Rr-type two-dimensional perovskite thin film, solar cell and preparation method thereof
By using alicyclic amine compounds and controlling the composition of the precursor solution, RP-type two-dimensional perovskite thin films were prepared, solving the stability and efficiency problems of two-dimensional perovskite solar cells and achieving high-efficiency photoelectric conversion and long-term stability.
Patent Information
- Application Number
- CN202310435012.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-20
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-04-20
AI Technical Summary
Existing two-dimensional perovskite solar cells are prone to decomposition under light, humidity and high temperature environments, and their stability issues limit their commercial application. Furthermore, current research on organic spacer cations mainly focuses on straight-chain aliphatic compounds, which have low photoelectric conversion efficiency.
Alicyclic amine compounds were used as organic spacer cations. The molar concentration of lead ions and the molar ratio of FAI to MAI in the precursor solution were controlled. RP-type two-dimensional perovskite thin films were prepared by solution spin coating and then combined with conventional materials to prepare perovskite solar cells.
It improves the photoelectric conversion efficiency and stability of perovskite solar cells, with a maximum photoelectric conversion efficiency of 16.70%, and the efficiency can still be maintained at over 70% after 400 hours of operation.
Smart Images

Figure CN116669505B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the technical field of perovskite solar cells, and more specifically, relates to RP-type two-dimensional perovskite thin films, solar cells, and methods for their fabrication. Background Technology
[0002] Energy shortages and the resulting pollution are receiving increasing attention, and the development of clean and renewable energy sources has long been a research hotspot. Solar energy, due to its cleanliness, high energy output, wide distribution, and long-lasting nature, is gradually becoming one of the main forms of future energy supply. A solar cell is a device that directly converts solar radiation energy into electrical energy using the photoelectric effect. Given sufficient light intensity, this device can output voltage and generate current when a circuit is established, making it an important means of efficiently utilizing solar energy. Silicon-based solar cells have a mature commercial industry, but their high cost and energy consumption significantly limit their application scope.
[0003] As a third-generation solar cell, perovskite solar cells possess a series of advantages such as solution-processability and low cost. Since their development in 2009, their photoelectric conversion efficiency has significantly improved in just fourteen years, and their industrialization scale has been gradually expanding in recent years, attracting considerable attention and research from scientists. However, three-dimensional perovskites are prone to decomposition under light, humidity, and high-temperature environments, and their stability issues pose a significant obstacle to commercial applications. Compared to three-dimensional perovskites, two-dimensional or quasi-two-dimensional perovskites exhibit superior moisture and temperature stability due to the presence of organic spacer cations in their structure. Furthermore, the diversity of organic spacer cations endows two-dimensional perovskites with a variety of types and properties, thus attracting widespread attention.
[0004] Currently, Ruddlesden-Popper type perovskite solar cells are a research hotspot. Researchers have identified many high-performing organic spacer cations. However, current research on organic spacer cations mainly focuses on linear aliphatic and aromatic compounds, while alicyclic compounds are rarely used as organic spacer cations, and their photoelectric conversion efficiency is relatively low. Therefore, finding more high-performance organic spacer cations to expand the application range of two-dimensional perovskite solar cells has become an urgent technical problem to be solved. Summary of the Invention
[0005] To address the aforementioned technical problems, the primary objective of this invention is to provide a method for preparing RP-type two-dimensional perovskite thin films, using alicyclic amine compounds as organic spacer cations. Based on this method, the prepared RP-type two-dimensional perovskite thin films and solar cells exhibit good photoelectric conversion efficiency and device stability.
[0006] The second objective of this invention is to provide an RP-type two-dimensional perovskite thin film prepared by the above-described preparation method.
[0007] A third objective of this invention is to provide the application of the above-mentioned RP-type two-dimensional perovskite thin film in the fabrication of perovskite solar cells.
[0008] The fourth objective of this invention is to provide a perovskite solar cell containing the above-mentioned RP-type two-dimensional perovskite thin film.
[0009] The fifth objective of this invention is to provide a method for preparing a perovskite solar cell containing the above-mentioned RP-type two-dimensional perovskite thin film.
[0010] To achieve the above objectives, the present invention is implemented through the following technical solution:
[0011] A method for preparing RP-type two-dimensional perovskite thin films includes the following steps:
[0012] S1. Preparation of organic spacer cation: Hydroiodic acid and solvent are mixed, and an alicyclic amine compound is added in an ice-water bath and stirred to react. The solvent is removed, and the organic spacer cation is obtained by post-treatment. The alicyclic amine compound is R-CH2-NH2, wherein R is selected from cycloalkyl groups containing 3 to 6 carbon atoms.
[0013] S2. Preparation of precursor solution: The organic spacer cation, formamidinium hydroiodate, methyl iodide, and lead iodide are mixed in a molar ratio of 2:3.6:0.4:5, and added to a mixed solvent of dimethyl sulfoxide and N,N-dimethylformamide. The mixture is stirred until completely dissolved to obtain a perovskite precursor solution. The molar ratio of formamidinium hydroiodate to methyl iodide is 0.5:0.5 to 0.92:0.08. The molar concentration of lead ions in the perovskite precursor solution is 1.05 to 1.5 mol / L.
[0014] S3. Preparation of RP-type two-dimensional perovskite thin film: The perovskite precursor solution is prepared by solution spin coating to obtain the RP-type two-dimensional perovskite thin film.
[0015] Through extensive and long-term research, the inventors have discovered an RP-type two-dimensional perovskite thin film with excellent photoelectric conversion efficiency and stability, as well as perovskite solar cells based on the RP-type two-dimensional perovskite thin film. The inventors found that by using alicyclic amine compounds with a specific number of carbon atoms as organic spacer cations in two-dimensional or quasi-two-dimensional perovskites, and by simultaneously controlling the molar concentration of lead ions in the precursor components (≥1.05 mol / L) and the molar ratio of FAI (formamidinium hydroiodide) and MAI (methylamine iodide) within a specific range (0.5:0.5 to 0.92:0.08), the prepared RP-type two-dimensional perovskite thin film or perovskite solar cell can achieve excellent photoelectric conversion efficiency and device stability. The inventors discovered that, compared to linear aliphatic compounds, alicyclic amines exhibit weaker steric effects under the same carbon number conditions. This reduces the thickness of the insulating layer, alleviates insufficient interlayer charge transport, and thus improves device performance. Furthermore, the inventors found that alicyclic amines with ≥7 carbon atoms cannot form a three-dimensional perovskite structure. The inventors also discovered that increasing the molar concentration of lead ions in the perovskite precursor solution within a certain range yields a thicker perovskite film. As a light-absorbing layer, this film absorbs more photons under the same light intensity, generating more photogenerated carriers, resulting in increased short-circuit current and improved battery efficiency. In addition, by adjusting the molar ratio of FAI (formamidinium hydroiodide) and MAI (methylamine iodide), the inventors improved the stability of methylamine iodide at high temperatures, reduced the escape of methylamine iodide from the perovskite film, and prevented the perovskite structure from being destroyed, thereby improving battery stability. By controlling the above-mentioned process conditions and combining them with other process steps and conditions in this invention, this invention provides a perovskite solar cell based on RP-type two-dimensional perovskite thin film, which has a photoelectric conversion efficiency of up to 16.70%. After the cell has been running for 400 hours, the efficiency can still be maintained at more than 70% of the initial efficiency, showing good device stability.
[0016] The molecular formula of the RP-type two-dimensional perovskite thin film prepared by the above method is A'2A. (n-1) Pb n I 3n+1 Where n is 5, A' is the alicyclic amine compound, and A is FA. X MA 1-X FAI stands for formamidin hydroiodide, MAI stands for methyl iodide, and the ratio of X to 1-X is the molar ratio of FAI to MAI.
[0017] In some embodiments, the alicyclic amine compound is selected from cyclopropylmethylamine, cyclobutylmethylamine, cyclopentylmethylamine, or cyclohexylmethylamine. Preferably, the alicyclic amine compound is cyclopropylmethylamine. Under this preferred condition, the perovskite solar cell exhibits higher photoelectric conversion efficiency and stability.
[0018] In some embodiments, the volume ratio of dimethyl sulfoxide to N,N-dimethylformamide is 2:3 to 12. Preferably, the volume ratio of dimethyl sulfoxide to N,N-dimethylformamide is 2:3 to 8; more preferably, the volume ratio of dimethyl sulfoxide to N,N-dimethylformamide is 2:3. Under these preferred conditions, the perovskite solar cell exhibits higher photoelectric conversion efficiency and stability.
[0019] In some embodiments, the molar ratio of formamidinium hydroiodate to methyl iodide is 0.7:0.3 to 0.9:0.1. Preferably, the molar ratio of formamidinium hydroiodate to methyl iodide is 0.7:0.1 to 0.9:0.1; more preferably, the molar ratio of formamidinium hydroiodate to methyl iodide is 0.9:0.1. Under these preferred conditions, the perovskite solar cell exhibits higher photoelectric conversion efficiency and stability.
[0020] In some embodiments, the molar concentration of lead ions in the perovskite precursor solution is 1.1–1.4 mol / L. Preferably, the molar concentration of lead ions in the perovskite precursor solution is 1.1–1.2 mol / L; more preferably, the molar concentration of lead ions in the perovskite precursor solution is 1.1 mol / L. Under these preferred conditions, the perovskite solar cell exhibits higher photoelectric conversion efficiency and stability.
[0021] In some embodiments, the molar ratio of hydroiodic acid to alicyclic amine compound is 1:1 to 1.05.
[0022] In some embodiments, the volume-to-mass ratio of the solvent to the alicyclic amine compound is 5–10:1 mL / g.
[0023] In some implementations, the solvent in step S1 is anhydrous ethanol.
[0024] In some embodiments, the solvent is removed by rotary evaporation in step S1. More specifically, the temperature of the rotary evaporation is 30–45°C.
[0025] In some embodiments, the post-treatment involves washing away anhydrous ethanol from the crude product with an organic solvent, followed by drying to obtain an organic spacer cation. More specifically, the organic solvent may be diethyl ether, and to ensure thorough washing of the crude product, the volume of diethyl ether used may be at least five times the volume of anhydrous ethanol; more specifically, the drying temperature is 40–65°C.
[0026] In some embodiments, the solvent spin-coating method includes: spin-coating the perovskite precursor solution onto the front electrode, then adding an antisolvent, and annealing at 110–130°C to crystallize the perovskite and form the RP-type two-dimensional perovskite film. More specifically, the antisolvent can be a conventionally used antisolvent in the art, such as chlorobenzene. More specifically, during spin-coating, the spin-coating speed can be controlled at 4500–5500 rpm, the spin-coating time at 55–65 s, and the antisolvent is gradually added starting after the 30th second of spin-coating.
[0027] In some embodiments, the front electrode is ITO transparent conductive glass.
[0028] In some implementations, the temperature of the ice water bath is between 10 and 20°C.
[0029] Furthermore, this invention claims protection for the RP-type two-dimensional perovskite thin film prepared by the above preparation method.
[0030] Furthermore, the present invention also claims protection for a perovskite solar cell, which comprises, from bottom to top: a front electrode, a light-absorbing layer, and a metal electrode; the light-absorbing layer is an RP-type two-dimensional perovskite thin film prepared by the above-described preparation method.
[0031] Furthermore, the present invention also claims protection for a perovskite solar cell, which comprises, from bottom to top: a front electrode, a hole transport layer, a light-absorbing layer, an electron transport layer, an interface modification layer, and a metal electrode; wherein the light-absorbing layer is an RP-type two-dimensional perovskite thin film prepared by the above preparation method.
[0032] In some embodiments, the front electrode, hole transport layer, electron transport layer, interface modification layer, or metal electrode can be materials conventionally used in the art for fabricating perovskite solar cells. More specifically, the front electrode includes, but is not limited to, ITO transparent conductive glass; the hole transport layer includes, but is not limited to, PEDOT:PSS; the electron transport layer includes, but is not limited to, C60; the interface modification layer includes, but is not limited to, BCP; and the metal electrode material includes, but is not limited to, Ag.
[0033] Furthermore, this invention also claims protection for a method for preparing the above-mentioned perovskite solar cell, comprising the following steps:
[0034] (1) A hole transport layer is prepared by depositing a hole transport material on the front electrode;
[0035] (2) Prepare a light-absorbing layer on the hole transport layer in step (1);
[0036] (3) An electron transport layer, an interface modification layer and a metal electrode are sequentially prepared on the light-absorbing layer in step (2).
[0037] The hole transport layer and / or light-absorbing layer can be prepared by solvent spin coating; the electron transport layer, interface modification layer, and / or metal electrode can be prepared by vacuum deposition. More specifically, when preparing the hole transport layer, the annealing temperature of the solvent spin coating method can be 150°C and the annealing time can be 15 min; more specifically, the thickness of the metal electrode Ag is 150 nm.
[0038] Compared with the prior art, the present invention has the following beneficial effects: The present invention provides alicyclic amine compounds that can serve as organic spacer cations. Based on this, the inventors further controlled the molar ratio of FAI to MAI in the precursor solution, the molar concentration of lead ions, and the parameters such as dimethyl sulfoxide (DMSO) and N,N-dimethylformamide (DMF) in the solvent. The perovskite solar cells prepared based on this have excellent photoelectric conversion efficiency and device stability. The photoelectric conversion efficiency can reach up to 16.70%, and the efficiency can still be maintained at more than 70% of the initial efficiency after the cell has been running for 400 hours. Attached Figure Description
[0039] Figure 1 The X-ray diffraction patterns are those of the RP-type two-dimensional perovskite films prepared in Examples 1-4.
[0040] Figure 2 The UV-Vis absorption spectra of the RP-type two-dimensional perovskite films prepared in Examples 1-4 are shown.
[0041] Figure 3 The MPP test curve of the RP-type two-dimensional perovskite solar cell prepared in Example 13 is shown. Detailed Implementation
[0042] The present invention will be further described below with reference to the accompanying drawings and specific embodiments, but the embodiments do not limit the present invention in any way. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in this technical field.
[0043] Example 1: Preparation of RP-type two-dimensional perovskite thin films
[0044] RP-type two-dimensional perovskite thin films have the general structural formula (A'I)2(FA). 0.9 MA 0.1I)4(PbI2)5, wherein A'I is cyclopropylmethylamine hydroiodate, FAI is formamidin hydroiodate, MAI is methylamine iodide, and PbI2 is lead iodide, is prepared by the following steps:
[0045] (1) Preparation of organic spacer cation: Take 10 mmol of cyclopropyl methylamine solution and 10 mmol of hydroiodic acid solution and mix them in 3.56 ml of anhydrous ethanol. Stir for 4 h under ice bath conditions until the reaction is complete. Rotate the solution in step (1) at 40 °C until all the solvent evaporates to obtain crude product. Wash the crude product obtained in step (2) four times with diethyl ether to obtain the purified target product - cyclopropyl methylamine hydroiodide. Then, vacuum dry for 36 hours to obtain organic spacer cation (cyclopropyl methylamine hydroiodide).
[0046] (2) Preparation of precursor solution: Weigh 43.79 mg cyclopropylmethylamine hydroiodate, 68.10 mg formamidin hydroiodate, 6.99 mg methylamine iodide and 253.55 mg lead iodide and dissolve them in 500 μL of a mixed solvent of dimethyl sulfoxide (DMSO) and N,N-dimethylformamide (DMF), wherein the solvent ratio of DMSO:DMF = 2:3, and stir at 65 °C for 1.5 hours until completely dissolved to prepare a perovskite precursor solution (wherein the molar concentration of lead ions is 1.1 mol / L);
[0047] (3) Preparation of RP-type two-dimensional perovskite thin film: Take 30 μL of the perovskite precursor solution prepared in step (2) and drop it onto the front electrode. Control the rotation speed to ① 2000 rpm for 10 seconds; ② 5000 rpm for 55 seconds. Add 110 μL of chlorobenzene at the 30th second of step ② and anneal in a dry air atmosphere at 120℃ for 12 minutes. After the annealing is completed, RP-type two-dimensional perovskite thin film is obtained.
[0048] Example 2: Preparation of RP-type two-dimensional perovskite thin films
[0049] The difference between this embodiment and embodiment 1 is that in step (1), 10 mmol of cyclobutyl methylamine solution is taken.
[0050] Example 3: Preparation of RP-type two-dimensional perovskite thin films
[0051] The difference between this embodiment and embodiment 1 is that in step (1), 10 mmol of cyclopentylmethylamine solution is taken.
[0052] Example 4: Preparation of RP-type two-dimensional perovskite thin films
[0053] The difference between this embodiment and embodiment 1 is that in step (1), 10 mmol of cyclohexylmethylamine solution is taken.
[0054] Example 5: Preparation of RP-type two-dimensional perovskite thin films
[0055] The difference between this embodiment and embodiment 1 is that in step (2), 37.83 mg of formamidin hydroiodide and 34.97 mg of methyl iodide are taken (the molar ratio of formamidin hydroiodide and methyl iodide is 0.5:0.5).
[0056] Example 6: Preparation of RP-type two-dimensional perovskite thin films
[0057] The difference between this embodiment and embodiment 1 is that in step (2), 52.97 mg of formamidin hydroiodide and 20.98 mg of methyl iodide are taken (the molar ratio of formamidin hydroiodide to methyl iodide is 0.7:0.3).
[0058] Example 7: Preparation of RP-type two-dimensional perovskite thin films
[0059] The difference between this embodiment and embodiment 1 is that in step (2), 69.61 mg of formamidin hydroiodide and 5.60 mg of methyl iodide are taken (the molar ratio of formamidin hydroiodide to methyl iodide is 0.92:0.08).
[0060] Example 8: Preparation of RP-type two-dimensional perovskite thin films
[0061] The difference between this embodiment and embodiment 1 is that in step (2), the molar concentration of lead ions in the perovskite precursor solution is 1.2 mol / L.
[0062] Example 9: Preparation of RP-type two-dimensional perovskite thin films
[0063] The difference between this embodiment and embodiment 1 is that in step (2), the molar concentration of lead ions in the perovskite precursor solution is 1.3 mol / L.
[0064] Example 10: Preparation of RP-type two-dimensional perovskite thin films
[0065] The difference between this embodiment and embodiment 1 is that in step (2), the molar concentration of lead ions in the perovskite precursor solution is 1.4 mol / L.
[0066] Example 11: Preparation of RP-type two-dimensional perovskite thin films
[0067] The difference between this embodiment and embodiment 1 is that in step (2), DMSO:DMF = 2:8.
[0068] Example 12: Preparation of RP-type two-dimensional perovskite thin films
[0069] The difference between this embodiment and embodiment 1 is that in step (2), DMSO:DMF = 2:12.
[0070] Example 13 Fabrication of Perovskite Solar Cells
[0071] (1) Pretreatment of the front electrode: After cleaning the etched ITO transparent conductive glass with detergent, it is ultrasonicated for 15 minutes each with ultrapure water and anhydrous ethanol, then dried with nitrogen and placed in a clean petri dish to obtain a clean ITO transparent conductive glass front electrode, which is then treated with ultraviolet ozone for 20 minutes.
[0072] (2) Hole transport layer preparation: Take 70 μL of hole transport material PEDOT:PSS (solid content of about 1.5%, PEDOT content of about 0.21%, Xi'an Baolait, Al 4083) and drop it onto the ITO transparent conductive glass front electrode treated in step (1) with a pipette. After rotating at 5000 rpm for 30 seconds, place the ITO transparent conductive glass front electrode coated with PEDOT:PSS at 150℃ for annealing for 15 min. After annealing, place the ITO transparent conductive glass front electrode coated with hole transport layer on a spin coater and clean the surface with a rubber bulb.
[0073] (3) Preparation of light-absorbing layer: Using the preparation process in step (3) of Example 1, the titanium dioxide precursor solution prepared in Example 1 is spin-coated onto the ITO transparent conductive glass front electrode coated with the hole transport layer to form a thin film.
[0074] (4) Preparation of electron transport layer, interface modification layer and metal electrode: The above substrate is transferred to a vacuum chamber and an electron transport layer (C60, 40 nm thick), an interface modification layer (BCP (2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline, 8 nm thick) and a metal electrode (Ag, 150 nm thick) are sequentially deposited on the thin film of step (3) to obtain a perovskite solar cell.
[0075] Examples 14-24: Fabrication of Perovskite Solar Cells
[0076] The difference between Examples 14-24 and Example 13 is that Examples 14-24 use the perovskite precursor solutions of Examples 2-12 to prepare perovskite solar cells.
[0077] Comparative Example 1
[0078] The difference between this embodiment and embodiment 1 is that in step (2), 74.15 mg of formamidin hydroiodide and 1.40 mg of methyl iodide are taken (the molar ratio of formamidin hydroiodide to methyl iodide is 0.98:0.02).
[0079] Comparative Example 2
[0080] The difference between this embodiment and embodiment 1 is that in step (2), the molar concentration of lead ions in the perovskite precursor solution is 1.0 mol / L.
[0081] Comparative Example 3
[0082] The difference between this embodiment and Example 1 is that Comparative Example 3 uses a straight-chain aliphatic n-butylamine with the same number of carbon atoms (4).
[0083] Comparative Examples 4-6
[0084] The difference between Comparative Examples 4-6 and Example 13 is that Comparative Examples 4-6 used the perovskite precursor solutions of Comparative Examples 1-3 to prepare perovskite solar cells.
[0085] Test Example 1
[0086] X-ray diffraction and ultraviolet-visible absorption spectroscopy tests were performed on the RP-type two-dimensional perovskite films prepared in Examples 1-4. Figure 1 The X-ray diffraction patterns of the RP-type two-dimensional perovskite thin films prepared in Examples 1-4 are shown below. Figure 2 The UV-Vis absorption spectra of the RP-type two-dimensional perovskite films prepared in Examples 1-4 are shown.
[0087] Depend on Figure 1 It can be seen that the X-ray diffraction patterns of the RP-type two-dimensional perovskite films prepared in Examples 1 and 2 show peaks at angles below 10°, indicating the presence of a (0k0) crystal plane with a low n value. Two distinct peaks were observed at diffraction angles (2θ) near 14° and 28°, which are attributed to the (111) and (202) diffraction of the two-dimensional perovskite, respectively. Compared to Example 1, the XRD patterns of Examples 2–4 show more impurity peaks, indicating relatively poor crystal quality, which is also consistent with the difference in device efficiency.
[0088] Depend on Figure 2 It can be seen that the UV-Vis absorption spectra of the RP-type two-dimensional perovskite films prepared in Examples 1-4 show multiple absorption peaks, indicating the presence of multiple phases with different n values in the films. Compared to Example 1, the absorption peak positions of Examples 2-4 show a red shift.
[0089] also, Figure 3 MPP test of the two-dimensional perovskite solar cell prepared in Example 1, such as Figure 3 As shown, under N2 atmosphere and maximum power point tracking test, the battery efficiency can still be maintained at more than 77% of the initial efficiency after 400 hours of operation.
[0090] Test Example 2
[0091] The perovskite solar cells prepared in Examples 13-24 and Comparative Examples 4-6 were subjected to MPP tests, and the data are shown in Table 2 below.
[0092] Table 2
[0093] project Voc(V) <![CDATA[Jsc(mA / cm 2 )]]> FF (%) PCE (%) Example 13 1.04 21.61 74.08 16.70 Example 14 1.06 14.34 58.57 8.93 Example 15 1.06 15.46 63.40 10.43 Example 16 1.05 11.75 58.35 7.22 Example 17 0.94 17.57 53.83 8.92 Example 18 1.00 18.29 60.56 11.06 Example 19 0.88 18.67 64.57 10.59 Example 20 1.00 21.45 67.97 14.59 Example 21 1.00 21.80 65.63 14.33 Example 22 0.98 21.17 67.54 14.08 Example 23 0.98 19.00 68.68 12.84 Example 24 0.98 18.98 66.71 12.40 Comparative Example 4 0.85 12.69 44.65 4.83 Comparative Example 5 0.96 13.92 51.19 6.82 Comparative Example 6 0.92 7.46 53.24 3.65
[0094] The foregoing examples are merely illustrative, used to explain some features of the method described in this invention. The appended claims are intended to claim the broadest possible scope, and the embodiments presented herein are demonstrated by the applicant's actual experimental results. Therefore, the applicant intends that the appended claims are not limited by the selection of examples illustrating the features of the invention. Some numerical ranges used in the claims are also included therein.
[0095] Sub-scopes, and variations within these scopes, should also be interpreted, where possible, as being covered by the appended claims.
Claims
1. A method for preparing RP-type two-dimensional perovskite thin films, characterized in that, Includes the following steps: S1. Preparation of organic spacer cations: Hydroiodic acid and solvent are mixed, and an alicyclic amine compound is added in an ice-water bath and stirred to react. The solvent is removed, and the reaction is post-treated to obtain organic spacer cations. The alicyclic amine compound is R-CH2-NH2, wherein R is selected from cycloalkyl groups containing 3 to 6 carbon atoms. S2. Preparation of precursor solution: The organic spacer cation, formamidinium hydroiodate, methyl iodide, and lead iodide are mixed in a molar ratio of 2:3.6:0.4:5, and added to a mixed solvent of dimethyl sulfoxide and N,N-dimethylformamide. The mixture is stirred until completely dissolved to obtain a perovskite precursor solution. The molar ratio of formamidinium hydroiodate to methyl iodide is 0.5:0.5 to 0.92:0.
08. The molar concentration of lead ions in the perovskite precursor solution is 1.05 to 1.5 mol / L. S3. Preparation of RP-type two-dimensional perovskite thin film: The perovskite precursor solution is prepared by solution spin coating to obtain the RP-type two-dimensional perovskite thin film.
2. The preparation method according to claim 1, characterized in that, The alicyclic amine compound is selected from cyclopropylmethylamine, cyclobutylmethylamine, cyclopentylmethylamine, or cyclohexylmethylamine; the molar concentration of lead ions in the perovskite precursor solution is 1.1–1.4 mol / L.
3. The preparation method according to claim 2, characterized in that, The alicyclic amine compound is cyclopropylmethylamine; the molar concentration of lead ions in the perovskite precursor solution is 1.1–1.2 mol / L.
4. The preparation method according to claim 3, characterized in that, The molar ratio of hydroiodic acid to alicyclic amine compound is 1:1 to 1.
05.
5. The preparation method according to claim 4, characterized in that, The volume ratio of dimethyl sulfoxide to N,N-dimethylformamide is 2:3 to 12; the molar ratio of formamidinium hydroiodate to methyl iodide is 0.7:0.3 to 0.9:0.
1.
6. The preparation method according to claim 5, characterized in that, The volume ratio of dimethyl sulfoxide to N,N-dimethylformamide is 2:3 to 8; the molar ratio of formamidinium hydroiodate to methyl iodide is 0.7:0.1 to 0.9:0.
1.
7. The preparation method according to claim 6, characterized in that, The solvent spin coating method includes: spin coating the perovskite precursor solution onto the front electrode, then adding an antisolvent, and annealing at 110-130°C to crystallize the perovskite and form the RP-type two-dimensional perovskite film.
8. The RP-type two-dimensional perovskite thin film prepared by the preparation method according to any one of claims 1 to 7.
9. A perovskite solar cell, characterized in that, The perovskite solar cell comprises, from bottom to top: a front electrode, a light-absorbing layer, and a metal electrode; or the perovskite solar cell comprises, from bottom to top: a front electrode, a hole transport layer, a light-absorbing layer, an electron transport layer, an interface modification layer, and a metal electrode. The light-absorbing layer is an RP-type two-dimensional perovskite thin film prepared by the preparation method according to any one of claims 1 to 7.
10. The perovskite solar cell according to claim 9, characterized in that: The hole transport layer is made of PEDOT:PSS; the electron transport layer is made of C60; the interface modification layer is made of BCP; and the metal electrode is made of Ag.
Citation Information
Patent Citations
Quasi-two-dimensional perovskite solar cell doped with three-dimensional perovskite and preparation method thereof
CN113078267A
Two-dimensional perovskite thin film material, solar cell and preparation method of two-dimensional perovskite thin film material
CN113285027A