spaced apart along the second direction.

[0028] According to some embodiments of this disclosure, the method for fabricating the semiconductor structure further includes:

[0029] Along the second direction, a support structure is formed on both sides of the word line isolation structure.

[0030] According to some embodiments of this disclosure, forming support structures on both sides of the word line isolation structure includes:

[0031] A portion of the first dielectric layer and a portion of the bit line isolation structure are removed to expose a portion of the word line isolation structure and a portion of the silicon pillar structure, and a second trench is formed between the word line isolation structure and the silicon pillar structure along a second direction;

[0032] A support structure is formed within the second trench.

[0033] According to some embodiments of this disclosure, the step of performing a pre-processing on a portion of the silicon pillars to form the active pillars includes:

[0034] Remove a portion of the first dielectric layer and a portion of the bit line isolation structure to expose the second portion;

[0035] The second portion of the silicon pillar is subjected to an oxidation process to remove part of the second portion, forming the active pillar, wherein the first portion of the silicon pillar forms the first segment of the active pillar, the second portion of the silicon pillar that is retained forms the second segment of the active pillar, and the third portion of the silicon pillar forms the third segment of the active pillar.

[0036] According to some embodiments of this disclosure, a third groove is formed between the second segment and the word line isolation structure;

[0037] The formation of a first gate oxide layer on the sidewall of the second segment, the top surface of the first segment, and the bottom surface of the third segment includes:

[0038] An atomic layer deposition process is used to form a first gate oxide layer on the sidewall of the third trench, and the first gate oxide layer in the third trench forms a fourth trench.

[0039] According to some embodiments of this disclosure, forming a second gate oxide layer on the first gate oxide layer includes:

[0040] A first initial character line is formed in the fourth groove, and the first initial character line fills the fourth groove;

[0041] A portion of the first initial word line is removed, and the remaining first initial word line forms the first word line. A fifth trench is formed between the first word line and the first gate oxide layer.

[0042] A second gate oxide layer is formed in the fifth trench and on the sidewall of the first gate oxide layer, and a sixth trench is formed on the sidewall of the second gate oxide layer and the top surface of the first word line.

[0043] A second initial character line is formed within the sixth groove;

[0044] By removing a portion of the second initial character line, the remaining second initial character line forms the second character line, wherein the first character line and the second character line form a character line structure.

[0045] According to some embodiments of this disclosure, forming a second gate oxide layer on the first gate oxide layer includes:

[0046] A sacrificial layer is formed in the fourth trench, and the sacrificial layer fills the fourth trench;

[0047] A portion of the sacrificial layer is removed, and a fifth trench is formed between the remaining sacrificial layer and the sidewall of the first gate oxide layer.

[0048] A second gate oxide layer is formed within the fifth trench and on the sidewall of the first gate oxide layer;

[0049] The remaining sacrificial layer is removed, and a seventh trench is formed between the sidewall of the second gate oxide layer and the sidewall of the first gate oxide layer at the location where the sacrificial layer was removed;

[0050] A character line structure is formed within the seventh groove.

[0051] According to some embodiments of this disclosure, the method for fabricating the semiconductor structure further includes:

[0052] A second dielectric layer is formed on the word line structure, and the top surface of the second dielectric layer is flush with the top surface of the active column.

[0053] A second aspect of this disclosure provides a semiconductor structure, the semiconductor structure comprising:

[0054] Base;

[0055] An active column, wherein there are multiple active columns, and an array of multiple active columns is arranged in the substrate, wherein, along the first direction, the active column includes a first segment, a second segment and a third segment connected in sequence, with a plane perpendicular to the first direction as the cross-section, and the cross-sectional area of ​​the second segment is smaller than the cross-sectional areas of the first segment and the third segment;

[0056] A first gate oxide layer is disposed on the sidewall of the second segment, the top surface of the first segment, and the bottom surface of the third segment;

[0057] A second gate oxide layer is disposed on the sidewall of the first gate oxide layer. Along the first direction, the length of the second gate oxide layer is less than the length of the first gate oxide layer, and the second gate oxide layer is disposed close to the third segment. The thickness of the second gate oxide layer is greater than the thickness of the first gate oxide layer.

[0058] According to some embodiments of this disclosure, the semiconductor structure further includes a plurality of bit line isolation structures and a plurality of word line isolation structures;

[0059] Along the second direction, a plurality of the bit line isolation structures are spaced apart;

[0060] Along a third direction, multiple word line isolation structures are spaced apart.

[0061] According to some embodiments of this disclosure, the semiconductor structure further includes a plurality of bit lines, the plurality of bit lines being spaced apart along a second direction, the bit lines being located below the active pillar.

[0062] According to some embodiments of this disclosure, the semiconductor structure further includes a plurality of word line structures, the plurality of word line structures being spaced apart along a third direction;

[0063] The word line structure is arranged around the second segment of the active column. The word line structure includes a first word line and a second word line. The bottom surface of the first word line is close to the first segment, and the top surface of the second word line is close to the third segment. The longitudinal section is a plane perpendicular to the second direction. The area of ​​the longitudinal section of the first word line is greater than the area of ​​the longitudinal section of the second word line.

[0064] In the semiconductor structure fabrication method and semiconductor structure provided in this disclosure, by forming a first gate oxide layer on the sidewall of the second segment of the active pillar and forming a second gate oxide layer on the first gate oxide layer, the charge storage capacity of the gate oxide layer is increased, thereby effectively reducing the problems of gate-induced drain leakage current and inter-band tunneling. On the other hand, by making the length of the second gate oxide layer shorter than the length of the first gate oxide layer and the thickness of the second gate oxide layer greater than the thickness of the first gate oxide layer, and by placing the second gate oxide layer close to the third segment, gate oxide layers of different thicknesses are formed at different positions in the second segment, which is beneficial for controlling the turn-off current of the semiconductor structure, thereby effectively improving the performance and yield of the semiconductor structure.

[0065] After reading and understanding the accompanying diagrams and detailed descriptions, the other aspects can be understood. Attached Figure Description

[0066] The accompanying drawings, which are incorporated in and form a part of this specification, illustrate embodiments of the present disclosure and, together with the description, serve to explain the principles of these embodiments. In these drawings, similar reference numerals are used to denote similar elements. The drawings described below are some embodiments of the present disclosure, but not all embodiments. Other drawings will be readily available to those skilled in the art from these drawings without inventive effort.

[0067] Figure 1 This is a flowchart illustrating a method for fabricating a semiconductor structure according to an exemplary embodiment.

[0068] Figure 2 This is a schematic diagram illustrating the formation of a strip in a method for fabricating a semiconductor structure according to an exemplary embodiment.

[0069] Figure 3 This is a schematic diagram illustrating the formation of a silicon pillar structure in a method for fabricating a semiconductor structure according to an exemplary embodiment.

[0070] Figure 4 This is a schematic diagram illustrating a method for fabricating a semiconductor structure according to an exemplary embodiment, in which a first initial dielectric layer and silicon pillars are formed.

[0071] Figure 5 This is a schematic diagram illustrating a method for fabricating a semiconductor structure according to an exemplary embodiment, showing the formation of a first transition dielectric layer and bit lines.

[0072] Figure 6 This is a schematic diagram illustrating a method for fabricating a semiconductor structure according to an exemplary embodiment, in which a first dielectric layer and a word line isolation structure are formed.

[0073] Figure 7This is a schematic diagram illustrating the formation of a second trench in a method for fabricating a semiconductor structure according to an exemplary embodiment.

[0074] Figure 8 This is a schematic diagram illustrating the formation of a support structure in a method for fabricating a semiconductor structure according to an exemplary embodiment.

[0075] Figure 9 This is a schematic diagram illustrating the removal of a portion of the first dielectric layer in a method for fabricating a semiconductor structure according to an exemplary embodiment.

[0076] Figure 10 This is a schematic diagram illustrating the formation of a third trench in a method for fabricating a semiconductor structure according to an exemplary embodiment.

[0077] Figure 11 This is a schematic diagram illustrating the formation of a first gate oxide layer in a method for fabricating a semiconductor structure according to an exemplary embodiment.

[0078] Figure 12 This is a schematic diagram illustrating the formation of a first word line in a method for fabricating a semiconductor structure according to an exemplary embodiment.

[0079] Figure 13 This is a schematic diagram illustrating the formation of a second gate oxide layer in a method for fabricating a semiconductor structure according to an exemplary embodiment.

[0080] Figure 14 This is a schematic diagram illustrating the formation of a second word line in a method for fabricating a semiconductor structure according to an exemplary embodiment.

[0081] Figure 15 This is a schematic diagram illustrating the formation of a second dielectric layer in a method for fabricating a semiconductor structure according to an exemplary embodiment.

[0082] Figure 16 This is a schematic diagram illustrating the formation of a sacrificial layer in a method for fabricating a semiconductor structure according to an exemplary embodiment.

[0083] Figure 17 This is a schematic diagram illustrating the formation of a second gate oxide layer and a seventh trench in a semiconductor structure fabrication method according to an exemplary embodiment.

[0084] Figure 18 This is a schematic diagram illustrating the formation of a word line structure and a second dielectric layer in a method for fabricating a semiconductor structure according to an exemplary embodiment.

[0085] Figure label:

[0086] 10. Substrate; 20. Active column;

[0087] 30. Partial isolation structure; 40. Strip-shaped body;

[0088] 41. Silicon pillar structure; 42. Silicon pillar;

[0089] 50. Bit line groove; 60. Word line isolation structure;

[0090] 70. Word line groove; 80. First dielectric layer;

[0091] 81. First initial dielectric layer; 82. First transition dielectric layer;

[0092] 90. First trench; 100. Bit line;

[0093] 110. Support structure; 120. Second trench;

[0094] 130. Third trench; 140. First gate oxide layer;

[0095] 150. Fourth trench; 160. Second gate oxide layer;

[0096] 170, First line; 180, Fifth groove;

[0097] 190, Sixth groove; 200, Second letter line;

[0098] 201. First paragraph; 202. Second paragraph;

[0099] 203. The third paragraph; 210. Character structure;

[0100] 220, Sacrificial Layer; 230, Seventh Trench;

[0101] 240. Second dielectric layer; 411. First part;

[0102] 412. Part Two; 413. Part Three. Detailed Implementation

[0103] To make the objectives, technical solutions, and advantages of the embodiments of this disclosure clearer, the technical solutions in the disclosed embodiments will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some, not all, of the embodiments of this disclosure. All other embodiments obtained by those skilled in the art based on the embodiments of this disclosure without creative effort are within the scope of protection of this disclosure. It should be noted that, unless otherwise specified, the embodiments and features in the embodiments of this disclosure can be arbitrarily combined with each other.

[0104] Dynamic random access memory (DRAM) is a semiconductor memory that allows for high-speed, random data writing and reading, and is widely used in data storage devices. DRAM consists of multiple repeatedly arranged memory cells, each including a transistor and a capacitor. The capacitor is connected to the source and drain of the transistor through capacitor contact areas and structures. As electronic products increasingly strive for lighter, thinner, shorter, and smaller designs, the design of DRAM components is also evolving towards higher integration, higher density, and miniaturization.

[0105] In semiconductor structures, a transistor can be understood as a current-switching structure made of semiconductor material. A metal gate is placed between the source and drain of the transistor, and this metal gate is used to control the flow of current between the source and drain. One type of transistor is the GAA transistor (Gate-All-Around), which uses gate-all-around technology. With the development of semiconductor technology, the size of semiconductor devices is becoming smaller and smaller. During the fabrication of GAA transistors, there is a problem of gate-induced drain leakage (GIDL), which reduces the performance and yield of the semiconductor structure.

[0106] In the semiconductor structure fabrication method and semiconductor structure provided in this disclosure, by forming a first gate oxide layer on the sidewall of the second segment of the active pillar and forming a second gate oxide layer on the first gate oxide layer, the charge storage capacity of the gate oxide layer is increased, thereby effectively reducing the problems of gate-induced drain leakage current and inter-band tunneling. On the other hand, by making the length of the second gate oxide layer shorter than the length of the first gate oxide layer and the thickness of the second gate oxide layer greater than the thickness of the first gate oxide layer, and by placing the second gate oxide layer close to the third segment, gate oxide layers of different thicknesses are formed at different positions in the second segment, which is beneficial for controlling the turn-off current of the semiconductor structure, thereby effectively improving the performance and yield of the semiconductor structure.

[0107] This disclosure provides a method for fabricating a semiconductor structure in exemplary embodiments, which will be described below in conjunction with... Figures 1-18 The methods for fabricating semiconductor structures are introduced.

[0108] This embodiment does not limit the semiconductor structure. The following description will take dynamic random access memory (DRAM) as an example, but this embodiment is not limited to this. The semiconductor structure in this embodiment can also be other structures, such as GAA transistors or vertical gate ring transistors.

[0109] like Figure 1As shown, an exemplary embodiment of this disclosure provides a method for fabricating a semiconductor structure, including the following steps:

[0110] Step S100: Provide a substrate.

[0111] Step S200: Multiple active pillars are formed on the substrate, and the multiple active pillars are arranged in an array. Along the first direction, the active pillars include a first segment, a second segment, and a third segment connected in sequence. Along the first direction, the cross-sectional area of ​​the second segment is smaller than the cross-sectional areas of the first segment and the third segment.

[0112] Step S300: A first gate oxide layer is formed on the sidewall of the second segment, the top surface of the first segment, and the bottom surface of the third segment.

[0113] Step S400: A second gate oxide layer is formed on the first gate oxide layer. Along the first direction, the length of the second gate oxide layer is less than the length of the first gate oxide layer, and the second gate oxide layer is disposed close to the third segment. The thickness of the second gate oxide layer is greater than the thickness of the first gate oxide layer.

[0114] According to an exemplary embodiment, this embodiment is a further description of step S100 above, and the method in this embodiment includes the following.

[0115] like Figure 2 As shown, a substrate 10 is provided. The substrate 10 serves as a support component for a dynamic random access memory (DRAM) and is used to support other components disposed thereon. The substrate 10 may be made of a semiconductor material, which may be one or more of silicon, germanium, silicon-germanium compounds, and silicon-carb compounds.

[0116] According to an exemplary embodiment, this embodiment is a further explanation of step S200 above, and the method in this embodiment includes the following.

[0117] like Figure 10 As shown, a plurality of active pillars 20 are formed on the substrate 10. The plurality of active pillars 20 are arranged in an array on the substrate 10, that is, the plurality of active pillars 20 can be arranged in a multi-row, multi-column manner.

[0118] In some embodiments, the active pillars 20 arranged in an array on the substrate 10 can be formed using the following methods:

[0119] Reference Figure 2 , Figure 3 As shown, a plurality of bit line isolation structures 30 are formed within the substrate 10. These bit line isolation structures 30 are spaced apart along the second direction Y, and strip-shaped bodies 40 are formed on the substrate 10 between adjacent bit line isolation structures 30. (Referring to...) Figure 2 As shown in the figure, taking the orientation shown in the figure as an example, the second direction Y is the extension direction perpendicular to the front side of the base 10.

[0120] In some embodiments, refer to Figure 3 As shown, during the process of forming the bit line isolation structure 30 on the substrate 10, a mask layer with a mask pattern can first be formed on the substrate 10. Taking the direction from the top surface of the substrate 10 to the bottom surface of the substrate 10 as the extension direction, along the extension direction, a portion of the substrate 10 is removed according to the mask pattern to form a structure along the second direction Y (refer to...). Figure 2 Multiple bit line grooves 50 are spaced apart in the direction shown.

[0121] Then, a bit line isolation structure 30 can be formed within the bit line trench 50 using atomic layer deposition, chemical vapor deposition, or physical vapor deposition processes. The material of the bit line isolation structure 30 can be, but is not limited to, silicon oxide or silicon nitride. In some embodiments, the bit line isolation structure 30 can also be a silicon oxide-silicon nitride-silicon oxide (ONO) structure, but is not limited thereto. The bit line isolation structure 30 formed within the substrate 10 can achieve insulation between adjacent bit lines subsequently formed within the substrate 10, ensuring the performance and yield of the semiconductor structure.

[0122] like Figure 2 and Figure 3 As shown, after the strip 40 is formed, the strip 40 is processed to form a silicon pillar structure 41.

[0123] Processing the strip 40 includes processing it through an ion implantation process. For example, firstly, the ion implantation energy and the type of implanted dopant ions can be controlled to form a first portion 411 at the bottom of the silicon pillar structure 41; then, the ion implantation energy and the type of implanted dopant ions can be controlled to form a second portion 412 in the middle of the silicon pillar structure 41; finally, the ion implantation energy and the type of implanted dopant ions can be controlled to form a third portion 413 at the top of the silicon pillar structure 41. The type of dopant ions in the first portion 411 can be the same as the type of dopant ions in the third portion 413; for example, the dopant ions can include N-type ions. The type of dopant ions in the second portion 412 is different from the type of dopant ions in the drain region; for example, the dopant ions can include P-type ions.

[0124] It should be noted that the first part 411 can be used as one of the source region or drain region of the active pillar 20 formed subsequently, the second part 412 can be used as the channel region of the active pillar 20 formed subsequently, and the third part 413 can be used as the other of the source region or drain region of the active pillar 20 formed subsequently. For example, if the first part 411 is used as the source region, then the third part 413 is used as the drain region accordingly.

[0125] like Figure 6As shown, after forming the silicon pillar structure 41, a plurality of word line isolation structures 60 are formed within the substrate 10. The plurality of word line isolation structures 60 are spaced apart along a third direction Z. (Refer to...) Figure 6 As shown in the figure, taking the orientation shown as an example, the third direction Z is an extension direction parallel to the front side of the base 10. The second direction Y and the third direction Z intersect on the same horizontal plane. The second direction Y can be set perpendicular to the third direction Z, or the second direction Y can be set to intersect the third direction Z at a predetermined angle.

[0126] In some embodiments, during the formation of the word line isolation structure 60 on the substrate 10, a mask layer with a mask pattern can first be formed on the top surface of the substrate 10. Using the direction from the top surface to the bottom surface of the substrate 10 as the extending direction, a portion of the substrate 10 is etched away according to the mask pattern along the extending direction to form a plurality of word line trenches 70 spaced Z-spaced along a third direction. The depth of the word line trenches 70 is less than the depth of the bit line trenches 50.

[0127] Then, a first dielectric layer 80 can be formed on the sidewall of the word line trench 70 by atomic layer deposition, chemical vapor deposition or physical vapor deposition.

[0128] During the formation of the first dielectric layer 80, reference Figure 4 and Figure 5 As shown, in one embodiment, a first initial dielectric layer 81 can be formed on the sidewalls and bottom of the word line trench 70, and on the top surface of the silicon pillar structure 41 and the bit line isolation structure 30 using an atomic layer deposition process. Then, the first initial dielectric layer 81 at the bottom of the word line trench 70 is etched away in the opposite direction to the first direction X, leaving the remaining first initial dielectric layer 81 on the sidewalls of the word line trench 70, the top surface of the silicon pillar structure 41, and the top surface of the bit line isolation structure 30 to form a first transition dielectric layer 82. Forming the first transition dielectric layer 82 protects the sidewalls and top surface of the silicon pillar structure 41, preventing damage to the silicon pillar 42 from other structures subsequently formed within the substrate 10. The material of the first transition dielectric layer 82 may include silicon nitride, silicon dioxide, or silicon oxynitride.

[0129] After the first transition medium layer 82 is formed, a first groove 90 is formed between the first transition medium layers 82 on both sides of the second direction Y, in the second direction Y.

[0130] like Figure 6 As shown, a word line isolation structure 60 is formed in the first trench 90. In some embodiments, before forming the word line isolation structure 60 in the first trench 90, a bit line 100 is first formed in the first trench 90. There are multiple bit lines 100, and the multiple bit lines 100 are spaced apart along the second direction Y.

[0131] In one embodiment, cobalt (Co) or nickel-platinum alloy (NiPt) can be implanted into the bottom of the first trench 90 using an ion implantation process. The cobalt (Co) or nickel-platinum alloy (NiPt) reacts with the substrate 10 to form cobalt silicide (CoSi) or platinum-nickel silicide (PtNiSi). Then, after annealing, the cobalt silicide (CoSi) or platinum-nickel silicide (PtNiSi) diffuses towards the bottom surface of the active pillar 20 within the substrate 10, thereby forming a bit line 100. The bit line 100 can be connected to the first segment of a plurality of active pillars 20 subsequently formed along a third direction Z and aligned on the same straight line.

[0132] In this embodiment, the bit line formation method is simple and easy to control and operate. It should be noted that the bit line can be connected to the drain of the subsequently formed active pillar 20, the gate of the transistor is connected to the word line, and the source is connected to the capacitor structure. The voltage signal on the word line can control the transistor to turn on or off, thereby reading the data information stored in the capacitor structure through the bit line, or writing the data information into the capacitor structure for storage through the bit line.

[0133] Then, refer to Figure 6 As shown, an initial word line isolation structure is formed within a first trench 90. The first trench 90 is filled with a filler material using atomic layer deposition, chemical vapor deposition, or physical vapor deposition to form the initial word line isolation structure. The top surface of the initial word line isolation structure is flush with the top surface of the first transition dielectric layer 82. Suitable filler materials include insulating materials. In some embodiments, the filler material includes nitrides, oxides, high-k dielectric materials, or other suitable insulating materials.

[0134] After the initial word line isolation structure is formed, a portion of the first transition dielectric layer 82 and a portion of the initial word line isolation structure are removed by chemical mechanical polishing (CMP), exposing the top surface of the silicon pillar 42. The retained first transition dielectric layer 82 forms the first dielectric layer 80, and the retained initial word line isolation structure forms the word line isolation structure 60. CMP flattens the surfaces of the first dielectric layer 80, the word line isolation structure 60, and the silicon pillar, reducing defect density and improving the yield of the semiconductor structure.

[0135] After forming the word line isolation structure 60, silicon pillar structures 41 between adjacent word line isolation structures 60 and adjacent bit line isolation structures 30 on the substrate 10 form silicon pillars 42. It should be noted that the first portion 411 of the silicon pillar structure 41 forms the lower half of the silicon pillar 42, the second portion 412 forms the middle section of the silicon pillar 42, and the third portion 413 forms the upper half of the silicon pillar 42. The word line isolation structure 60 is used to achieve insulation between adjacent word lines subsequently formed within the substrate 10, ensuring the performance and yield of the semiconductor structure.

[0136] For example, such as Figure 8 As shown, after the word line isolation structure 60 is formed in the substrate 10, in order to facilitate the subsequent pre-processing of the silicon pillars to form the active pillars 20 and improve the formation accuracy of the gate oxide layer and other structures formed later, support structures 110 are first formed on both sides of the word line isolation structure 60.

[0137] Among them, reference Figure 7 As shown, in some embodiments, the first dielectric layer 80 and the bit line isolation structure 30 can be etched to remove a portion of the first dielectric layer 80 and the bit line isolation structure 30, exposing a portion of the word line isolation structure 60 and the silicon pillar 42. Along the second direction Y, a second trench 120 is formed between the top surface of the retained bit line isolation structure 30 and the exposed word line isolation structure 60 and silicon pillar 42.

[0138] Subsequently, an initial support structure can be formed within the second trench 120 using atomic layer deposition, chemical vapor deposition, or physical vapor deposition. In some embodiments, the initial support structure can be deposited within the second trench 120 using atomic layer deposition, filling the second trench 120 completely. A portion of the initial support structure is then removed by etching, retaining the initial support structures located on both sides of the word line isolation structure 60. The retained initial support structures form support structures 110. Support structures 110 are spaced apart along a third direction. It should be noted that the material of the support structure 110 includes, but is not limited to, silicon nitride.

[0139] In this embodiment, the support structure 110 is formed by atomic layer deposition, which can improve the film density of the support structure 110. This is used to prevent the third segment 203 of the active pillar 20 from tilting during the subsequent word line formation process, thereby ensuring the formation accuracy of the subsequently formed first gate oxide layer 140 and second gate oxide layer 160, and thus improving the performance and yield of the semiconductor structure.

[0140] Reference Figure 10As shown, a portion of the silicon pillar 42 undergoes a pre-processing step to form an active pillar 20. The pre-processing step includes an oxidation process. In one example, the middle section of the silicon pillar 42 is oxidized before etching or cleaning, thereby forming the active pillar 20. It should be understood that the middle section of the silicon pillar 42 in this embodiment is the second part 412 of the silicon pillar structure 41 in the above embodiment.

[0141] In some embodiments, such as Figure 9 As shown, before performing an oxidation process on the second portion 412 of the silicon pillar 42, a portion of the first dielectric layer 80 and a portion of the bit line isolation structure 30 are etched away in the opposite direction to the first direction X. The etching endpoint of the first dielectric layer 80 and the bit line isolation structure 30 is located at the boundary between the lower half and the middle section of the silicon pillar 42, that is, the entire middle section of the silicon pillar 42 is exposed. In some embodiments, the etching depth of the first dielectric layer 80 and the bit line isolation structure 30 may also be located at two-thirds of the height of the subsequently formed active pillar 20, that is, the height of the retained first dielectric layer 80 may be one-third of the height of the active pillar 20.

[0142] After the etching of a portion of the first dielectric layer 80 and a portion of the bit line isolation structure 30 is completed, an oxidation process is performed on the exposed middle section of the silicon pillar 42 to remove a portion of the middle section of the silicon pillar 42 along the radial direction of the silicon pillar 42. It should be noted that in some embodiments, the oxidation process includes thermal oxidation or steam oxidation. In the oxidation process, the middle section of the silicon pillar 42 is exposed to the outside environment. Through thermal oxidation or steam oxidation, an oxide layer, such as silicon oxide, is formed on the surface of the middle section. This oxide layer can then be removed by etching or cleaning processes, thereby removing a portion of the middle section of the silicon pillar 42.

[0143] After the oxidation process is completed, the lower half of the silicon pillar 42 forms the first segment 201 of the active pillar 20, which can form the drain or source of the active pillar 20; the middle segment of the retained silicon pillar 42 forms the second segment 202 of the active pillar 20, which can form the channel region of the active pillar 20; and the upper half of the silicon pillar 42 forms the third segment 203 of the active pillar 20, which can form the source or drain of the active pillar 20. Therefore, taking a plane perpendicular to the first direction X as a cross-section, the cross-section of the second segment 202 is smaller than the cross-sections of the first segment 201 and the third segment 203. In one example, the first segment 201 of the active pillar 20 forms the drain, and the third segment 203 of the active pillar 20 forms the source.

[0144] According to an exemplary embodiment, this embodiment is a further description of step S300 above, and the method in this embodiment includes the following.

[0145] like Figure 10 and Figure 11 As shown, a first gate oxide layer 140 is formed on the sidewall of the second segment 202, the top surface of the first segment 201, and the bottom surface of the third segment 203 of the active column 20.

[0146] After forming multiple active pillars 20 arranged in an array through the above steps, a third groove 130 is formed between the sidewall of the second segment 202 of the active pillar 20 and the word line isolation structure 60 along the extension direction of the first direction X.

[0147] Then, an atomic layer deposition (ALD) process is used to form a first gate oxide layer 140 on the sidewall of the third trench 130. ASD processes are characterized by slow deposition rates, high film density, and good step coverage. The first gate oxide layer 140 formed using ASD can effectively isolate and protect the second segment of the active pillar, i.e., the gate, even with a relatively thin thickness, avoiding occupying a large space and facilitating the subsequent filling or formation of other structural layers. The material of the first gate oxide layer 140 can include, but is not limited to, silicon dioxide, silicon monoxide, hafnium oxide, or titanium oxide.

[0148] According to an exemplary embodiment, this embodiment is a further description of step S400 above, and the method in this embodiment includes the following.

[0149] A second gate oxide layer 160 is formed on the first gate oxide layer 140. The length of the second gate oxide layer 160 is less than the length of the first gate oxide layer 140 along the first direction X, and the thickness of the second gate oxide layer 160 is greater than the thickness of the first gate oxide layer 140.

[0150] The second gate oxide layer 160 can be formed using the following method:

[0151] Reference Figure 11 and Figure 12 As shown, after the first gate oxide layer 140 is formed, the first gate oxide layer 140 located in the third trench 130 forms a fourth trench 150.

[0152] A first initial word line (not shown in the figure) is formed in the fourth trench 150 using atomic layer deposition, physical vapor deposition, or chemical vapor deposition, and the first initial word line fills the fourth trench 150.

[0153] Then, refer to Figure 12As shown, a portion of the first initial word line is etched away, wherein the etch endpoint of the first initial word line along the extension direction of the first direction X can be located at a position between one-third and two-thirds of the height of the second segment 202. In one embodiment, the etch endpoint of the first initial word line is located at a position at half the height of the second segment 202. Thus, the retained first initial word line forms the first word line 170. The material of the first word line 170 includes, but is not limited to, tungsten or polysilicon. A fifth trench 180 is formed between the top surface of the first word line 170 and the exposed first gate oxide layer 140.

[0154] Then, an atomic layer deposition (ALD) process is used to form a second initial gate oxide layer on the fifth trench 180. The second initial gate oxide layer located on the top surface of the first word line 170 is etched away, while the second initial gate oxide layer located on the sidewalls and top surface of the fifth trench 180 is retained. The retained second initial gate oxide layer forms the second gate oxide layer 160. The second gate oxide layer 160 formed by the ALD process can effectively isolate and protect the second segment of the active pillar, i.e., the gate, with a relatively thin thickness, avoiding occupying a large space and facilitating the subsequent filling or formation of other structural layers.

[0155] The material of the second gate oxide layer 160 may include, but is not limited to, silicon dioxide, silicon monoxide, hafnium oxide, or titanium oxide. The material of the second gate oxide layer 160 may be the same as that of the first gate oxide layer 140, or the material of the second gate oxide layer 160 may be different from that of the first gate oxide layer 140.

[0156] Because a first word line 170 of a predetermined thickness is formed in the fourth trench 150 before the second gate oxide layer 160 is formed, the formation length of the second gate oxide layer 160 in the first direction X is less than the length of the first gate oxide layer 140. At the same time, during the formation of the second gate oxide layer 160, the formation thickness of the second gate oxide layer 160 is controlled to be greater than the thickness of the first gate oxide layer 140.

[0157] In semiconductor structures, gate-induced drain (GIDL) transistors suffer from a problem. The reason for this GIDL is that the thin gate oxide layer reduces its charge storage capacity. When the GAA transistor is in a static state, electrons generated at the gate or a small number of current carriers can pass through the gate oxide layer into the drain, creating a high electric field and causing leakage current. In this embodiment, a first gate oxide layer 140 and a second gate oxide layer 160 are sequentially formed on the sidewall of the second segment 202 of the active pillar 20, resulting in different thicknesses of the gate oxide layer at different locations on the second segment 202. This increases the charge storage capacity of the gate oxide layer, preventing electrons generated at the gate or a small number of current carriers from passing through the gate oxide layer into the source or drain of the semiconductor structure, thus reducing the GIDL and improving the performance and yield of the semiconductor structure.

[0158] Reference Figure 13 As shown, after the second gate oxide layer 160 is formed, a sixth trench 190 is formed on the sidewall of the second gate oxide layer 160 and the top surface of the first word line 170. The longitudinal section of the second gate oxide layer 160, with a plane perpendicular to the second direction Y as its longitudinal section, includes a horizontal segment along the horizontal direction and two vertical segments along the vertical direction, with the two ends of the horizontal segment connected to the top surfaces of the two vertical segments.

[0159] Then, refer to Figure 14 As shown, a second initial word line can be formed in the sixth trench 190 using atomic layer deposition, physical vapor deposition, or chemical vapor deposition. The second initial word line fills the entire sixth trench 190.

[0160] A portion of the second initial word line is etched away, wherein the etch endpoint of the second initial word line is flush with the bottom surface of the horizontal segment of the second gate oxide layer 160 located in the sixth trench 190. The retained second initial word line forms a second word line 200. The material of the second word line 200 includes, but is not limited to, tungsten or polysilicon. The first word line 170 and the second word line 200 form a word line structure 210.

[0161] The first word line 170 and the second word line 200 can be made of the same material, or they can be made of different materials. In one embodiment, the first word line 170 and the second word line 200 can be made of tungsten or polysilicon. It should be noted that the thickness of the word lines formed by materials such as tungsten or polysilicon will not affect the potential of the word lines.

[0162] In some embodiments, the gate structure of the duplex function is generally obtained by depositing word line metal layers of different materials at the gate. However, the process required to deposit metal layers of different materials is relatively complex, and an isolation layer is required between metal layers of different materials due to diffusion issues.

[0163] In this embodiment, at the second segment, i.e., the gate position, the first word line 170 and the second word line 200 can be metal layers of the same material, or both can be formed using materials such as tungsten or polycrystalline silicon. By setting gate oxide layers of different thicknesses at different positions on the second segment 202, a doubly functional effect is achieved, which not only simplifies the manufacturing process but also makes it easier to control and implement. Specifically, the thickness of the gate oxide layer in the portion of the second segment 202 near the third segment 203 is greater than the thickness of the gate oxide layer in the portion of the second segment 202 near the first segment 201. Therefore, when the transistor formed by the semiconductor structure of this embodiment, such as a GAA transistor, is used, the increased thickness of the gate oxide layer near the source increases the turn-on voltage VT applied at that terminal to enable transistor conduction, which in turn raises the potential of the second word line 200, making the potential of the second word line 200 higher than that of the first word line 170.

[0164] Furthermore, as the turn-on voltage VT applied to the source terminal increases, the source voltage Vs at the source terminal will also increase. The turn-off current (Ioff) and the source voltage Vs are related as shown in the following formula:

[0165] I off∝e -(Vs*ε / kt)

[0166] Where ε / kt is a constant, approximately 0.0256. Therefore, when the source voltage Vs at the source terminal increases, the turn-off current (Ioff) decreases. Since the turn-off current and the source voltage Vs satisfy an exponential relationship of e, when the thickness of the gate oxide layer at the source terminal of the transistor increases, the turn-off current decreases exponentially. This facilitates the control of the turn-off current of the semiconductor structure, thereby reducing the gate-induced drain leakage current and inter-band tunneling of the semiconductor structure, and improving the performance and yield of the semiconductor structure.

[0167] Reference Figure 15As shown, in some embodiments, the thickness of the second gate oxide layer 160 is 1 to 2 times the thickness of the first gate oxide layer 140. Therefore, in this embodiment, the thickness of the gate oxide layer of the second segment 202 near the third segment 203 is 2 to 3 times the thickness of the gate oxide layer of the second segment 202 near the first segment 201. In one specific embodiment, the thickness of the second gate oxide layer 160 is 1.5 times the thickness of the first gate oxide layer 140. By setting the above thickness ratio, the turn-off current of the semiconductor structure can be reduced by 6 orders of magnitude, and the induced drain leakage current and inter-band tunneling of the semiconductor structure are also reduced, thereby improving the performance and yield of the semiconductor structure.

[0168] like Figures 16 to 18 As shown, in some other embodiments, the second gate oxide layer 160 can be formed using the following methods:

[0169] After the first gate oxide layer 140 is formed, the first gate oxide layer 140 located in the third trench 130 forms a fourth trench 150.

[0170] Reference Figure 16 As shown, a sacrificial layer 220 is formed in the fourth trench 150 using atomic layer deposition, physical vapor deposition, or chemical vapor deposition processes, and the sacrificial layer 220 completely fills the fourth trench 150. The material of the sacrificial layer 220 includes, but is not limited to, polycrystalline silicon.

[0171] In the opposite direction to the first direction X, a portion of the sacrificial layer 220 is removed by etching, wherein the etching endpoint of the sacrificial layer 220 may be located at one-third to two-thirds of the height of the second segment 202. In one embodiment, the etching endpoint of the sacrificial layer 220 is located at half the height of the second segment 202. A fifth trench 180 is formed between the retained sacrificial layer 220 and the sidewall of the first gate oxide layer 140.

[0172] Reference Figure 17 As shown, a second gate oxide layer 160 is formed within the fifth trench 180 and on the sidewall of the first gate oxide layer 140. In some embodiments, the second gate oxide layer 160 can be formed by atomic layer deposition. The second gate oxide layer 160 formed by atomic layer deposition can effectively isolate and protect the second segment of the active pillar, i.e., the gate, with a relatively thin thickness, avoiding occupying a large space and facilitating the subsequent filling or formation of other structural layers.

[0173] The remaining sacrificial layer 220 is etched away in the opposite direction of the first direction X. After all the sacrificial layer 220 is removed, a seventh trench 230 is formed between the sidewall of the second gate oxide layer 160 and the sidewall of the first gate oxide layer 140 at the location of the removed sacrificial layer 220.

[0174] An initial word line structure is deposited in the seventh trench 230 using atomic layer deposition, physical vapor deposition, or chemical vapor deposition. A portion of the initial word line structure is then etched away, leaving the retained initial word line structure to form word line structure 210. The material of word line structure 210 includes, but is not limited to, tungsten or polysilicon. It should be noted that the etching endpoint of the initial word line structure in this embodiment is the same as the etching endpoint of the word line structure formed in the embodiments for forming the first word line 170 and the second word line 200 described above.

[0175] In this embodiment, the character line structure 210 is deposited in one step, which is simple and easy to control.

[0176] like Figure 15 and Figure 18 As shown, in one embodiment, after the word line structure 210 is formed, a second dielectric layer 240 can be formed on the top surface of the word line structure 210 using atomic layer deposition, physical vapor deposition, or chemical vapor deposition. Then, the top surface of the second dielectric layer 240 is processed by chemical mechanical polishing, so that the top surface of the retained second dielectric layer 240 is flush with the top surface of the active pillar 20. Forming the second dielectric layer 240 on the word line structure 210 facilitates the subsequent formation of other semiconductor structures on the substrate 10. The material of the second dielectric layer 240 includes, but is not limited to, silicon nitride, silicon dioxide, or silicon oxynitride.

[0177] like Figure 15 As shown, an exemplary embodiment of this disclosure provides a semiconductor structure, wherein the semiconductor structure includes: a substrate 10, an active pillar 20, a first gate oxide layer 140, and a second gate oxide layer 160.

[0178] For example, there are multiple active pillars 20, and the multiple active pillars 20 are arranged in an array within the substrate 10. Specifically, along the first direction X, each active pillar 20 includes a first segment 201, a second segment 202, and a third segment 203 connected in sequence. Along the second direction Y, the cross-sectional area of ​​the second segment 202 is smaller than the cross-sectional areas of the first segment 201 and the third segment 203.

[0179] The first gate oxide layer 140 is disposed on the sidewall of the second section 202, the top surface of the first section 201, and the bottom surface of the third section 203.

[0180] The second gate oxide layer 160 is disposed outside the first gate oxide layer 140 and is disposed close to the third segment 203. Along the first direction X, the length of the second gate oxide layer 160 is less than the length of the first gate oxide layer 140, and the thickness of the second gate oxide layer 160 is greater than the thickness of the first gate oxide layer 140. In some embodiments, the thickness of the second gate oxide layer 160 is 1 to 2 times the thickness of the first gate oxide layer 140.

[0181] In this embodiment, by forming a first gate oxide layer on the sidewall of the second segment of the active pillar and a second gate oxide layer on the first gate oxide layer, the gate-induced drain leakage current and inter-band tunneling are effectively reduced. On the other hand, by making the length of the second gate oxide layer shorter than the length of the first gate oxide layer and the thickness of the second gate oxide layer greater than the thickness of the first gate oxide layer, and by placing the second gate oxide layer close to the third segment, gate oxide layers of different thicknesses are formed at different positions in the second segment, which is beneficial for controlling the turn-off current of the semiconductor structure, thereby effectively improving the performance and yield of the semiconductor structure.

[0182] like Figure 15 As shown, in one embodiment, the semiconductor structure further includes a plurality of bit line isolation structures 30 and a plurality of word line isolation structures 60 disposed within the substrate 10.

[0183] The multiple bit line isolation structures 30 are spaced apart along the second direction Y. The bit line isolation structures 30 are used to achieve insulation between adjacent bit lines 100 subsequently formed in the substrate 10.

[0184] Multiple word line isolation structures 60 are spaced apart along the third direction Z. The word line isolation structures 60 are used to achieve insulation between adjacent word line structures 210 subsequently formed in the substrate 10.

[0185] It should be noted that support structures 110 are provided on both sides of the word line isolation structure 60. The support structures 110 facilitate the subsequent formation of the active pillar 20 and improve the formation accuracy of the first gate oxide layer 140 and the second gate oxide layer 160 on the second segment 202 of the active pillar 20.

[0186] like Figure 15 As shown, in some embodiments, the semiconductor structure further includes a plurality of bit lines 100 disposed within the substrate 10. The plurality of bit lines 100 are spaced apart along a second direction and are located below the active pillars 20. In one embodiment, cobalt (Co) or nickel-platinum alloy (NiPt) is implanted into the bottom of the active pillars 20 via an ion implantation process. The cobalt (Co) or nickel-platinum alloy (NiPt) reacts with the substrate 10 to form cobalt silicide (CoSi) or platinum-nickel silicide (PtNiSi). Then, after annealing, the cobalt silicide (CoSi) or platinum-nickel silicide (PtNiSi) diffuses towards the bottom surface of the active pillars 20 within the substrate 10, thereby forming a bit line 100. The bit line 100 is connected to a first segment 201 of the plurality of active pillars 20 along a third direction Z and aligned with the first segment. A first dielectric layer 80 is provided between the bit line 100 and the word line isolation structure 60.

[0187] like Figure 15As shown, in some embodiments, the semiconductor structure further includes a plurality of word line structures 210. The plurality of word line structures 210 are spaced apart along a third direction Z.

[0188] The word line structure 210 is arranged around the second segment 202 of the active pillar 20, thereby forming a GAA transistor structure. The word line structure 210 includes a first word line 170 and a second word line 200 connected in sequence. The bottom surface of the first word line 170 is close to the first segment 201, and the top surface of the second word line 200 is close to the third segment 203. Taking a plane perpendicular to the second direction Y as the longitudinal section, the area of ​​the longitudinal section of the first word line 170 is larger than the area of ​​the longitudinal section of the second word line 200.

[0189] It should be noted that a second dielectric layer 240 is provided on the top surface of the word line structure 210 to facilitate the subsequent formation of other structures of the semiconductor structure on the substrate 10.

[0190] In the description of this disclosure, it should be noted that the terms "center", "upper", "lower", "left", "right", "vertical", "horizontal", "inner", "outer", etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are only for the convenience of describing this disclosure and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this disclosure.

[0191] It is understood that the terms "first," "second," etc., as used in this disclosure may be used to describe various structures, but these structures are not limited by these terms. These terms are only used to distinguish one structure from another.

[0192] In one or more accompanying drawings, the same elements are represented by similar reference numerals. For clarity, many parts in the drawings are not drawn to scale. Furthermore, certain well-known parts may not be shown. For simplicity, a structure obtained after several steps may be depicted in a single drawing. Many specific details of this disclosure, such as the structure, materials, dimensions, processing methods, and techniques of the devices, are described below to provide a clearer understanding of the disclosure. However, as those skilled in the art will understand, this disclosure may be implemented without adhering to these specific details.

[0193] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of this disclosure, and are not intended to limit them. Although this disclosure has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features therein. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of this disclosure.

Claims

1. A method for fabricating a semiconductor structure, characterized in that, The method for fabricating the semiconductor structure includes: Provide a base; Multiple active pillars are formed in an array on the substrate, and the active pillars include a first segment, a second segment and a third segment arranged sequentially along the vertical direction of the substrate surface; A support structure is formed at the corresponding position of the third segment of the active column; A gate structure is formed in the second section of the active pillar; It also includes: forming a word line isolation structure on the substrate, the word line isolation structure extending along a second direction and spaced apart along a third direction, the second direction and the third direction intersecting at a predetermined angle; A silicon pillar structure is formed between adjacent word line isolation structures, the silicon pillar structure being used to form the active pillar; The support structure is formed on both sides of the word line isolation structure, and the support structure is located between the silicon pillar structure and the word line isolation structure.

2. The method for fabricating a semiconductor structure according to claim 1, characterized in that, The method for fabricating the semiconductor structure further includes: A limiting structure is formed in the first segment of the active column.

3. The method for fabricating a semiconductor structure according to claim 2, characterized in that, The method of forming a limiting structure in the first segment of the active column includes: A first dielectric layer is formed on the sidewall of the active column; The limiting structure is formed by etching the first dielectric layer.

4. The method for fabricating a semiconductor structure according to claim 1, characterized in that, The formation of a word line isolation structure between the active pillars includes: A first dielectric layer is formed on the sidewall of the active column; The word line isolation structure is formed outside the first dielectric layer.

5. The method for fabricating a semiconductor structure according to claim 4, characterized in that, The formation of the support structure between the word line isolation structure and the active post includes: The first dielectric layer is etched to expose the third segment of the active pillar, and the support structure is formed between the third segment of the active pillar and the word line isolation structure.

6. A method for fabricating a semiconductor structure, characterized in that, The method for fabricating the semiconductor structure includes: Provide a base; Multiple active pillars are formed in an array on the substrate. Along a first direction, the active pillars include a first segment, a second segment, and a third segment connected in sequence. The first direction is perpendicular to the surface of the substrate. A gate oxide layer and a gate electrode are formed in the second section of the active pillar; A support structure is formed at the corresponding position of the third segment of the active column; It also includes: forming a plurality of word line isolation structures within the substrate, the plurality of word line isolation structures being spaced apart along a third direction, and forming a silicon pillar structure between two adjacent word line isolation structures, the silicon pillar structure being used to form the active pillar; Along the second direction, the support structure is formed on both sides of the word line isolation structure, the support structure being located between the silicon pillar structure and the word line isolation structure, wherein the second direction intersects the third direction at a predetermined angle.

7. The method for fabricating a semiconductor structure according to claim 6, characterized in that, The support structure is formed on both sides of the word line isolation structure, including: A second trench is formed between the word line isolation structure and the silicon pillar, wherein the silicon pillar is formed based on the silicon pillar structure; An initial support structure is formed within the second trench; The initial support structure is formed by removing a portion of it and retaining the initial support structures located on both sides of the word line isolation structure.

8. The method for fabricating a semiconductor structure according to claim 7, characterized in that, The method further includes forming multiple word line isolation structures within the substrate, and further includes: A plurality of word line grooves are formed on the substrate at intervals along the third direction; A first dielectric layer is formed on the sidewall of the character line groove, and the first dielectric layer on both sidewalls of the character line groove forms a first groove; The word line isolation structure is formed within the first trench.

9. The method for fabricating a semiconductor structure according to claim 8, characterized in that, The method for fabricating the semiconductor structure further includes: A plurality of bit line trenches are formed on the substrate at intervals along the second direction; A bit line isolation structure is formed in the bit line trench.

10. The method for fabricating a semiconductor structure according to claim 9, characterized in that, The first dielectric layer is formed on the sidewall of the character line groove, comprising: A first initial dielectric layer is formed on the sidewalls and bottom of the word line trench, as well as on the top surface of the silicon pillar structure and the bit line isolation structure; Along the direction from the top surface of the substrate to the bottom surface of the substrate, the first initial dielectric layer at the bottom of the word line trench is removed, and the remaining first initial dielectric layer located on the sidewall of the word line trench, the top surface of the silicon pillar structure and the top surface of the bit line isolation structure forms a first transition dielectric layer. The first groove is formed between the first transition medium layers on both sides of the word line groove; An initial word line isolation structure is formed in the first trench, and the top surface of the initial word line isolation structure is flush with the top surface of the first transition dielectric layer. A portion of the first transition dielectric layer is removed to expose the top surface of the silicon pillar, and the remaining first transition dielectric layer forms the first dielectric layer.

11. The method for fabricating a semiconductor structure according to claim 9, characterized in that, The silicon pillar is formed based on the silicon pillar structure, including: The silicon pillar is formed by the silicon pillar structure between adjacent word line isolation structures and adjacent bit line isolation structures on the substrate.

12. A semiconductor structure, characterized in that, include: Base; Multiple active pillars are arranged in an array within the substrate. Along a first direction, each active pillar includes a first segment, a second segment, and a third segment. The first direction is perpendicular to the surface of the substrate. A support structure is provided in the third segment of the active column; A gate structure is disposed in the second segment of the active pillar; It also includes: multiple word line isolation structures, the multiple word line isolation structures being spaced apart along a third direction, the word line isolation structures being disposed between the active pillars; Along the second direction, the support structure is disposed on both sides of the word line isolation structure, and the support structure is located between the active column and the word line isolation structure, wherein the second direction intersects the third direction at a predetermined angle.

13. The semiconductor structure according to claim 12, characterized in that, The semiconductor structure also includes: A limiting structure is provided in the first segment of the active column.

14. The semiconductor structure according to claim 13, characterized in that, The height of the limiting structure is one-third of the height of the active column.

15. The semiconductor structure according to claim 12, characterized in that, The word line isolation structure is flush with the top surface of the support structure.

Citation Information

Patent Citations

  • Semiconductor structure and preparation method thereof

    CN113611671A

  • Semiconductor devices having buried metal silicide layers and methods of fabricating the same

    US20140175555A1