A CsPbBr3 perovskite thin-film solar cell with a smooth surface and its preparation method.

By treating the surface of CsPbBr₃ perovskite with atomized aqueous solution, the problem of low efficiency of CsPbBr₃ perovskite solar cells is solved, and the surface flatness and photoelectric conversion efficiency are improved. This method is suitable for building-integrated photovoltaics and top cells of silicon tandem solar cells.

CN116669504BActive Publication Date: 2026-11-24XIDIAN UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202210153474.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-02-18
Publication Date
2026-11-24
Estimated Expiration
2042-02-18

AI Technical Summary

Technical Problem

The low efficiency of existing CsPbBr₃ perovskite solar cells is mainly due to the low fill factor. This is because the CsPbBr₃ perovskite surface has many defects and poor flatness, resulting in poor morphology of the transport layer deposited on it, high interfacial recombination, and low transport efficiency.

Method used

The surface of CsPbBr₃ perovskite is treated with atomized aqueous solution, which decomposes and reconstructs it during heating to form a smooth CsPbBr₃ perovskite light-absorbing layer, reducing surface defects, improving smoothness, and reducing interfacial recombination.

Benefits of technology

By improving surface smoothness, photoelectric conversion efficiency is increased, making it suitable for large-area or large-scale solar cell fabrication and reducing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116669504B_ABST
    Figure CN116669504B_ABST
Patent Text Reader

Abstract

This invention discloses a CsPbBr3 perovskite thin-film solar cell with a smooth surface and its fabrication method. The cell, from bottom to top, comprises: a transparent electrode layer, a first transport layer, a smooth CsPbBr3 perovskite light-absorbing layer, a second transport layer, and a metal electrode layer. This invention utilizes a fog-grown CsPbBr3 perovskite thin film, which reduces surface defects and improves surface smoothness, thereby improving the morphology of the second transport layer, reducing electron-hole recombination between the CsPbBr3 perovskite and the transport layer, and enhancing the photoelectric conversion efficiency of the CsPbBr3 perovskite thin-film solar cell.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of semiconductor technology, specifically relating to a CsPbBr3 perovskite thin-film solar cell with a smooth surface and its preparation method. Background Technology

[0002] In recent years, novel perovskite thin-film solar cells have attracted increasing attention and research due to their advantages such as tunable bandgap (1.2-2.3 eV), high light absorption coefficient, high energy conversion efficiency (25.7%), and low manufacturing cost. In particular, all-inorganic perovskites based on metallic Cs and lead halides are increasingly favored by researchers at home and abroad due to their excellent thermal stability, ultra-low cost, and simple preparation process.

[0003] Among many inorganic perovskite materials, CsPbBr3 has attracted much attention due to its superior stability caused by its extremely high band gap (>2.3eV).

[0004] However, existing methods for preparing CsPbBr3 perovskite solar cells result in low efficiency, primarily due to a low fill factor (FF). This is caused by numerous surface defects and poor smoothness in CsPbBr3 perovskites, leading to poor morphology of the transport layer deposited on it, high interfacial recombination rates, and low transport efficiency. These factors limit the application of CsPbBr3 solar cells in semi-transparent and tandem applications. Summary of the Invention

[0005] To address the aforementioned problems in the prior art, this invention provides a CsPbBr3 perovskite thin-film solar cell with a smooth surface and its fabrication method. The technical problem to be solved by this invention is achieved through the following technical solution:

[0006] A CsPbBr3 perovskite thin-film solar cell with a smooth surface, comprising, from bottom to top: a transparent electrode layer, a first transport layer, a CsPbBr3 perovskite light-absorbing layer with a smooth surface, a second transport layer, and a metal electrode layer.

[0007] In one embodiment of the present invention, the first transport layer and the second transport layer are either an electron transport layer or a hole transport layer, and are not the same.

[0008] In one embodiment of the present invention, the electron transport layer is made of an n-type semiconductor material; the hole transport layer is made of a p-type semiconductor material.

[0009] The beneficial effects of this invention are:

[0010] This invention treats the perovskite surface with an atomized aqueous solution during the heating process, enabling the CsPbBr3 surface to decompose and reconstruct instantly, thereby greatly reducing surface defects, improving surface smoothness, reducing interfacial recombination, and increasing light conversion efficiency.

[0011] The present invention will be further described in detail below with reference to the accompanying drawings and embodiments. Attached Figure Description

[0012] Figure 1 This is a schematic diagram of a CsPbBr3 perovskite thin-film solar cell with a smooth surface provided in an embodiment of the present invention.

[0013] Figure 2 This is a schematic diagram of a method for preparing a CsPbBr3 perovskite thin-film solar cell with a smooth surface, provided in an embodiment of the present invention.

[0014] Figure 3 These are schematic diagrams of two CsPbBr3 perovskite thin-film solar cell structures with smooth surfaces provided in embodiments of the present invention. Detailed Implementation

[0015] The present invention will be further described in detail below with reference to specific embodiments, but the implementation of the present invention is not limited thereto.

[0016] Example 1

[0017] Please see Figure 1 , Figure 1 This is a schematic diagram of a CsPbBr3 perovskite thin-film solar cell with a smooth surface, provided in an embodiment of the present invention. The cell comprises, from bottom to top, the following components:

[0018] The structure consists of a transparent electrode layer 1, a first transport layer 2, a flat CsPbBr3 perovskite light-absorbing layer 3, a second transport layer 4, and a metal electrode layer 5.

[0019] For example, the transparent electrode layer may be made of transparent oxides such as indium tin oxide (ITO), fluorine-doped tin oxide (FTO), or aluminum-doped zinc oxide (AZO), which have high light transmittance and low resistance. The electrode material may also be a precious metal such as gold (Au) or silver (Ag).

[0020] It should be noted that the CsPbBr3 perovskite light-absorbing layer 3 described in this invention is prepared through a fogging process. Fogging can reduce surface defects in CsPbBr3 and improve surface smoothness, thereby improving the morphology of the second transport layer, reducing electron-hole recombination between the CsPbBr3 perovskite and the transport layer, and enhancing the photoelectric conversion efficiency of the battery. This method can be applied to building-integrated photovoltaics, top-mounted silicon tandem solar cells, etc. Furthermore, the fogging chemical deposition method can be performed at ambient pressure and relatively low temperatures.

[0021] Optionally, the first transport layer and the second transport layer are either electron transport layers or hole transport layers, and they are not the same.

[0022] For example, if the first transport layer is an electron transport layer, then the second transport layer is a hole transport layer; if the first transport layer is a hole transport layer, then the second transport layer is an electron transport layer.

[0023] Optionally, the electron transport layer is made of an n-type semiconductor material; the hole transport layer is made of a p-type semiconductor material.

[0024] n-type semiconductor materials include, for example, metal oxides such as titanium oxide (TiO2), tin oxide (SnO2), and zinc oxide (ZnO), and organic materials such as fullerenes (PCBM).

[0025] p-type semiconductor materials, examples of which include 2,2',7,7'-tetratetra[N,N-di(4-methoxyphenyl)amino]-9,9'-spirodifluorene (spiro-OMeTAD), 3-hexylthiophene (P3HT), poly(ethylenedioxythiophene-poly(styrene sulfonate)) (PEDOT: PSS), and other organic materials, as well as nickel oxide (NiO). x Inorganic materials such as molybdenum oxide (MoO3) and cuprous thiocyanate (CuSCN).

[0026] Optionally, the CsPbBr3 perovskite light-absorbing layer is inorganic CsPbBr3 (Eg>2.3eV).

[0027] In summary, the atomization treatment provided by this invention can reduce surface defects of CsPbBr3 and improve surface smoothness, thereby improving the morphology of the second transport layer, reducing electron-hole recombination between CsPbBr3 perovskite and the transport layer, and improving the photoelectric conversion efficiency of the battery. It can be applied to building-integrated photovoltaics, top cells of silicon tandem solar cells, etc.

[0028] Example 2

[0029] Please see Figure 2 , Figure 2 This is a schematic diagram of a method for fabricating a CsPbBr3 perovskite thin-film solar cell with a smooth surface, provided by an embodiment of the present invention. The method includes:

[0030] Step 1: Deposit the first transport layer on the transparent electrode layer using a solution spin coating method.

[0031] For example, the transparent electrode layer may be made of transparent oxides such as indium tin oxide (ITO), fluorine-doped tin oxide (FTO), or aluminum-doped zinc oxide (AZO), which have high light transmittance and low resistance. The electrode material may also be a precious metal such as gold (Au) or silver (Ag).

[0032] Step 2: A CsPbBr3 perovskite light-absorbing layer is grown on the first transport layer by a two-step aqueous solution spin coating method.

[0033] Optionally, step 2 includes:

[0034] Step 2-1: Spin-coat the perovskite precursor solution onto the first transport layer to obtain the perovskite precursor layer, and perform a first annealing treatment on the perovskite precursor layer.

[0035] Step 2-2: Spin-coat CsBr solution onto the annealed perovskite precursor layer and perform a second annealing treatment to grow a CsPbBr3 perovskite light-absorbing layer on the first transport layer.

[0036] For example, in this invention, a perovskite precursor solution is spin-coated onto the first transport layer at a rotation speed of 2000 rpm for 30 s, followed by annealing at 90°C for 30 min to prepare a perovskite precursor layer. A CsBr solution is then spin-coated onto the perovskite precursor layer at a rotation speed of 2000 rpm for 30 s, followed by annealing at 250°C for 5 min to form a perovskite layer.

[0037] Optionally, the CsPbBr3 perovskite light-absorbing layer is inorganic CsPbBr3 (Eg>2.3eV).

[0038] Step 3: Spray an atomized solution onto the surface of the CsPbBr3 perovskite light-absorbing layer to obtain a smooth CsPbBr3 perovskite light-absorbing layer.

[0039] Optionally, the atomizing solution is a deionized aqueous solution.

[0040] Examples include isopropanol or methanol. The proportion of atomized particles with a diameter <5μm is approximately 65%, the mist flow rate is ≥2mL / min, the atomization treatment time is 30min, and the treatment temperature is 250℃.

[0041] Optionally, the first transport layer and the second transport layer are either electron transport layers or hole transport layers, and they are not the same.

[0042] For example, if the first transport layer is an electron transport layer, then the second transport layer is a hole transport layer; if the first transport layer is a hole transport layer, then the second transport layer is an electron transport layer.

[0043] Optionally, the electron transport layer is made of an n-type semiconductor material; the hole transport layer is made of a p-type semiconductor material.

[0044] n-type semiconductor materials include, for example, metal oxides such as titanium oxide (TiO2), tin oxide (SnO2), and zinc oxide (ZnO), and organic materials such as fullerenes (PCBM).

[0045] p-type semiconductor materials, examples of which include 2,2',7,7'-tetratetra[N,N-di(4-methoxyphenyl)amino]-9,9'-spirodifluorene (spiro-OMeTAD), 3-hexylthiophene (P3HT), poly(ethylenedioxythiophene-poly(styrene sulfonate)) (PEDOT: PSS), and other organic materials, as well as nickel oxide (NiO). x Inorganic materials such as molybdenum oxide (MoO3) and cuprous thiocyanate (CuSCN).

[0046] Step 4: Deposit the second transport layer on the smooth CsPbBr3 perovskite light-absorbing layer using a solution spin coating method.

[0047] Step 5: Grow a metal electrode layer on the second transport layer.

[0048] This invention enables the growth of metal electrode layers using thermal evaporation or magnetron sputtering.

[0049] Optionally, the growth conditions for the metal electrode layer are 1E-4Pa, 100w, and a film thickness of 100nm.

[0050] In summary, the beneficial effects of this invention are as follows:

[0051] 1. The main component of the treatment solution in this invention is an aqueous solution, which is environmentally friendly.

[0052] 2. CsPbBr3 perovskite thin films grown by fog can reduce surface defects and improve surface smoothness, thereby improving the morphology of the second transport layer, reducing electron-hole recombination between CsPbBr3 perovskite and the transport layer, and improving the photoelectric conversion efficiency of CsPbBr3 perovskite thin film solar cells.

[0053] 3. This invention, through atomization, can utilize the Leidenfrost effect (the phenomenon that a liquid does not wet a hot surface but only forms a vapor layer on it) to prevent a large amount of water from penetrating the perovskite layer into the film, while ensuring a sufficient amount of solution for surface reaction.

[0054] 4. Compared with the prior art, the present invention is applicable to the fabrication of large-area or large-scale solar cells and can reduce costs.

[0055] Example 3

[0056] See Figure 3 Figure a illustrates a surface-smooth CsPbBr3 perovskite thin-film solar cell with FTO conductive glass as the transparent electrode layer, Spiro-OMeTAD as the hole transport layer, and tin oxide (SnO2) as the electron transport layer, using a deionized aqueous solution as the atomizing solution. The preparation method is as follows:

[0057] Step 1: Deposit the first transport layer on the transparent electrode layer using a solution spin coating method.

[0058] The transparent FTO conductive glass substrate was ultrasonically cleaned for 15 minutes each with a detergent, deionized water, acetone and anhydrous ethanol, and then air-dried with nitrogen gas.

[0059] The tin oxide solution was diluted with deionized water at a ratio of 1:3 and set aside. The FTO conductive glass substrate was treated with UV-ozone for 15 minutes, and then the tin oxide solution was spin-coated onto the FTO at a speed of 3000 rpm for 30 seconds. After spin-coating, it was annealed at 150°C for 30 minutes to crystallize and form an n-type electron transport layer.

[0060] Step 2: A CsPbBr3 perovskite light-absorbing layer is grown on the first transport layer by a two-step aqueous solution spin coating method.

[0061] On the substrate where the n-type electron transport layer has already been prepared, the perovskite precursor solution (PbBr2 solution, DMF solvent, DMF: dimethylformamide) was spin-coated at 2000 rpm for 30 s, followed by annealing at 90 °C for 30 min. Then, the CsBr aqueous solution was spin-coated at 2000 rpm for 30 s, followed by annealing at 250 °C for 5 min.

[0062] Step 3: Spray an atomized solution onto the surface of the CsPbBr3 perovskite light-absorbing layer to obtain a smooth CsPbBr3 perovskite light-absorbing layer.

[0063] The prepared CsPbBr3 perovskite film was placed in the chamber, which was then positioned at the heating center inside the quartz tube of a tubular furnace. The furnace was heated to 250°C, and a deionized aqueous solution was atomized using an ultrasonic atomizer (with approximately 65% ​​particles <5 μm in diameter and a mist flow rate ≥2 mL / min) and introduced into the chamber (nitrogen was used as the carrier gas at a flow rate of 0.5 m³ / min). 3 The processing time is 30 minutes ( / h).

[0064] Step 4: Deposit the second transport layer on the smooth CsPbBr3 perovskite light-absorbing layer using a solution spin-coating method.

[0065] The prepared Spiro-OMeTAD solution was first spin-coated at 1000 rpm for 5 seconds, and then at 4000 rpm for 40 seconds onto the CsPbBr3 perovskite light-absorbing layer. The solution was then air-dried in a dry nitrogen atmosphere for two minutes to allow it to oxidize for one day.

[0066] Step 5: Grow a metal electrode layer on the second transport layer.

[0067] A 100 nm Ag(Au) layer was grown on the substrate where the p-type hole transport layer had already been prepared using thermal evaporation. The preparation conditions were: growth pressure of 1E-4 Pa and growth rate of 0.5%. A conductive electrode is obtained.

[0068] Example 4

[0069] See Figure 3 b, shows a method using transparent FTO conductive glass as a substrate, NiO x The CsPbBr3 perovskite solar cell uses PCBM as the hole transport layer material and has a smooth electron transport layer surface. A 10% isopropanol deionized water solution is used as the atomizing solution, and its preparation method is as follows:

[0070] Step 1: Deposit the first transport layer on the transparent electrode layer using a solution spin coating method.

[0071] The transparent FTO conductive glass substrate was ultrasonically cleaned for 15 minutes each with a detergent, deionized water, acetone and anhydrous ethanol, and then air-dried with nitrogen gas.

[0072] The cleaned transparent FTO conductive glass substrate was treated with UV-ozone for 15 minutes. The pre-prepared nickel oxide solution was then spin-coated onto the FTO substrate at a speed of 3000 rpm for 30 seconds. The substrate was then annealed at 250°C for 45 minutes to crystallize into a film.

[0073] Step 2: A CsPbBr3 perovskite light-absorbing layer is grown on the first transport layer by a two-step aqueous solution spin coating method.

[0074] On the substrate where the p-type hole transport layer has already been prepared, the perovskite precursor solution (DMF solution of PbBr2) is spin-coated at 2000 rpm for 30 s, followed by annealing at 90 °C for 30 min. Then, the CsBr aqueous solution is spin-coated at 2000 rpm for 30 s, followed by annealing at 250 °C for 5 min.

[0075] Step 3: Spray an atomized solution onto the surface of the CsPbBr3 perovskite light-absorbing layer to obtain a smooth CsPbBr3 perovskite light-absorbing layer.

[0076] The prepared CsPbBr3 perovskite film was placed in the chamber, which was then positioned at the heating center inside the quartz tube of a tubular furnace. The furnace was heated to 250°C, and an isopropanol solution was atomized into the chamber using an ultrasonic atomizer (with approximately 65% ​​of the particles having a diameter <5μm and a mist flow rate ≥2mL / min). Nitrogen was used as the carrier gas at a flow rate of 0.5m³ / min. 3 The processing time is 30 minutes ( / h).

[0077] Step 4: Deposit the second transport layer on the smooth CsPbBr3 perovskite light-absorbing layer using a solution spin coating method.

[0078] The prepared PCBM solution was spin-coated onto the atomized CsPbBr3 perovskite light-absorbing layer at a speed of 2000 rpm for 30 s. After spin-coating, the layer was air-dried in a dry nitrogen atmosphere for two minutes to obtain the n-type electron transport layer.

[0079] Step 5: Grow a metal electrode layer on the second transport layer.

[0080] A 100 nm Ag(Au) layer was grown on the substrate where the n-type electron transport layer had already been prepared using thermal evaporation. The preparation conditions were: growth pressure of 1E-4 Pa and growth rate of 0.5%. A conductive electrode is obtained.

[0081] The above description, in conjunction with specific preferred embodiments, provides a further detailed explanation of the present invention. It should not be construed that the specific implementation of the present invention is limited to these descriptions. For those skilled in the art, various simple deductions or substitutions can be made without departing from the concept of the present invention, and all such modifications and substitutions should be considered within the scope of protection of the present invention.

Claims

1. A type of surface with a smooth surface A method for fabricating perovskite thin-film solar cells, characterized in that, The method includes: Step 1: Deposit the first transport layer on the transparent electrode layer using a solution spin coating method; Step 2: Growth on the first transport layer using a two-step aqueous solution spin coating method. Perovskite light-absorbing layer; Step 3: Prepare the... The substrate of the perovskite light-absorbing layer is placed in a heating chamber and heated to 250°C. An atomized solution is then introduced into the chamber using an ultrasonic atomizer. Utilizing the Leidenfrost effect, the atomized solution... A vapor layer is formed on the surface of the perovskite light-absorbing layer to absorb the light. The surface of the perovskite light-absorbing layer is treated to obtain a smooth surface. A perovskite light-absorbing layer; wherein the atomized particles of the atomized solution have a diameter of <5μm and a particle ratio of 65%, the atomization volume is ≥2mL / min, and the processing time is 30min; Step 4: Apply the solution to a smooth surface using spin coating. A second transport layer is deposited on the perovskite light-absorbing layer; Step 5: Grow a metal electrode layer on the second transport layer.

2. The method according to claim 1, characterized in that, Step 2 includes: Step 2-1: Spin-coat the perovskite precursor solution onto the first transport layer to obtain a perovskite precursor layer, and perform a first annealing treatment on the perovskite precursor layer; the temperature of the first annealing treatment is 90℃. Step 2-2: Spin-coat CsBr solution onto the annealed perovskite precursor layer and perform a second annealing treatment at a temperature of 250°C to grow on the first transport layer. Perovskite light-absorbing layer.

3. A type of surface with a smooth surface Perovskite thin-film solar cells, characterized in that, The surface smooth according to claim 1 or 2 The perovskite thin-film solar cell is prepared by a method for fabricating perovskite thin-film solar cells, wherein the cells, from bottom to top, comprise: Transparent electrode layer (1), first transport layer (2), and smooth surface The perovskite light-absorbing layer (3), the second transport layer (4), and the metal electrode layer (5) are all present.

4. The battery according to claim 3, characterized in that, The first transport layer and the second transport layer are either electron transport layer or hole transport layer, and they are not the same.

5. The battery according to claim 4, characterized in that, The electron transport layer is made of n-type semiconductor material; The hole transport layer uses a p-type semiconductor material.

Citation Information

Patent Citations

  • Perovskite solar cell with organic skeletal structure and manufacturing method therefor