Self-coated perovskite absorbing layer containing 2D composite functional material and inverted structure solar cell
By coating perovskite crystals with 2D BP-GO NSs, the problems of grain boundary defects and interface charge recombination in perovskite solar cells were solved, achieving efficient separation and directional transport of photogenerated charges, thus improving the conversion efficiency and stability of the cells.
Patent Information
- Application Number
- CN202310797972.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-03
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-07-03
AI Technical Summary
Traditional perovskite solar cells suffer from problems such as high grain boundary and surface ion defects, low photogenerated carrier collection efficiency, and insufficient driving force for interface charge separation, resulting in severe charge recombination loss and affecting conversion efficiency and stability.
3D perovskite crystal material is coated with 2D black phosphorus-graphene oxide composite nanosheets (BP-GO NSs) to form a self-coated perovskite absorption layer. By controlling the grain size and spin coating process, the built-in electric field and interface band alignment are enhanced, which promotes the separation and directional transport of photogenerated charges.
It significantly improves the photovoltaic output parameters of solar cells, such as open-circuit voltage, fill factor and stability, reduces charge recombination loss, and improves cell efficiency and environmental stability.
Smart Images

Figure CN116669446B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of semiconductor functional materials technology, and relates to upright perovskite solar cells, specifically to a method for preparing an upright perovskite absorber layer containing a 2D composite functional material. Background Technology
[0002] Solar photovoltaic (PV) power generation technology is one of the effective ways to ensure the sustainable development of renewable energy in the international community, and it is of great significance for solving problems such as the energy crisis and environmental pollution. Developing high-efficiency, high-stability, and low-cost solar cell technology is the only way to promote the vigorous development of the PV power generation industry. Among many PV power generation technologies, nip-type perovskite solar cells (PSCs) have become a research hotspot in the PV field due to their advantages such as high conversion efficiency, rapid development, simple fabrication process, low processing energy consumption, and low production cost.
[0003] It is reported that the i-type perovskite absorber layer, located between the n-type electron transport layer (ETL) and the p-type hole transport layer (HTL), is a core component of the photoelectric cell (PSC) and crucial for achieving high-efficiency photoelectric conversion. However, polycrystalline perovskite materials prepared using conventional processes currently possess high densities of ionic defects or dangling bonds at their grain boundaries and surfaces. These act as deep-level traps, leading to severe defect-assisted nonradiative recombination, thereby reducing the photovoltaic output performance of the cell. Simultaneously, due to insufficient charge separation driving force within the bulk perovskite material and at its interfaces, randomly separated and transported photogenerated carriers in the absorber layer cannot be rapidly collected by adjacent charge transport layers, further exacerbating defect-assisted charge recombination in the PSC. Furthermore, in nip-type upright PSCs, the extraction and collection efficiency of photogenerated holes at the top interface of the perovskite is far lower than that of photogenerated electrons at the bottom interface. This not only causes severe interfacial carrier accumulation and recombination losses but also accelerates the decomposition of the perovskite material, thereby reducing the photovoltaic output characteristics and stability of the cell. Therefore, synergistically reducing the trap-assisted charge recombination loss and interface carrier recombination loss of upright PSC is an important means to overcome the bottleneck of battery conversion efficiency and stability. Simultaneously improving the quality of the perovskite absorber layer (including crystal quality and interface quality) and charge transport dynamics is the first priority to solve the above recombination loss problem.
[0004] Organic-inorganic metal halide perovskite materials possess the potential to fundamentally transform optoelectronics due to their unique self-doping properties, bipolar charge transfer characteristics, and excellent photoelectric properties. In recent years, researchers have discovered that by using organic small-molecule additives with abundant functional groups to passivate perovskite defects, the perovskite surface energy can be completely transformed from n-type (p-type) to p-type (n-type). This creates an additional built-in electric field in the absorption layer, promoting and enhancing the efficient separation and directional transport of photogenerated electrons and holes, effectively suppressing defect-assisted charge recombination. Furthermore, the enhanced built-in electric field induces band alignment between the perovskite and adjacent charge transport layers, significantly accelerating the selective extraction and collection of interface charges, effectively suppressing interface charge accumulation and recombination losses. Ultimately, this significantly improves the efficiency of the photoelectric converter (PSC) and various photovoltaic output parameters, particularly the open-circuit voltage (Voc) and fill factor (FF).
[0005] Although this technology shows great potential in passivating perovskite-related defects, altering the electronic properties of the absorber layer (including carrier type and concentration), regulating the energy level barrier structure, reducing charge recombination losses, and improving photovoltaic output performance, most small organic molecules readily escape from the perovskite crystal structure, leading to a decline in the photovoltaic properties and stability of PSCs. Therefore, considering the crystallization kinetics, surface energy, band theory, and the synergistic mechanism of space charge transport and recombination behavior of perovskite materials, it is crucial to explore an ideal electronic passivation material as an additive that combines excellent charge mobility, tunable band gap, high conductivity, good chemical / humidity / thermal stability, excellent flexibility, easy processing, and low cost. Furthermore, developing innovative technical solutions that can both stabilize perovskite crystal quality and enhance carrier dynamics is of great significance for promoting the commercialization of high-efficiency, high-stability PSCs. Summary of the Invention
[0006] This invention addresses the key issues hindering the improvement of PSC efficiency and stability in current polycrystalline perovskite material systems, such as trap-assisted charge recombination loss and interface carrier recombination loss. It proposes a positive-structure solar cell with a self-coated perovskite absorber layer containing two-dimensional (2D) composite functional materials and its preparation method.
[0007] The specific technical solution adopted in this invention is as follows:
[0008] The present invention proposes a self-coated perovskite absorber layer (A) containing 2D composite functional materials, which consists of 2D black phosphorus-graphene oxide composite nanosheets (BP-GO NSs) and three-dimensional (3D) perovskite crystal material (A). 3D It consists of two parts, with 2DBP-GO NSs coating each 3D perovskite grain, and its thickness controlled at 5~10 nm. A 3DThe grain size is controlled at 800~1000 nm, and its thickness is controlled at around 1 μm. A 3D The grain boundaries between grains are arranged in an orderly manner along the normal direction.
[0009] This invention also provides a positively mounted solar cell with a self-coated perovskite absorber layer containing 2D composite functional materials, comprising, from bottom to top: a transparent conductive ITO glass substrate, an electron transport layer (ETL), a self-coated perovskite absorber layer containing 2D composite functional materials, a hole transport layer (HTL), and a metal back electrode (E). M ).
[0010] The preparation method of a self-encapsulated perovskite absorber layer containing 2D composite functional materials includes the following steps:
[0011] 1) In a glove box containing 0.1 ppm oxygen and 0.1 ppm water vapor, 1.75 mmol lead iodide and 1.6 mmol ammonium methyl iodide were weighed out and dissolved in a mixed solvent containing 750 μL N,N-dimethylformamide and 250 μL dimethyl sulfoxide. After magnetic stirring at room temperature for 30 min, a perovskite precursor solution (A) was obtained. aq1 ).
[0012] 2) Weigh 0.076 mmol of formamidin hydroiodate and dissolve it in 1 mL of isopropanol. After magnetic stirring at room temperature for 30 min, a post-treatment solution of the perovskite precursor (A) is obtained. aq2 ).
[0013] 3) Weigh 0.8~1.4 mg of 2D BP-GO NSs powder and disperse it in 1 mL of the perovskite precursor post-treatment solution A prepared in step 2). aq2 After sealing the bottle opening tightly, remove it from the glove box and perform physical ultrasonic treatment. During ultrasonic treatment, the water temperature in the ultrasonic machine is controlled at 25±2 ℃, the ultrasonic frequency is set to 40 kHz, and the ultrasonic input power is controlled at 300 W. After 4 hours of ultrasonic treatment, a 2D BP-GO NSs dispersion (A) is obtained. 2D-aq2 ).
[0014] 4) In the glove box, draw 100 μL of the perovskite precursor solution A prepared in step 1). aq1 The perovskite precursor film was drop-coated onto the substrate surface, first spin-coated at a low speed of 500 rpm for 3 s, then spin-coated at a high speed of 4000 rpm for 40 s. 400 μL of chlorobenzene was added 10 s before the end of the spin-coating process. The film was then heat-annealed at 100 °C for 10 min to obtain the perovskite precursor film. After the sample cooled to room temperature, 100 μL of the 2D BP-GO NSs dispersion A prepared in step 3) was pipetted into the sample. 2D-aq2The material is drop-coated onto the surface of the perovskite precursor film, left to stand for 5 seconds, then spin-coated at a high speed of 1500~3000 rpm for 40 seconds, and then heat-annealed at 120~150 ℃ for 10~30 min to obtain a dry self-encapsulated perovskite absorber layer containing 2D composite functional material.
[0015] A method for fabricating a positively oriented solar cell containing a self-coated perovskite absorber layer made of 2D composite functional materials includes the following steps:
[0016] I. Solution preparation:
[0017] a. Solution preparation for perovskite absorber layer:
[0018] 1) In a glove box containing 0.1 ppm oxygen and 0.1 ppm water vapor, 1.75 mmol lead iodide and 1.6 mmol ammonium methyl iodide were weighed out and dissolved in a mixed solvent containing 750 μL N,N-dimethylformamide and 250 μL dimethyl sulfoxide. After magnetic stirring at room temperature for 30 min, a perovskite precursor solution (A) was obtained. aq1 ).
[0019] 2) Weigh 0.076 mmol of formamidin hydroiodate and dissolve it in 1 mL of isopropanol. After magnetic stirring at room temperature for 30 min, a post-treatment solution of the perovskite precursor (A) is obtained. aq2 ).
[0020] 3) Weigh 0.8~1.4 mg of 2D BP-GO NSs powder and disperse it in 1 mL of the perovskite precursor post-treatment solution A prepared in step 2). aq2 After sealing the bottle opening tightly, remove it from the glove box and perform physical ultrasonic treatment. During ultrasonic treatment, the water temperature in the ultrasonic machine is controlled at 25±2 ℃, the ultrasonic frequency is set to 40 kHz, and the ultrasonic input power is controlled at 300 W. After 4 hours of ultrasonic treatment, a 2D BP-GO NSs dispersion (A) is obtained. 2D-aq2 ).
[0021] b. Solution preparation for charge transport layers:
[0022] 1) A tin dioxide (SnO2) colloidal solution was mixed with deionized water at a 1:1 volume ratio, and the mixture was magnetically stirred at room temperature for 4 hours to obtain a well-dispersed SnO2 dilution solution (ETL). -aq ).
[0023] 2) 72.3 mg of 2,2',7,7'-tetra(N,N-p-methoxyaniline)-9,9'-spirodifluorene (Spiro-OMeTAD) powder, 28.5 μL of TBP solvent, and 18.5 μL of Li-TFSI / acetonitrile dispersion (0.52 g Li-TFSI dissolved in 1 mL acetonitrile) were mixed together in 1 mL of chlorobenzene. After magnetic stirring at room temperature for 30 min, Spiro-OMeTAD dispersion (HTL) was obtained. -aq ).
[0024] II. Materials and Battery Preparation:
[0025] 1) Preparation of electron transport substrate material: Under laboratory room temperature conditions, 90 μL of SnO2 dilution solution was ETL -aq The material was spin-coated at 4000 rpm for 50 s onto a pre-cleaned ITO substrate, and then annealed at 150 °C for 25 min to obtain an n-type ETL with a thickness of 40 nm. After UV ozone treatment for 30 min, it was transferred to a glove box for later use. The oxygen content and water vapor content in the glove box should be controlled at 0.1 ppm.
[0026] 2) Preparation of the self-coated perovskite absorber layer containing the 2D composite functional material: In a glove box, 100 μL of the perovskite precursor solution A prepared in step one was drawn up. aq1 The n-type ETL surface obtained in step 1) was drop-coated, first at a low speed of 500 rpm for 3 s, then at a high speed of 4000 rpm for 40 s. 400 μL of chlorobenzene was added 10 s before the end of the program, followed by heat annealing at 100℃ for 10 min to obtain the perovskite precursor film. After the sample cooled to room temperature, 100 μL of the 2D BP-GO NSs dispersion A prepared in step 1 was pipetted into the sample. 2D-aq2 The material is drop-coated onto the surface of the perovskite precursor film, left to stand for 5 seconds, then spin-coated at a high speed of 1500~3000 rpm for 40 seconds, and then heat-annealed at 120~150 ℃ for 10~30 min to obtain a dry self-encapsulated perovskite absorber layer containing 2D composite functional material.
[0027] 3) Preparation of hole transport materials: After the self-coated perovskite absorber layer containing 2D composite functional materials is cooled to room temperature, 100 μL of the Spiro-OMeTAD dispersion HTL prepared in step one is added. -aqSpin-coating the surface of the self-coated perovskite absorber layer containing 2D composite functional material obtained in step 2) and drying it at room temperature yields a p-type HTL with a thickness of 150 nm. The spin-coating speed is set at 4000 rpm and held for 50 s. The sample based on the ITO / ETL / self-coated perovskite absorber layer containing 2D composite functional material / HTL structure is removed from the glove box for later use.
[0028] 4) Fabrication of metal electrode materials: Using vacuum thermal evaporation technology, a silver or gold back electrode with a thickness of 80 nm is deposited on the sample surface obtained in step 3) based on the ITO / ETL / self-coated perovskite absorber layer / HTL structure containing 2D composite functional materials, thus completing the fabrication of the entire solar cell; wherein, the background vacuum level of the vacuum thermal evaporation chamber should be controlled at 10 -1 Below Pa, the vacuum degree reaches 10. -3 After Pa, the coating operation should be performed, and the target power should be controlled at 5~15 W / cm². 2 The evaporation rate should be controlled between 0.9 and 1.2 Å / s.
[0029] The present invention has the following advantages over the prior art:
[0030] 1. Based on Lewis acid-base theory, this invention employs 2D BP-GONSs, which possess low defect density, high conductivity, high carrier mobility, adjustable band gap, abundant surface groups, and a flexible structure, as an additive to treat the surface of perovskite precursors during the van der Waals ripening process. This is because the surface groups of 2D BP-GONSs and the P and C elements can interact with uncoordinated metal ions (Pb) in the perovskite. 2+ ), organic cations (MA) + and FA + Strong chemical bonding occurs between 2D BP-GO NSs, allowing them to serve as growth templates. This not only slows down perovskite nucleation and crystallization rates but also ensures stable adhesion at grain boundaries and surfaces, enabling the grains to grow into a high-quality self-coated absorber layer structure. Furthermore, the passivation effect of 2D BP-GO NSs on deep-level defects in perovskite stabilizes the crystal structure and improves film quality, effectively reducing charge recombination losses due to internal defects and improving flyback factor (FF) and short-circuit current density (J / L). SC Improvements in photovoltaic output parameters such as PCE.
[0031] 2. The 2D BP-GO NSs treatment technology proposed in this invention not only exhibits a significant chemical passivation effect on internal and interface defects in perovskite materials, but also demonstrates excellent electronic passivation effects. Because the 2D BP-GO NSs coated on perovskite grains possesses a high work function and rapid photoinduced electron transfer characteristics, it can induce a transformation of the self-coated perovskite system structure towards p-type semiconductor characteristics. This leads to a significant difference in the electronic properties (including carrier type and concentration) between the top and bottom materials of the absorption layer, thereby enhancing the built-in electric field, accelerating the efficient separation and directional transport of photogenerated charges, and further suppressing defect-assisted nonradiative recombination. Simultaneously, this enhancement of the built-in electric field and surface energy transformation caused by the electronic passivation of 2D BP-GO NSs can drive the interface band alignment of the self-coated perovskite system structure, effectively reducing the interface energy level barrier, improving the selective extraction and collection efficiency of interface charges, and effectively suppressing interface charge accumulation and recombination losses. Furthermore, the 2D BP-GO NSs coating the perovskite grains form a rapid channel for the extraction and transfer of photogenerated holes, further reducing charge recombination losses while balancing carrier transport dynamics at the top and bottom interfaces of the perovskite, ultimately improving the battery's Vo. OC It has the effects of FF, PCE, and stability. Therefore, 2D BP-GO NSs is considered an ideal additive that is low-cost, environmentally friendly, and stable.
[0032] 3. Compared with traditional controlled self-doping techniques and organic small molecule passivation techniques, the 2D BP-GONSs chemical and electronic passivation strategy adopted in this invention not only avoids the conflict between parasitic absorption and device series resistance caused by simple heavy doping processes, but also avoids the instability factors of most organic small molecules easily escaping from the perovskite crystal structure. Therefore, by controlling and optimizing the relevant process parameters of the technology described in this invention, effective regulation of the phase structure, crystallization kinetics, surface energy, band theory, and space charge transport and recombination behavior of the self-coated perovskite absorber layer system containing 2D composite functional materials can be achieved. Using a 1.2 mg / mL 2D BP-GO NSs / isopropanol dispersion, a spin coating speed of 2000 rpm for 40 s, and a heat annealing treatment at 140 ℃ for 20 min, a high-quality, large-grained self-coated perovskite absorber layer containing 2D BP-GO NSs was obtained on an ITO / SnO2 substrate. The perovskite grain size was approximately 800~1000 nm, the absorber layer thickness was 800~1000 nm, and the BP-GO NSs coating layer thickness was approximately 5~10 nm.
[0033] 4. By adjusting and optimizing process parameters such as spin coating speed, solution drop volume, annealing temperature and time, this invention enables the controllable construction of upright solar cells with self-coated perovskite absorber layers containing 2D composite functional materials. The photoelectric conversion efficiency is significantly improved compared to conventional devices, and the environmental stability of this type of unencapsulated cell is greatly improved, with an efficiency loss of only 20% after 500 hours of storage.
[0034] 5. The perovskite self-coating technology described in this invention is compatible with existing PSC preparation processes and features simple operation, safety, environmental friendliness, and low cost. It provides technical support for the controllable construction of high-performance polycrystalline perovskite absorber layers and the industrialization of high-efficiency and high-stability photovoltaic devices. Attached Figure Description
[0035] Figure 1 This is a schematic diagram of the upright solar cell structure with a self-coated perovskite absorber layer containing 2D composite functional materials prepared according to the present invention.
[0036] Figure 2 The images show cross-sectional SEM images and corresponding high-resolution XPS spectra of the self-coated perovskite absorber layer containing 2D composite functional material prepared in this invention and the conventional 3D perovskite absorber layer.
[0037] Figure 3 UPS spectra and KPFM images of the self-coated perovskite thin film containing 2D composite functional materials prepared in this invention and conventional 3D perovskite thin films.
[0038] Figure 4 The IV characteristic curves of upright solar cells prepared using conventional perovskite and self-encapsulated perovskite absorber layers containing 2D composite functional materials of the present invention are shown.
[0039] Figure 5 The graph shows the atmospheric efficiency degradation trend of upright solar cells prepared using conventional perovskite and self-coated perovskite absorber layers containing 2D composite functional materials of the present invention. Detailed Implementation
[0040] The technical solution of the present invention will be further described in detail below with reference to the accompanying drawings and specific embodiments.
[0041] Example 1
[0042] 1) Preparation of solutions for self-coated perovskite absorber layers containing 2D composite functional materials: 1.75 mmol of lead iodide and 1.6 mmol of methylammonium iodide were weighed and dissolved in a mixed solvent containing 750 μL of N,N-dimethylformamide and 250 μL of dimethyl sulfoxide in a glove box with an oxygen content of 0.1 ppm and a water vapor content of 0.1 ppm. After magnetic stirring at room temperature for 30 min, perovskite precursor solution A was prepared. aq1 Weigh 0.076 mmol of formamidin hydroiodate and dissolve it in 1 mL of isopropanol. After magnetic stirring at room temperature for 30 min, post-treatment solution A of the perovskite precursor is obtained. aq2 Weigh 1.2 mg of 2D BP-GONSs powder and disperse it in the 1 mL of A solution prepared above. aq2 After sealing the bottle tightly in the solution, the bottle was removed from the glove box and subjected to physical ultrasonic treatment. The water temperature in the ultrasonic machine was controlled at 25±2 ℃, the ultrasonic frequency was set to 40 kHz, and the ultrasonic input power was controlled at 300 W. After 4 h of ultrasonic treatment, a dispersion A of 2D BP-GO NSs was obtained. 2D-aq2 .
[0043] 2) Preparation of relevant solutions for the charge transport layer: Under laboratory room temperature conditions, SnO2 colloidal solution and deionized water were mixed at a volume ratio of 1:1 and magnetically stirred at room temperature for 4 h to obtain a well-dispersed SnO2 dilution ETL. -aq In a glove box, 72.3 mg Spiro-OMeTAD powder, 28.5 μL TBP solvent, and 18.5 μL Li-TFSI / acetonitrile dispersion (0.52 g Li-TFSI dissolved in 1 mL acetonitrile) were mixed together with 1 mL chlorobenzene. After magnetic stirring at room temperature for 30 min, the dispersion HTL for HTL deposition was obtained. -aq .
[0044] 3) Preparation of SnO2 substrate material for electron transport: First, a clean ITO transparent conductive glass substrate was subjected to ultraviolet ozone treatment for 30 min; then, 90 μL of ETL was drawn using a pipette at room temperature in the laboratory. -aq The solution was dropped onto the surface of the ITO substrate and spin-coated at 4000 rpm for 50 s to obtain a wet SnO2 film. After annealing at 150 °C for 25 min, an n-type ETL with a thickness of about 40 nm was obtained. After UV ozone treatment for 30 min, it was transferred to a glove box for subsequent use.
[0045] 4) Preparation of self-coated perovskite absorber layer containing 2D composite functional material and its solar cell: In a glove box, 100 μL of perovskite precursor solution A was drawn using a pipette. aq1The ITO / SnO2 substrate obtained in step 3) was drop-coated onto the surface of the substrate. First, it was spin-coated at a low speed of 500 rpm for 3 s, then at a high speed of 4000 rpm for 40 s. 400 μL of chlorobenzene was added 10 s before the end of the spin-coating process. The substrate was then heat-annealed at 100 °C for 10 min to obtain the perovskite precursor film. After the sample cooled to room temperature, 100 μL of the 2D BP-GO NSs dispersion A was pipetted onto the substrate. 2D-aq2 The sample was drop-coated onto the surface of the perovskite precursor film, allowed to stand for 5 seconds, then spin-coated at 2000 rpm for 40 seconds, followed by heat annealing at 140 °C for 20 min to obtain a dry self-encapsulated perovskite absorber layer containing 2D composite functional material. After the sample cooled to room temperature, 100 μL of HTL was added... -aq The solution was spin-coated onto the surface of a self-coated perovskite containing 2D composite functional materials at a speed of 4000 rpm for 50 s. After drying at room temperature, a p-type HTL was obtained. Finally, a silver electrode with a thickness of approximately 80 nm was deposited on the substrate based on the ITO / ETL / 2D BP-GO NSs-coated perovskite absorber layer / HTL structure using vacuum thermal evaporation to complete the fabrication of the entire solar cell. The structure of the upright solar cell with a self-coated perovskite absorber layer containing 2D composite functional materials is as follows. Figure 1 As shown.
[0046] Examples 2-4 (Preparation of comparative samples with different contents)
[0047] In Examples 2-4, the preparation processes in steps 1), 2), and 3) remain unchanged. The difference lies in that the masses of 2DBP-GO NSs powder weighed in step 1) are 0.8 mg, 1.0 mg, and 1.4 mg, respectively. After obtaining the perovskite precursor film using the same preparation process as in step 4), the 2DBP-GO NSs dispersions A prepared in step 1) containing 0.8 mg, 1.0 mg, and 1.4 mg of NSs are respectively... aq2 100 μL was dropped onto the surface of the prepared precursor film. After standing for 5 s, it was spin-coated at 2000 rpm for 40 s and then heat-annealed at 140 ℃ for 20 min to obtain a self-encapsulated perovskite absorber layer based on different contents of 2D composite functional materials. Subsequently, a comparative device was fabricated using the same p-type HTL and silver electrode fabrication process as in step 4).
[0048] Examples 5-7 (Preparation of comparative samples based on different spin coating speeds)
[0049] In Examples 5-7, the preparation processes in steps 1), 2), and 3) remain unchanged; after obtaining the perovskite precursor film using the same preparation process as in step 4), the dispersion A containing 1.2 mg of 2D BP-GO NSs prepared in step 1) is... aq2 100 μL was dropped onto the surface of the prepared precursor film. After standing for 5 s, it was spin-coated at speeds of 1500 rpm, 2500 rpm, and 3000 rpm for 40 s, respectively. After heat annealing at 140 ℃ for 20 min, self-encapsulated perovskite absorber layers of 2D composite functional materials based on different spin-coating speeds were obtained. Subsequently, a comparative device was fabricated using the same p-type HTL and silver electrode fabrication process as in step 4).
[0050] Examples 8-10 (Preparation of comparative samples based on different annealing conditions)
[0051] Keeping the preparation processes in steps 1), 2), and 3) unchanged, after obtaining the perovskite precursor film using the same preparation process as in step 4), the dispersion A containing 1.2 mg of 2D BP-GO NSs prepared in step 1) is then... aq2 100 μL was dropped onto the surface of the prepared precursor film. After standing for 5 seconds, it was spin-coated at 2000 rpm for 40 seconds. The film was then subjected to thermal annealing at 120℃, 130℃, and 150℃ for 10 min, 20 min, and 30 min, respectively, to obtain self-encapsulated perovskite absorber layers of 2D composite functional materials based on different annealing conditions. Subsequently, a comparative device was fabricated using the same p-type HTL and silver electrode fabrication process as in step 4).
[0052] Comparative examples (preparation of conventional 3D perovskite absorber layer comparison samples without 2D composite functional materials and their solar cell comparison samples)
[0053] Maintain the same as step 1) of Example 1, A aq1 Solution and ETL in step 2) -aq and HTL -aq The solution preparation conditions remain unchanged; the preparation process of n-type ETL in step 3) remains unchanged; after obtaining the perovskite precursor film using the same preparation process as in step 4), the difference lies in: the post-treatment solution A of the perovskite precursor prepared in step 1) is... aq2 100 μL was dropped onto the surface of the prepared precursor film. After standing for 5 seconds, it was spin-coated at 2000 rpm for 40 seconds and then heat-annealed at 140 °C for 20 min to obtain a dry conventional 3D perovskite absorber layer. Subsequently, a comparative device was fabricated using the same p-type HTL and silver electrode fabrication process as in step 4).
[0054] Effect verification
[0055] Figure 2 Sections (a) and (b) show cross-sectional scanning electron microscope (SEM) images of a conventional 3D perovskite absorber layer and a self-coated perovskite absorber layer containing 2D composite functional materials, respectively. As can be seen from the figures, the conventional 3D perovskite film generally has a small grain size and disordered grain boundary arrangement, with a film thickness of approximately 800 nm. In contrast, the self-coated perovskite film containing 2D composite functional materials exhibits a relatively large grain size and ordered grain boundary arrangement along the normal direction. This is beneficial for accelerating the directional transport of photogenerated charges, reducing the probability of carrier recombination, and thus improving the photovoltaic performance of the solar cell. This morphological evolution of the perovskite caused by the 2D BP-GO NSs coating may be attributed to: the A prepared in step 1). 2D-aq2 When the solution is spin-coated onto the surface of the perovskite precursor obtained in step 4), due to A 2D-aq2 The presence of isopropanol solvent in the solution will cause van der Waals ripening; at this time, A 2D-aq2 In solution, 2D BP-GO NSs utilizes its surface groups and P and C elements to strongly coordinate with free ionic defects in the perovskite, passivating perovskite grain boundaries and interface defects while delaying the crystallization process. This promotes perovskite grain growth, and the 2D BP-GO NSs firmly adheres to the perovskite grain boundaries and surface, thus growing into a self-encapsulated perovskite absorber layer containing 2D composite functional materials, improving crystal quality and electrical properties. Furthermore, compared to conventional 3D perovskite films without 2D BP-GO NSs, the self-encapsulated perovskite film containing 2D composite functional materials prepared in step 4) has a brighter surface, indicating that the 2D BP-GO NSs coating of the perovskite grains alters the surface energy properties of the absorber layer, significantly improving the film's conductivity.
[0056] To analyze the synergistic mechanism of 2D BP-GO NSs processing technology on the phase structure, surface chemistry, and electrical properties of the perovskite absorber layer, X-ray photoelectron spectroscopy (XPS) was used to detect the two perovskite samples mentioned above. Figure 2 In the high-resolution XPS spectra of (c) and (d), it was found that the characteristic peaks of Pb 4f and N 1s of self-coated perovskites containing 2D composite functional materials are shifted towards the direction of lower binding energy. This proves that in the case of A 2D-aq2During the van der Waals ripening process induced by solution treatment, strong chemical coordination occurs between the surface groups and P and C elements of 2D BP-GO NSs and the uncoordinated metal and organic cations in the perovskite. This promotes the firm attachment of 2D BP-GO NSs to the perovskite grain boundaries and surface, effectively passivating deep-level defects in the material, strengthening crystal stability, and helping to suppress defect-assisted nonradiative recombination, thereby improving the photovoltaic output and stability of the cell. More importantly, the low binding energy shift of the high-resolution XPS nuclear level of the self-encapsulated perovskite containing 2D composite functional materials indicates the p-type doping nature of the self-encapsulated perovskite system structure described in this invention. This may be attributed to the changes in film composition, electronic properties (e.g., carrier type, concentration, etc.) and surface energy dynamics caused by the coating of perovskite grains with 2D BP-GO NSs.
[0057] To elucidate the synergistic mechanism of the 2D BP-GO NSs treatment technique on the electronic properties, surface energy, and energy level structure of the two perovskite absorber layers, Kelvin probe force microscopy (KPFM) and ultraviolet photoelectron spectroscopy (UPS) were used to examine perovskite samples with and without 2D BP-GO NSs coating. Figure 3 The UPS kinetic cutoff side (E) shown in sections (a) and (b) Cut - off The spectrum, combined with the work function (WF) = 21.22 eV - E Cut - off The formula allows us to calculate the WF values of conventional 3D perovskite films and self-coated perovskite films containing 2D composite functional materials to be 4.61 eV and 4.83 eV, respectively. From this, we can derive the corresponding Fermi levels (E0, E ... F The values are -4.61 eV and -4.83 eV, respectively. Furthermore, according to... Figure 3 The UPS Fermi edge (E) shown in sections (c) and (d) F,edge ) spectrum, combined with valence band (E) VB )= E F - E F , edge Formulas were used to calculate the E values of conventional 3D perovskite films and self-coated perovskite films containing 2D composite functional materials. VB The maximum values are -5.40 eV and -5.25 eV, respectively. It is evident that 2D BP-GO NSs can passivate deep-level defects while inducing band alignment at the absorber interface; this beneficial "energy ladder" lowers the interface energy barrier, accelerating the directional transport, extraction, and collection of photogenerated electrons and holes, thereby minimizing charge accumulation and recombination losses at the absorber layer and HTL interface, ultimately improving the photovoltaic output parameters of the solar cell, especially FF and Voc. Furthermore, KPFM images of the corresponding samples further validate the UPS observation results, such as... Figure 3As shown in (c) and (d), compared to conventional 3D perovskite films, the self-coated perovskite surface containing 2D composite functional materials prepared in step 4) exhibits a lower contact potential. This further confirms that 2D BP-GO NSs facilitates a closer proximity of the Fermi level to the valence band in the self-coated perovskite architecture, which helps accelerate photogenerated charge transfer and improve the Vo of the cell. OC This is consistent with the XPS results mentioned above.
[0058] Figure 4 The IV characteristic curves of upright solar cells fabricated using a self-coated perovskite absorber layer containing 2D composite functional materials and a conventional 3D perovskite absorber layer are shown. The effective area of both cells is 0.1 cm². 2 All tests were conducted under AM1.5G simulated sunlight. The photovoltaic performance of the self-coated perovskite absorber layer containing 2D composite functional materials described in this invention is higher than that of traditional uncoated devices, especially J... SC V OC The synergistic effect of 2D BP-GO NSs coating on perovskite grains alters the composition and electronic properties of the absorber layer, enhancing the built-in electric field and promoting efficient separation and directional transport of photogenerated electrons and holes within the absorber layer; 2) The enhanced built-in electric field and surface energy transition caused by the electronic passivation of 2DBP-GO NSs drive the interface energy level alignment between the self-coated perovskite and the adjacent charge transport layer, improving the preferential extraction and collection efficiency of photogenerated holes; 3) The 2D BP-GO NSs located at the grain boundaries and surface of the perovskite not only passivates deep-level defects but also provides a "fast path" for the transfer of photogenerated holes, balancing the carrier transport dynamics at the top and bottom interfaces of the perovskite while reinforcing the crystal quality of the absorber layer. Therefore, the key problems restricting the improvement of PSC efficiency and stability, such as trap-assisted charge recombination loss and interface carrier recombination loss in traditional polycrystalline perovskite material systems, have been solved.
[0059] In addition to the photovoltaic output performance of solar cells, examining the long-term storage stability of the upright solar cell with a self-coated perovskite absorber layer containing 2D composite functional materials prepared in this invention under environmental atmosphere is of great significance for estimating the commercial value of the device. Figure 5The diagram shows the efficiency degradation trend of a self-encapsulated perovskite absorber layer based on 2D composite functional materials and an unencapsulated cell based on a conventional 3D perovskite absorber layer stored for 500 hours under atmospheric conditions with an average relative humidity of ≈40±5% and an average temperature of ≈25±2 ℃. Due to the synergistic enhancement of the crystal quality, interface characteristics, built-in electric field, energy level structure, and charge dynamics of the BP-GO NSs-encapsulated perovskite absorber layer, the unencapsulated cell exhibits an efficiency loss of only 20% after 500 hours of storage, while the efficiency loss of the conventional unencapsulated cell is as high as 40%. This demonstrates that the structural design of the self-encapsulated perovskite absorber layer with 2D composite functional materials described in this invention effectively improves the storage stability of photovoltaic cells.
[0060] The above description is merely a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention should be included within the scope of protection of the present invention. Therefore, the scope of protection of the present invention should be determined by the scope of the claims.
Claims
1. A method for preparing a self-coated perovskite absorber layer containing a 2D composite functional material, characterized in that, The specific steps of the method are: 1) In a glove box with an oxygen content of 0.1 ppm and a water vapor content of 0.1 ppm, 1.75 mmol of lead iodide and 1.6 mmol of methylammonium iodide were weighed and dissolved in a mixed solvent containing 750 μL of N,N-dimethylformamide and 250 μL of dimethyl sulfoxide, and after magnetic stirring at room temperature for 30 min, a perovskite precursor solution was obtained; 2) 0.076 mmol of formamidinium hydriodate was weighed and dissolved in 1 mL of isopropanol solvent, and after magnetic stirring at room temperature for 30 min, a post-processing solution of the perovskite precursor was obtained; 3) 0.8-1.4 mg of two-dimensional black phosphorus-oxidized graphene composite nanosheet powder was dispersed in 1 mL of the post-processing solution of the perovskite precursor prepared in step 2), the bottle opening was tightly sealed, and then the glove box was removed and physical ultrasonic treatment was performed; the temperature of the water in the ultrasonic machine was controlled at 25±2 ℃, the ultrasonic frequency was set to 40 KHz, and the ultrasonic input power was controlled at 300 W; after 4 h of ultrasonic treatment, a two-dimensional black phosphorus-oxidized graphene composite nanosheet dispersion was obtained; 4) In the glove box, 100 μL of the perovskite precursor solution prepared in step 1) was dropped on the surface of the substrate, and then low-speed spinning at 500 rpm for 3 s was performed, followed by high-speed spinning at 4000 rpm for 40 s, and 400 μL of chlorobenzene was added 10 s before the end of the program, and then 100 ℃ thermal annealing treatment was performed for 10 min to obtain a perovskite precursor film; after the sample was cooled to room temperature, 100 μL of the two-dimensional black phosphorus-oxidized graphene composite nanosheet dispersion prepared in step 3) was dropped on the surface of the perovskite precursor film, and then high-speed spinning at 1500-3000 rpm for 40 s was performed, and then 120-150 ℃ thermal annealing treatment was performed for 10-30 min to obtain a dry self-coated perovskite absorption layer containing 2D composite functional material.
2. The method for preparing a self-coated perovskite absorber layer containing 2D composite functional materials according to claim 1, characterized in that, The mass of the two-dimensional black phosphorus-oxidized graphene composite nanosheet powder in step 3) is 1.2 mg.
3. The method for preparing a self-coated perovskite absorber layer containing 2D composite functional materials according to claim 1, characterized in that, The spinning speed of the two-dimensional black phosphorus-oxidized graphene composite nanosheet dispersion in step 4) is 2000 rpm.
4. The method for preparing a self-coated perovskite absorption layer containing 2D composite functional material according to claim 1, characterized in that, The thermal annealing treatment condition is: 140 ℃ for 20 min.
5. The self-coated perovskite absorber layer containing 2D composite functional material prepared by the method according to claim 1, characterized in that, The absorption layer is composed of two-dimensional black phosphorus-oxidized graphene composite nanosheets and three-dimensional perovskite crystal materials, wherein the two-dimensional black phosphorus-oxidized graphene composite nanosheets are coated on each three-dimensional perovskite crystal grain, and the thickness is controlled at 5-10 nm; the three-dimensional perovskite crystal grains have a grain size of 800-1000 nm and a thickness of 1 μm, and the grain boundaries between the three-dimensional perovskite crystal grains are orderly arranged along the normal direction.
6. A method for preparing a top structure solar cell with a self-coated perovskite absorption layer containing a 2D composite functional material, characterized in that, The method comprises the following steps: I. Solution preparation: a. Solution preparation for perovskite absorption layer: 1) In a glove box with oxygen content of 0.1 ppm and water vapor content of 0.1 ppm, 1.75 mmol of lead iodide and 1.6 mmol of methylammonium iodide were weighed and dissolved in a mixed solvent containing 750 μL of N,N-dimethylformamide and 250 μL of dimethyl sulfoxide, and after magnetic stirring at room temperature for 30 min, a perovskite precursor solution was obtained; 2) 0.076 mmol of formamidinium hydriodide was weighed and dissolved in 1 mL of isopropanol solvent, and after magnetic stirring at room temperature for 30 min, a post-processing solution of perovskite precursor was obtained; 3) 0.8-1.4 mg of two-dimensional black phosphorus-oxidized graphene composite nanosheet powder was dispersed in 1 mL of the post-processing solution of perovskite precursor prepared in step 2), and after the bottle opening was tightly sealed, it was removed from the glove box and subjected to physical ultrasonic treatment; the temperature of water in the ultrasonic machine was controlled at 25±2 ℃, the ultrasonic frequency was set at 40 KHz, and the ultrasonic input power was controlled at 300 W, and after 4 h of ultrasonic treatment, a two-dimensional black phosphorus-oxidized graphene composite nanosheet dispersion was obtained; b, solution preparation for charge transport layer: 1) Colloidal tin dioxide solution was mixed with ionized water at a volume ratio of 1:1, and after magnetic stirring at room temperature for 4 h, a well-dispersed SnO2 diluent was obtained; 2) 72.3 mg of Spiro-OMeTAD powder, 28.5 μL of TBP solvent and 18.5 μL of Li-TFSI / acetonitrile dispersion were mixed together in 1 mL of chlorobenzene, and after magnetic stirring at room temperature for 30 min, a Spiro-OMeTAD dispersion was obtained; the Li-TFSI / acetonitrile dispersion was prepared by dissolving 0.52 g of Li-TFSI in 1 mL of acetonitrile; II. Material and battery preparation: 1) Preparation of electron transport base material: In the laboratory at room temperature, 90 μL of SnO2 diluent was high-speed spin-coated at 4000 rpm for 50 s on an ITO substrate which had been cleaned beforehand, and after annealing treatment at 150 ℃ for 25 min, an n-type ETL with a thickness of 40 nm was obtained; after ultraviolet ozone treatment for 30 min, it was moved to a glove box for standby; wherein the oxygen content of the glove box should be controlled at 0.1 ppm, and the water vapor content should be controlled at 0.1 ppm; 2) Preparation of the self-coated perovskite absorber layer containing the 2D composite functional material: In a glove box, 100 μL of the perovskite precursor solution prepared in step 1 was drop-coated onto the n-type ETL surface obtained in step 1). First, it was spin-coated at a low speed of 500 rpm for 3 s, then at a high speed of 4000 rpm for 40 s. 400 μL of chlorobenzene was added 10 s before the end of the program. The mixture was then heat-annealed at 100 ℃ for 10 min to obtain the perovskite precursor film. After the sample cooled to room temperature, 100 μL of the two-dimensional black phosphorus-graphene oxide composite nanosheet dispersion prepared in step 1 was drop-coated onto the surface of the perovskite precursor film using a pipette. After standing for 5 s, it was spin-coated at a high speed of 1500~3000 rpm for 40 s, and then heat-annealed at 120~150 ℃ for 10~30 min. min, to obtain a dry self-encapsulated perovskite absorber layer containing 2D composite functional material; 3) Preparation of hole transport material: After the self-coated perovskite absorber layer containing 2D composite functional material is cooled to room temperature, 100 μL of the Spiro-OMeTAD dispersion prepared in step 1 is spin-coated onto the surface of the self-coated perovskite absorber layer containing 2D composite functional material obtained in step 2). After drying at room temperature, a p-type HTL with a thickness of 150 nm is obtained. The spin-coating speed is set at 4000 rpm and held for 50 s. The sample based on the ITO / ETL / self-coated perovskite absorber layer containing 2D composite functional material / HTL structure is removed from the glove box for later use. 4) Fabrication of metal electrode materials: Using vacuum thermal evaporation technology, a silver or gold back electrode with a thickness of 80 nm is deposited on the sample surface obtained in step 3) based on the ITO / ETL / self-coated perovskite absorber layer / HTL structure containing 2D composite functional materials, thus completing the fabrication of the entire solar cell; wherein, the background vacuum level of the vacuum thermal evaporation chamber should be controlled at 10 -1 Below Pa, the vacuum degree reaches 10. -3 After Pa, the coating operation should be performed, and the target power should be controlled at 5~15 W / cm². 2 The evaporation rate should be controlled between 0.9 and 1.2 Å / s.
7. A perovskite solar cell with a self-coated perovskite absorber layer and a 2D composite functional material in a normal structure, prepared by the method of claim 6, characterized in that, The solar cell, from bottom to top, consists of: a transparent conductive ITO glass substrate, an electron transport layer, a self-coated perovskite absorber layer containing 2D composite functional materials, a hole transport layer, and a metal back electrode.