Process for producing polyacrylonitrile-based fibers with controlled morphology

By using polymer blends to control the structure and porosity of carbon fibers, the problem of declining fiber mechanical properties in existing technologies has been solved, and polymer recycling has been achieved, thereby improving the quality of carbon fibers.

CN116670341BActive Publication Date: 2026-11-24CYTEC IND INC
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202180086827.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-12-23
Filing Date
2021-12-08
Publication Date
2026-11-24
Estimated Expiration
2041-12-08

AI Technical Summary

Technical Problem

Existing technologies struggle to effectively control the structure and porosity of carbon fibers, leading to a decline in mechanical properties. Furthermore, the sacrificial polymer cannot be recovered during oxidation and carbonization, impacting the quality of both the fiber and the carbon fiber itself.

Method used

By forming polymer blends, polymer A and polymer B are co-precipitated in different liquids, followed by selective removal of polymer B to control fiber morphology, and polymer B is recovered before oxidation and carbonization to avoid damage to mechanical properties.

Benefits of technology

It enables the production of fibers with controlled morphology, improves the mechanical properties of carbon fibers, and allows polymer B to be recycled and reused, reducing damage to fibers and carbon fibers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004297035240000101
    Figure BDA0004297035240000101
  • Figure BDA0004297035240000111
    Figure BDA0004297035240000111
Patent Text Reader

Abstract

This disclosure generally relates to a method for producing polymer fibers, typically polyacrylonitrile-based fibers, wherein the morphology of the fibers is controlled by forming polymer blends with polyacrylonitrile using polymer additives, and then subjecting the polymer blends to specific coagulation and washing conditions. This disclosure also relates to carbon fibers produced from polymer fibers through processing.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Cross-reference to related applications

[0002] This application claims priority to U.S. Provisional Application No. 63 / 129,891, filed December 23, 2020, the entire contents of which are incorporated herein by reference. Technical Field

[0003] This disclosure generally relates to a method for producing polymer fibers, typically polyacrylonitrile-based fibers, wherein the morphology of the fibers is controlled by forming polymer blends with polyacrylonitrile using polymer additives, and then subjecting the polymer blends to specific coagulation and washing conditions. This disclosure also relates to carbon fibers produced from polymer fibers through processing. Background Technology

[0004] Carbon fiber has been used in a variety of applications due to its desirable properties such as high strength and stiffness, high chemical resistance, and low thermal expansion. For example, carbon fiber can be formed into structural parts that combine high strength and high stiffness while being significantly lighter than metal parts with equivalent properties. Carbon fiber is increasingly being used as structural components in composite materials, particularly for aerospace and automotive applications. In particular, composite materials in which carbon fiber acts as a reinforcing material in a resin or ceramic matrix have been developed.

[0005] Over 90% of carbon fibers are derived from polyacrylonitrile (PAN)-based precursors. Typically, methods for converting PAN into carbon fibers include solvent spinning (solution spinning), coagulation, oxidation, stabilization, and then carbonization.

[0006] During solidification, a non-solvent (typically water) flows into the polymer solution and a solvent (typically DMF, DMSO, etc.) flows into the bath, thereby generating fiber filaments through back diffusion. In the first few seconds of solidification, the fiber skin and core structure are initially formed, and subsequent baths are used to draw the filaments and remove residual solvent. While polymer chains can be aligned by stretching and adding crystalline domains, it is difficult to manipulate the fiber structure (or morphology), reconstruct the skin-core structure, or establish new features after solidification. Furthermore, the carbon fiber industry is increasingly focused on introducing porosity into the fibers. Porous fibers can provide the benefit of allowing resins to penetrate deeper into the fibers and creating larger interphase regions, thereby improving the mechanical bonding and conversion properties in composites. Another potential benefit of porous fibers may be their application in gas barrier technologies, where fibers facilitate the diffusion and / or separation of gases. Porous fibers can provide lighter and denser materials suitable for advanced membranes used in greenhouse gas separation, self-supporting energy storage materials, and hydrogen production. Porous fibers also have a lower density, showing promise for the production of lighter carbon fibers and potentially as an alternative to hollow fibers.

[0007] However, porous fibers are generally considered to have poor mechanical properties due to the presence of voids and defects within them. It is possible to produce porous fibers by intentionally selecting solidification conditions that accelerate the back diffusion of the solvent and rapidly cool the fiber structure to a porous state. However, large voids formed during solidification can interfere with the fiber's tensile and drawability. Furthermore, large voids formed prematurely in the early stages of fiber spinning may amplify the defects they generate.

[0008] Known techniques for producing porous carbon fibers include physical or chemical activation, polymer blend carbonization, and templated production using nanoparticles and block copolymers. Polymer blend carbonization involves blending incompatible polymers, whose microphases separate into a) a carbon source polymer forming the matrix and b) a sacrificial polymer dispersing the pores. This sacrificial polymer is then typically burned off via pyrolysis during the process of forming the porous carbon material. Not only can the sacrificial polymer not be recycled, but the removal of this polymer during oxidation and carbonization makes the carbon material or fiber susceptible to further damage, leading to degradation of mechanical properties.

[0009] Therefore, there is a continued need to develop methods for controlling fiber structure (or morphology), such as introducing and manipulating porosity in polymer fibers while mitigating the impact on the mechanical properties of the resulting fibers and subsequently carbon fibers. This paper describes a novel strategy for controlling fiber morphology, which involves forming a polymer blend with polyacrylonitrile using polymer additives, followed by subjecting the blend to specific coagulation and washing conditions. Summary of the Invention

[0010] Advantageously, it has been found that the morphology of carbon fibers can be controlled when polymeric additives are used to form polymer blends with polyacrylonitrile. The polymer blends are then subjected to controlled coagulation and washing conditions to remove the polymeric additives in a controlled manner, thereby introducing porosity into the resulting fibers with a controlled morphology. These fibers can then be converted into carbon fibers. The polymeric additives can be recycled and reused, and because the removal of the polymer blends occurs before oxidation and carbonization, damage and degradation of mechanical properties are avoided.

[0011] In a first aspect, this disclosure relates to a method for producing polyacrylonitrile-based fibers having a controlled morphology, the method comprising:

[0012] a) Forming a homogeneous solution comprising:

[0013] Polyacrylonitrile-based polymers (polymer A),

[0014] Polymers that are different from polyacrylonitrile-based polymers (polymer B), and

[0015] A first liquid containing a solvent for polymer A.

[0016] Polymer B is soluble in the first liquid;

[0017] b) By contacting the homogeneous solution formed in step a) with a second liquid containing a solvent for polymer A and a non-solvent for polymer A, polymer A and polymer B are co-precipitated.

[0018] Polymer B is insoluble in the second liquid, thereby forming a polyacrylonitrile-based material comprising polymer A and polymer B; and

[0019] c) Selectively removing polymer B from a polyacrylonitrile-based material by contacting it with a third liquid containing a non-solvent for polymer A.

[0020] Polymer B is soluble in the third liquid.

[0021] This results in polyacrylonitrile-based fibers with controlled morphology.

[0022] In a second aspect, this disclosure relates to polyacrylonitrile-based fibers produced by the methods described herein.

[0023] In a third aspect, this disclosure relates to a method for producing carbon fiber, the method comprising:

[0024] (i) Producing polyacrylonitrile-based fibers according to the methods described herein;

[0025] (ii) The polyacrylonitrile-based fibers produced in step (i) are oxidized to form stabilized carbon fiber precursor fibers and then the stabilized carbon fiber precursor fibers are carbonized to produce carbon fibers.

[0026] In a fourth aspect, this disclosure relates to carbon fibers produced by the methods described herein.

[0027] In a fifth aspect, this disclosure relates to a composite material comprising carbon fibers produced according to the methods described herein; and a matrix resin.

[0028] In a sixth aspect, this disclosure relates to a composite article obtained by curing the composite material described herein. Detailed Implementation

[0029] As used herein, unless otherwise stated, the terms “a / an” or “the” mean “a / an or more / multiple” or “at least one / a” and are used interchangeably.

[0030] As used in this article, the term “and / or” in phrases in the form of “A and / or B” means A alone, B alone, or A and B together.

[0031] As used herein, the term "comprises" includes "consistsessentially of" and "consists of". The term "comprising" includes "consisting essentially of" and "consisting of". "Comprising", synonymous with "including", "containing", or "characterized by", is intended to be inclusive or open-ended and does not exclude additional, unlisted elements or steps. The transitional phrase "consisting essentially of" includes specific materials or steps that do not materially affect the essential characteristics or function of the described composition, process, method, or article. The transitional phrase "composed of" does not include any unspecified elements, steps, or components.

[0032] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this specification pertains.

[0033] As used herein, and unless otherwise specified, the terms “about” or “approximately” mean an acceptable error for a particular value as determined by one of ordinary skill in the art, which depends in part on how the value is measured or determined. In some embodiments, the terms “about” or “approximately” mean within 1, 2, 3, or 4 standard deviations. In some embodiments, the terms “about” or “approximately” mean within 50%, 20%, 15%, 10%, 9%, 8%, 7%, 6%, 5%, 4%, 3%, 2%, 1%, 0.5%, or 0.05% of a given value or range.

[0034] Furthermore, it should be understood that any numerical ranges listed herein are intended to include all subranges included therein. For example, the range "1 to 10" is intended to include and encompass all subranges between the listed minimum value of 1 and the listed maximum value of 10; that is, a minimum value equal to or greater than 1 and a maximum value equal to or less than 10. Because the disclosed numerical ranges are continuous, they include every value between the minimum and maximum values. Unless otherwise clearly indicated, the various numerical ranges specified in this application are approximate values.

[0035] Throughout this disclosure, different publications may be incorporated by reference. Unless otherwise specified, if the meaning of any language in such publications incorporated by reference conflicts with the meaning of the language in this disclosure, the meaning of the language in this disclosure shall prevail.

[0036] The methods described herein utilize polymer blends comprising PAN and polymeric additives designed to control morphology, typically with carefully controlled coagulation and washing conditions. Specifically, the polymeric additives will be polymers that are soluble in both non-solvent and solvent forms of PAN. Solubility in the solvent is necessary to form a homogeneous solution in the viscous spinning “dosage” prior to spinning. This is important because if both the polymeric additives and PAN are insoluble, they cannot form a blend. Solubility in the non-solvent will be unique and provides the opportunity to intentionally control the reverse diffusion kinetics of fibril formation. Furthermore, if the polymeric additives blended with PAN are soluble, for example, by altering the conditions in the coagulation or washing bath, then the polymeric additives provide the opportunity to manipulate the structure after the initial stages of coagulation.

[0037] Therefore, the first aspect of this disclosure relates to a method for producing polyacrylonitrile-based fibers having a controlled morphology, the method comprising:

[0038] a) Forming a homogeneous solution comprising:

[0039] Polyacrylonitrile-based polymers (polymer A),

[0040] Polymers that are different from polyacrylonitrile-based polymers (polymer B), and

[0041] A first liquid containing a solvent for polymer A.

[0042] Polymer B is soluble in the first liquid;

[0043] b) By contacting the homogeneous solution formed in step a) with a second liquid containing a solvent for polymer A and a non-solvent for polymer A, polymer A and polymer B are co-precipitated.

[0044] Polymer B is insoluble in the second liquid, thereby forming a polyacrylonitrile-based material comprising polymer A and polymer B; and

[0045] c) Selectively removing polymer B from a polyacrylonitrile-based material by contacting it with a third liquid containing a non-solvent for polymer A.

[0046] Polymer B is soluble in the third liquid.

[0047] This results in polyacrylonitrile-based fibers with controlled morphology.

[0048] In step a) of the method, a homogeneous solution is formed comprising a polyacrylonitrile-based polymer (polymer A), a polymer different from the polyacrylonitrile-based polymer (polymer B), and a first liquid comprising a solvent for polymer A (wherein polymer B is soluble in the first liquid).

[0049] The polyacrylonitrile-based polymer (polymer A) can be any polymer comprising repeating units derived from acrylonitrile. Suitable polyacrylonitrile-based polymers can be homopolymers composed of repeating units derived from acrylonitrile or copolymers comprising repeating units derived from acrylonitrile and one or more comonomers. Such polymers can be obtained from commercially available sources or prepared according to methods known to those skilled in the art. For example, polymer A can be prepared by any polymerization method, including but not limited to solution polymerization, dispersion polymerization, precipitation polymerization, suspension polymerization, emulsion polymerization, and variations thereof.

[0050] Polyacrylonitrile-based polymers comprise repeating units derived from acrylonitrile and at least one comonomer selected from the group consisting of: vinyl-based acids, vinyl-based esters, vinyl amides, vinyl halides, ammonium salts of vinyl compounds, sodium salts of sulfonic acids, and mixtures thereof.

[0051] In one embodiment, the polyacrylonitrile-based polymer comprises repeating units derived from acrylonitrile and at least one comonomer selected from the group consisting of: methacrylic acid (MAA), acrylic acid (AA), itaconic acid (ITA), methacrylate (MA), ethyl acrylate (EA), butyl acrylate (BA), methyl methacrylate (MMA), ethyl methacrylate (EMA), propyl methacrylate, butyl methacrylate, β-hydroxyethyl methacrylate, dimethylaminoethyl methacrylate, 2-ethylhexyl acrylate, isopropyl acetate, vinyl acetate (VA), vinyl propionate, vinylimidazolium (VIM), acrylamide (AAm), diacetone acrylamide (DAAm), allyl chloride, vinyl bromide, vinyl chloride, vinylidene chloride, sodium vinyl sulfonate, sodium p-styrene sulfonate (SSS), sodium methyl allyl sulfonate (SMS), sodium 2-acrylamido-2-methylpropane sulfonate (SAMPS), and mixtures thereof.

[0052] There are no particular limitations on the comonomer ratio (the amount of one or more comonomers relative to the amount of acrylonitrile). However, suitable comonomer ratios are 0 to 20%, typically 1% to 5%, and more typically 1% to 3%.

[0053] The molecular weight of the polyacrylonitrile-based polymer suitable for use according to the method can be in the range of 60 to 500 kg / mol, typically 90 to 250 kg / mol, and more typically 115 to 180 kg / mol.

[0054] The first liquid contains a solvent for polymer A. Meanwhile, polymer B is soluble in the first liquid.

[0055] As used herein, the term "solvent" means any compound that, at the temperature at which the solvent is used, is generally able to completely dissolve the corresponding polymer. Conversely, the term "non-solvent" means any compound that, at the temperature at which the non-solvent is used, is not able to dissolve the corresponding polymer. Those skilled in the art will understand that solvents and non-solvents (typically miscible) can combine to form a liquid in which the solubility of the corresponding polymer differs from its solubility in either the solvent alone or the non-solvent alone.

[0056] As used herein, the term "soluble" when used to describe a material means that 1% or more, typically 5% or more, of a material relative to a particular solvent or liquid by weight is soluble in said solvent or liquid. As used herein, the term "insoluble" when used to describe a material means that less than 1% or more, typically less than 0.5%, of a material relative to a particular non-solvent or liquid by weight by weight is soluble in said non-solvent or liquid.

[0057] Suitable solvents for polymer A may be selected from the group consisting of: dimethyl sulfoxide (DMSO), dimethylformamide (DMF), dimethylacetamide (DMAc), ethylene carbonate (EC), N-methyl-2-pyrrolidone (NMP), zinc chloride (ZnCl2) / water, sodium thiocyanate (NaSCN) / water, and mixtures thereof, typically selected from the group consisting of: dimethyl sulfoxide (DMSO), dimethylformamide (DMF), dimethylacetamide (DMAc), ethylene carbonate (EC), and N-methyl-2-pyrrolidone (NMP).

[0058] In step a), the temperature of the first liquid is maintained above room temperature, i.e., greater than 25°C. In one embodiment, the temperature of the first liquid is about 40°C to about 85°C.

[0059] The resulting homogeneous solution is typically free of gelling and / or agglomerated polymers. The presence of gelling and / or agglomerated polymers can be determined using any method known to those skilled in the art. For example, the Hegman gauge can be used to determine the presence of gelling and / or agglomerated polymers. The prepared homogeneous solution is generally stable and does not exhibit gel formation over time.

[0060] Based on the total weight of the solution, a homogeneous solution may have a polymer concentration of at least 10 wt%, typically from about 16 wt% to about 28 wt%, and more typically from about 19 wt% to about 24 wt%.

[0061] Step b) involves contacting the homogeneous solution formed in step a) with a second liquid containing a solvent for polymer A and a non-solvent for polymer A to co-precipitate polymer A and polymer B, wherein polymer B is insoluble in the second liquid, thereby forming a polyacrylonitrile-based material containing polymer A and polymer B.

[0062] The second liquid contains a solvent for polymer A and a non-solvent for polymer A, and polymer B is insoluble in the second liquid. Therefore, when the homogeneous solution formed in step a) is brought into contact with the second liquid, polymer A and polymer B co-precipitate in the form of a polyacrylonitrile-based material, which is typically in solid form, such as a membrane, discrete particles, fibers, etc.

[0063] The second liquid used in this method is a mixture of solvent and non-solvent for polymer A. Suitable solvents include those described herein. In one embodiment, dimethyl sulfoxide, dimethylformamide, dimethylacetamide, or mixtures thereof are used as the solvent. In another embodiment, dimethyl sulfoxide is used as the solvent.

[0064] The non-solvent used for polymer A can be any compound known to those skilled in the art that does not dissolve polymer A at the temperature used. Exemplary non-solvents used for polymer A include water and C1-C6 alkanols such as methanol, ethanol, n-propanol, isopropanol, etc. In one embodiment, the non-solvent used for polymer A is water.

[0065] The ratio of solvent to non-solvent and the temperature are not particularly limited and can be adjusted according to known methods to achieve the desired curing rate. However, the second liquid suitably contains less than or equal to 85 wt% of the solvent for polymer A and more than or equal to 15 wt% of the non-solvent for polymer A relative to the total weight of the second liquid.

[0066] In another embodiment, the second liquid comprises 40 wt% to 85 wt% of one or more solvents, with the balance being a non-solvent. In one embodiment, the second liquid comprises 40 wt% to 70 wt% of one or more solvents, with the balance being a non-solvent. In yet another embodiment, the second liquid comprises 50 wt% to 85 wt% of one or more solvents, with the balance being a non-solvent.

[0067] Typically, the temperature of the second liquid is from 0°C to 80°C. In one embodiment, the temperature of the second liquid is from 30°C to 80°C. In another embodiment, the temperature of the second liquid is from 0°C to 20°C.

[0068] In an embodiment, step b) includes spinning or incorporating the homogeneous solution formed in step a) into a coagulation bath containing a second liquid to form a polyacrylonitrile-based material as one or more fibers, the second liquid containing a solvent for polymer A and a non-solvent for polymer A.

[0069] In this embodiment, a homogeneous solution is spun or spun into a coagulation bath. After removing air bubbles by vacuum, the homogeneous solution (“spin dope”) can undergo conventional wet spinning and / or air-gap spinning. In wet spinning, the dope is filtered and extruded through orifices in a spinneret (typically made of metal) into a liquid coagulation bath for the polymer to form filaments. The spinneret orifices determine the desired fiber count (e.g., 3,000 orifices for 3K carbon fibers). In air-gap spinning, a vertical air gap of 1 to 50 mm, typically 2 to 10 mm, is provided between the spinneret and the coagulation bath. In one embodiment, the polymer solution is filtered and extruded from the spinneret in air, and the extruded filaments are then coagulated in a coagulation bath.

[0070] The solvent used for polymer A in the first liquid and the solvent used for polymer A in the second liquid may be the same or different and each may be selected from the group consisting of: dimethyl sulfoxide (DMSO), dimethylformamide (DMF), dimethylacetamide (DMAc), ethylene carbonate (EC), N-methyl-2-pyrrolidone (NMP), zinc chloride (ZnCl2) / water, sodium thiocyanate (NaSCN) / water, and mixtures thereof, typically selected from the group consisting of: dimethyl sulfoxide (DMSO), dimethylformamide (DMF), dimethylacetamide (DMAc), ethylene carbonate (EC), and N-methyl-2-pyrrolidone (NMP).

[0071] In one embodiment, the solvent used for polymer A in the first liquid and the solvent used for polymer A in the second liquid are the same.

[0072] In step c), polymer B is selectively removed from the polyacrylonitrile-based material by contacting it with a third liquid containing a non-solvent for polymer A (in which polymer B is soluble).

[0073] The third liquid contains a non-solvent for polymer A, but makes polymer B soluble in the third liquid. Therefore, in step c), polymer B can be selectively removed from the PAN polymer fibers to produce polyacrylonitrile-based fibers with a controlled morphology.

[0074] The temperature of the third liquid ranges from 0°C to 100°C, typically from 0°C to 30°C, and more typically from 10°C to 25°C.

[0075] The non-solvent used for polymer A in the second liquid and the non-solvent used for polymer A in the third liquid may be the same or different. In one embodiment, the non-solvent used for polymer A in the second liquid and the non-solvent used for polymer A in the third liquid are the same.

[0076] In one embodiment, the non-solvent used for polymer A in the second liquid and the non-solvent used for polymer A in the third liquid are both water.

[0077] In one embodiment, the first liquid consists of a solvent for polymer A.

[0078] In another embodiment, the second liquid consists of a solvent for polymer A and a non-solvent for polymer A.

[0079] In yet another embodiment, the third liquid consists of a non-solvent for polymer A.

[0080] In an embodiment, step c) includes drawing one or more fibers by one or more drawing and washing baths, wherein at least one bath contains the third liquid containing a non-solvent for polymer A.

[0081] The stretching of the coagulated polymer fibers is performed by conveying the fibers through one or more stretching and washing baths, for example, by rollers. As a first step in controlling the carbon diameter, the coagulated polymer fibers are conveyed through one or more washing baths to remove any excess solvent, followed by stretching in a hot water bath (e.g., 40°C to 100°C) to impart molecular orientation to the filaments. The resulting stretched polymer fibers are substantially solvent-free.

[0082] Therefore, in one embodiment, step c) includes drawing one or more fibers through multiple drawing and washing baths, wherein the first bath contains a third liquid containing a non-solvent for the polymer, and wherein the temperature of the first bath is from 0°C to 30°C, typically from 10°C to 25°C. The first bath refers to the bath immediately following the bath used in step b). The bath following the first bath can have a temperature up to 100°C.

[0083] The polymer additive, i.e., polymer B, which is combined with polymer A to form a homogeneous solution in the methods described herein, is a polymer different from polymer A. A suitable polymer for use as polymer B is a polymer that is soluble in the first liquid, insoluble in the second liquid, and soluble in the third liquid at the temperature used, and can be a homopolymer or copolymer. A suitable polymer is a polymer comprising repeating units of one or more monomers derived from at least one monomer according to formula (I):

[0084]

[0085] in:

[0086] R 1 It is H or methyl.

[0087] R 2 and R 3 Each is independently H or alkyl, typically H or (C1-C6) alkyl.

[0088] As used herein, the term “Cx-Cy” or “(Cx-Cy)” for organic groups, where x and y are each integers, means that each group may contain from x carbon atoms to y carbon atoms.

[0089] As used herein, the term "alkyl" refers to a monovalent straight-chain or branched saturated hydrocarbon group, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, pentyl, hexyl, etc.

[0090] As used herein, the term "derived from" means that the repeating units in the polymer are formed by polymerization of the monomers described herein according to methods well known to those skilled in the art. Optionally, the polymer may have undergone subsequent chemical modification. For example, polymers produced by polymerization of acyl-containing monomers can be hydrolyzed to form polymers with hydroxyl groups.

[0091] In one embodiment, polymer B is a homopolymer derived from a monomer according to formula (I).

[0092] In another embodiment, polymer B is poly(N-isopropylacrylamide).

[0093] In one embodiment, polymer B is a copolymer comprising monomeric units derived from monomers according to formula (I), more typically wherein repeating units of the polymer are derived from monomers according to formula (I) by a weight percentage (“wt%”) greater than or equal to about 50 wt%.

[0094] Another suitable polymer is a polymer comprising repeating units of one or more monomers derived from at least one monomer according to formula (II):

[0095]

[0096] in:

[0097] R 4 It is H or methyl.

[0098] R 5 It is H, alkyl, or acyl, typically H or acyl.

[0099] As used herein, the term "acyl" refers to a substituent characterized by the formula -(C=O)-R, where R is an alkyl group.

[0100] In one embodiment, polymer B is a homopolymer derived from a monomer according to formula (II).

[0101] In another embodiment, polymer B is polyvinyl alcohol.

[0102] In another embodiment, polymer B is a copolymer comprising monomer units derived from monomers according to formula (II), more typically wherein repeating units of the polymer are derived from monomers according to formula (II) by a weight percentage (“wt%”) greater than or equal to about 50 wt%.

[0103] In step a), there is no particular limitation on the amount of polymer B that binds to polymer A to form a homogeneous solution. However, suitable results are obtained when the homogeneous solution contains less than or equal to 50 wt%, typically less than or equal to 20 wt%, and more typically less than or equal to 10 wt% of polymer B relative to the total weight of the homogeneous solution.

[0104] The method may further include step d), for example, drying substantially solvent-free drawn polymer fibers on drying rollers. The drying rollers may consist of multiple rotatable rollers arranged in a serpentine configuration, above which filaments pass sequentially from roller to roller under sufficient tension to provide filament stretching or relaxation on the rollers. At least some of the rollers are heated by pressurized steam, which circulates internally or via electrically heated elements within the rollers. Prior to drying, finishing oil may be applied to the drawn fibers to prevent the filaments from sticking together during downstream processes.

[0105] The method disclosed herein can be performed continuously or in batches. As used herein, a "continuous" method means in which fibers are conveyed through one or more processing steps, one single work unit at a time, without any interruption in time, material, or sequence. This contrasts with a batch method, which should be understood as a method comprising a series of one or more steps performed in a defined sequence, and whereby a limited quantity of material is processed or produced at the end of the sequence, and the sequence must be repeated to process or produce another batch of material. In one embodiment, the method is performed continuously.

[0106] Advantageously, the polymer additive (polymer B) can be recovered and recycled. The ability to recover polymer B from this method provides an advantage over a "sacrificial polymer" that volatilizes during pyrolysis and is lost during downstream carbon fiber formation. Therefore, in one embodiment, the method further includes step e) at least partially recovering polymer B. Polymer B can be recovered from any step of this method using any separation method known to those skilled in the art. For example, polymer B can be recovered from any liquid described herein using vacuum distillation, thin-film evaporation, etc.

[0107] In a second aspect, this disclosure relates to polyacrylonitrile-based fibers produced by the methods described herein. The polyacrylonitrile-based fibers produced by the methods described herein can be used as precursor fibers (so-called white fibers) for the production of carbon fibers.

[0108] Therefore, in a third aspect, this disclosure relates to a method for producing carbon fiber, the method comprising:

[0109] (i) Producing polyacrylonitrile-based fibers according to the methods described herein;

[0110] (ii) The polyacrylonitrile-based fibers produced in step (i) are oxidized to form stabilized carbon fiber precursor fibers and then the stabilized carbon fiber precursor fibers are carbonized to produce carbon fibers.

[0111] After producing polyacrylonitrile-based fibers according to the methods described herein, the polyacrylonitrile-based fibers can be oxidized to form stabilized carbon fiber precursor fibers, and the stabilized carbon fiber precursor fibers can then be carbonized to produce carbon fibers.

[0112] During the oxidation stage, polymer fibers are fed under tension through one or more dedicated ovens, each with a temperature ranging from 150°C to 300°C, typically from 200°C to 280°C, and more typically from 220°C to 270°C, wherein heated air is fed into each oven.

[0113] The oxidation process combines oxygen molecules from the air with the fiber and initiates cross-linking of the polymer chains, thereby increasing the fiber density to 1.30 g / cm³. 3 Up to 1.45 g / cm 3 This type of oxidized PAN fiber has an infusible ladder-shaped aromatic molecular structure and is ready for carbonization.

[0114] Carbonization leads to the crystallization of carbon molecules and thus produces finished carbon fibers with a carbon content greater than 90%. The carbonization of oxidized or stabilized carbon fiber precursor fibers occurs in an inert (oxygen-free) atmosphere, typically a nitrogen atmosphere, within one or more specially designed furnaces. The oxidized carbon fiber precursor fibers are then passed through one or more ovens, each heated to a temperature ranging from 300°C to 1650°C, typically from 1100°C to 1450°C.

[0115] The adhesion between the matrix resin and carbon fibers is a crucial standard in carbon fiber reinforced polymer composites. Therefore, during the manufacturing process of carbon fibers, surface treatments can be performed after oxidation and carbonization to enhance this adhesion.

[0116] Surface treatment may involve traction carbonized fibers through an electrolytic bath containing an electrolyte such as ammonium bicarbonate or sodium hypochlorite. The chemicals in the electrolytic bath etch or roughen the fiber surface, thereby increasing the surface area available for interfacial fiber / matrix bonding and adding reactive chemical groups.

[0117] Next, the carbon fibers can be subjected to sizing, in which a sizing coating (e.g., an epoxy-based coating) is applied to the fibers. Sizing can be performed by passing the fibers through a sizing bath containing a liquid coating material. Sizing protects the carbon fibers during processing and finishing into intermediate forms such as dry fabrics and prepregs. Sizing also holds the filaments together in individual bundles to reduce fuzz, improve processability, and increase the interfacial shear strength between the fibers and the matrix resin.

[0118] After applying the adhesive, the coated carbon fiber is dried and then wound onto a winding tube.

[0119] Those skilled in the art will understand that processing conditions (including the composition of the spinning solution and coagulation bath, the total bath volume, stretching, temperature, and filament speed) are correlated to provide filaments with desired structure and denier.

[0120] In a fourth aspect, this disclosure relates to carbon fibers produced by the methods described herein.

[0121] Carbon fibers produced according to the methods described herein can be characterized by mechanical properties such as tensile strength and tensile modulus obtained according to ASTM D4018 test methods.

[0122] The produced carbon fibers typically have tensile strengths ranging from 300 to 1000 ksi, with a typical range of 400 to 600 ksi.

[0123] The produced carbon fibers typically have a tensile modulus of 30 to 50 msi, typically 35 to 40 msi.

[0124] The produced carbon fibers can be characterized by their density. Typically, carbon fibers formed according to the methods described herein have a lower density than conventional carbon fibers. Advantageously, this disclosure provides low-density, lightweight carbon fibers. The density of carbon fibers produced according to this disclosure can be less than or equal to 1.80 g / cm³. 3 Typically less than or equal to 1.79 g / cm³ 3 More typically less than or equal to 1.78 g / cm³ 3 In one embodiment, the density is from 1.50 to 1.77 g / cm³. 3 In another embodiment, the density is from 1.70 to 1.77 g / cm³. 3 Or from 1.74 to 1.79 g / cm³ 3 .

[0125] The carbon fibers produced herein are suitable for use in the production of composite materials. Therefore, in a fifth aspect, this disclosure relates to a composite material comprising carbon fibers produced according to the methods described herein and a matrix resin.

[0126] Composite materials can be manufactured by molding preforms containing carbon fibers produced according to the methods described herein and by infusing the preforms with thermosetting resins in a variety of liquid molding methods. Liquid molding methods that can be used include, but are not limited to, vacuum-assisted resin transfer molding (VARTM), in which resin is infused into the preform using a pressure differential created by a vacuum. Another method is resin transfer molding (RTM), in which resin is infused into the preform under pressure in a closed mold. A third method is resin film infusion (RFI), in which a semi-solid resin is placed under or on top of the preform, suitable tools are placed on the part, the part is bagged, and then placed in an autoclave to melt and infuse the resin into the preform.

[0127] The matrix resin used for impregnating or potting the preforms described herein is a curable resin. In this disclosure, "curing" refers to the hardening of a polymer material through the chemical crosslinking of polymer chains. The term "curable" in relation to a composition means that the composition can withstand conditions that will cause the composition to reach a hardened or thermosetting state. The matrix resin is typically a curable or thermosetting resin comprising one or more uncured thermosetting or thermoplastic resins. Suitable thermosetting resins include, but are not limited to, epoxy resins, oxetanes, imides (such as polyimides or bismaleimides), vinyl ester resins, cyanate ester resins, isocyanate-modified epoxy resins, phenolic resins, furan resins, benzoxazine, formaldehyde condensation resins (such as those with urea, melamine, or phenol), polyesters, acrylic resins, mixtures therewith, blends, and combinations thereof. Suitable thermoplastic resins include, but are not limited to, polyolefins, fluoropolymers, perfluorosulfonic acids, polyamide-imides, polyamides, polyesters, polyketides, polyphenylene sulfides, polyvinylidene chloride, sulfone polymers, their hybrids, their blends, and combinations thereof.

[0128] Suitable epoxy resins include glycidyl derivatives of aromatic diamines, aromatic monoamines, aminophenols, polyphenols, polyols, and polycarboxylic acids, and non-glycidyl resins produced by the peroxidation of olefin double bonds. Examples of suitable epoxy resins include polyglycidyl ethers of bisphenols such as bisphenol A, bisphenol F, bisphenol S, bisphenol K, and bisphenol Z; polyglycidyl ethers of cresol and phenolic phenolic varnishes; glycidyl ethers of phenolic adducts; glycidyl ethers of aliphatic diols; diglycidyl ethers; diethylene glycol diglycidyl ethers; aromatic epoxy resins; aliphatic polyglycidyl ethers; epoxidized olefins; brominated resins; aromatic glycidyl amines; heterocyclic glycidyl imides and amides; glycidyl ethers; fluorinated epoxy resins; or combinations thereof.

[0129] Specific examples include tetraglycidyl derivatives of 4,4'-diaminodiphenylmethane (TGDDM), resorcinol diglycidyl ether, triglycidyl-p-aminophenol, triglycidyl-m-aminophenol, bromobisphenol F diglycidyl ether, tetraglycidyl derivatives of diaminodiphenylmethane, trihydroxyphenylmethane triglycidyl ether, polyglycidyl ether of phenol-formaldehyde phenolic varnish, polyglycidyl ether of o-cresol phenolic varnish, or tetraglycidyl ether of tetraphenylethane.

[0130] Suitable oxetane compounds are those containing at least one oxetane group per molecule, including compounds such as 3-ethyl-3-[[(3-ethyloxetane-3-yl)methoxy]methyl]oxetane, oxetane-3-methanol, 3,3-bis-(hydroxymethyl)oxetane, 3-butyl-3-methyloxetane, 3-methyl-3-oxetanemethanol, 3,3-dipropyloxetane, and 3-ethyl-3-(hydroxymethyl)oxetane.

[0131] The curable matrix resin may optionally contain one or more additives, such as curing agents, curing catalysts, comonomers, rheology control agents, tackifiers, inorganic or organic fillers, thermoplastic and / or elastomeric polymers as toughening agents, stabilizers, inhibitors, pigments, dyes, flame retardants, reactive diluents, UV absorbers, and other additives known to those skilled in the art for modifying the properties of the matrix resin before and / or after curing.

[0132] Examples of suitable curing agents include, but are not limited to, aromatic, aliphatic, and alicyclic amines, or guanidine derivatives. Suitable aromatic amines include 4,4'-diaminodiphenyl sulfone (4,4'-DDS), 3,3'-diaminodiphenyl sulfone (3,3'-DDS), 1,3-diaminobenzene, 1,4-diaminobenzene, 4,4'-diaminodiphenylmethane, and phenylenediamine (BDA); suitable aliphatic amines include ethylenediamine (EDA), 4,4'-methylenebis(2,6-diethylaniline) (M-DEA), m-xylenediamine (mXDA), diethylenetriamine (DETA), triethylenetetramine (TETA), trioxanetridecanediamine (TTDA), polyoxypropylenediamine, and other homologs. Compounds; alicyclic amines, such as diaminocyclohexane (DACH), isophorone diamine (IPDA), 4,4'-diaminodicyclohexylmethane (PACM), bis(aminopropyl)piperazine (BAPP), N-aminoethylpiperazine (N-AEP); other suitable curing agents include acid anhydrides, typically polycarboxylic acid anhydrides, such as nadic anhydride, methyl nadic anhydride, phthalic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, methylene-tetrahydrophthalic anhydride, pyromellitic dianhydride, chloroendic anhydride, and trimellitic anhydride.

[0133] Other curing agents are Lewis acid: Lewis base complexes. Suitable Lewis acid: Lewis base complexes include, for example, complexes of the following: BCl3:amine complexes; BF3:amine complexes, such as BF3:monoethylamine, BF3:propylamine, BF3:isopropylamine, BF3:benzylamine, BF3:chlorobenzylamine, BF3:trimethylamine, BF3:pyridine, BF3:THF; AlCl3:THF; AlCl3:acetonitrile; and ZnCl2:THF.

[0134] Additional curing agents include polyamides, polyamines, amide-based amines, polyamide-based amines, alicyclic compounds, polyetheramides, imidazoles, dicyandiamides, substituted ureas and urea-ketones, hydrazines, and silicones.

[0135] Urea-based curing agents are a range of materials available under the trade name DYHARD (sold by Alzchem), as well as urea derivatives, such as those commercially available as UR200, UR300, UR400, UR600, and UR700. Urea-ketone accelerators include, for example, 4,4-methylenediphenyl bis(N,N-dimethylurea) (available from Onmicure as U52 M).

[0136] When a curing agent is present, the total amount of the curing agent ranges from 1 wt% to 60 wt% of the resin composition. Typically, the curing agent is present in the range of 15 wt% to 50 wt%, more typically in the range of 20 wt% to 30 wt%.

[0137] Suitable toughening agents may include, but are not limited to, homopolymers or copolymers alone or in combination with the following: polyamides, copolyamides, polyimides, aromatic polyamides, polyketides, polyetherimides (PEI), polyetherketones (PEK), polyetherketoneketones (PEKK), polyetheretherketones (PEEK), polyethersulfones (PES), polyetherethersulfones (PEES), polyesters, polyurethanes, polysulfones, polysulfides, polyphenylene oxide (PPO) and modified PPO, poly(ethylene oxide) (PEO) and polypropylene oxide, polystyrene, polybutadiene, polyacrylates, polystyrene, polymethyl methacrylates, polyacrylates, polyphenylene sulfones, high-performance hydrocarbon polymers, liquid crystal polymers, elastomers, segmental elastomers and core-shell particles.

[0138] When toughening particles or toughening agents are present, they may be present in the range of 0.1 wt% to 30 wt% of the resin composition. In one embodiment, the toughening particles or toughening agents may be present in the range of 10 wt% to 25 wt%. In another embodiment, the toughening particles or toughening agents may be present in the range of 0.1 to 10 wt%. Suitable toughening particles or toughening agents include, for example, Virantage VW10200 FRP, VW10300 FP, and VW10700 FRP from Solvay, BASF Ultrason E2020, and Sumikaexcel5003P from Sumitomo Chemicals.

[0139] The toughening particles or toughening agents can be in the form of particles with a diameter greater than 20 micrometers to prevent them from binding into the fiber layer. The size of the toughening particles or toughening agents can be selected so that they are not filtered by the fiber reinforcement material. Optionally, the composition may also include inorganic ceramic particles, microspheres, microspheres, and clay.

[0140] The resin composition may also contain conductive particles, such as those described in PCT International Publications WO 2013 / 141916, WO 2015 / 130368 and WO 2016 / 048885.

[0141] The mold used for resin infusion can be a two-component closed mold or a vacuum-sealed single-sided mold. After the matrix resin is poured into the mold, the mold is heated to cure the resin.

[0142] During heating, the resin reacts with itself to form crosslinks within the matrix of the composite material. After an initial heating period, the resin gels. After gelation, the resin no longer flows but becomes solid. Following gelation, the temperature or curing temperature can be gradually increased to a final temperature to complete curing. The final curing temperature depends on the properties and characteristics of the selected thermosetting resin. Therefore, in a suitable method, the composite material is heated to a first temperature suitable for gelling the matrix resin, and then the temperature is gradually increased to a second temperature and held at that second temperature for a certain period to complete curing. This yields the composite article.

[0143] The following non-limiting examples further illustrate the methods disclosed herein and the carbon fibers produced therefrom.

[0144] Example

[0145] Example 1. PAN / pNIPAM membrane

[0146] A polyacrylonitrile-based polymer with repeating units derived from methacrylic acid (MAA) was used. Poly(N-isopropylacrylamide) (pNIPAM; available from Sigma-Aldrich with a number-average molecular weight of approximately 40,000 kDa) was used as a polymer additive. Blends of the two polymers were prepared using a Thinky AR-100 centrifuge mixer (2000 rpm) at approximately 6 g sample sizes with either 1 or 10 wt.% pNIPAM (relative to the concentration of the PAN-based polymer in DMSO, approximately 15 wt.%). Polymer membranes were prepared by spreading the solution onto a glass plate and allowing it to air dry. The membranes were then extracted using one of the following methods:

[0147] method illustrate 1 Methanol rinsing (spraying methanol onto the sample) 2 Accelerated solvent extraction (ASE) using methanol 3 Rinse with cold water (spray cold water onto the sample). 4 Cold water extraction (using room temperature water as a solvent in ASE extraction) 5 Hot water extraction (using hot water as a solvent in ASE extraction) 6 Soak in water (immerse the sample in a water bath for 2-3 hours). 7 Rinse with DMSO / water (using a 50 / 50 co-solvent mixture sprayed onto the sample).

[0148] FTIR was used to track two peaks at approximately 1540 and 1640 cm⁻¹, respectively, associated with the CN (extension) and C=O (extension) of the amide group. -1 To confirm the existence of pNIPAM. Because the peak is approximately 1640 cm⁻¹. -1 The peak overlaps with the baseline peak of polymers involving carboxylic acid functional groups, at approximately 1540 cm⁻¹. -1 Used for quantitative measurement of the presence of pNIPAM in polymers.

[0149] Compared to other extraction methods, Method 2 showed the greatest reduction in pNIPAM. Method 6 was the second most efficient extraction method. Rinse extraction (Methods 1, 3, and 7) was the least efficient and left the most pNIPAM residue. Among the methods using water, Method 6 was determined to be the most efficient in removing pNIPAM.

[0150] To further investigate the effect of temperature, 1 wt.% and 10 wt.% pNIPAM films (wt.% is relative to the PAN-based polymer) were immersed in water at 10°C or 50°C for 2–3 hours. Cold water rinsing showed a smaller peak at approximately 1540 cm⁻¹ at both loading levels. -1 .

[0151] Scanning electron microscopy (SEM) was used to examine the physical characteristics of the membrane before and after extraction. Before extraction, the membrane appeared smooth and, at higher magnification, showed a grainy texture, resembling a sponge-like network at 50,000x magnification. After extraction, lower magnification images revealed numerous surface features not present on the control membrane. The surface was riddled with small indentations or pores left after extracting pNIPAM from the PAN-based polymer. At higher magnification, these surface features appeared as submicron cavities.

[0152] Example 2. PAN / pNIPAM white fiber

[0153] Polymer blends were prepared using the PAN-based polymer and polymer additives used in Example 1. The PAN-based polymer and pNIPAM (3.16 kg of PAN-based polymer and 30 g of pNIPAM in 14.49 kg of DMSO) were dissolved using a 15-gallon Myers mixer, with the disperser at 500 rpm and the scrubber at 60 rpm. The temperature was raised to 80°C and run for 2 hours before cooling to 45°C. The polymer solution (“dosage”) was then spun into a coagulation bath (65% DMSO). The coagulation bath was varied between 40°C and 50°C, and the first drawing bath was either at 60°C or cooled to below 10°C with ice. As a control, the same spinning process was performed on a PAN-based polymer without pNIPAM.

[0154] All filaments imaged using standard sample preparation techniques appeared normal and showed no signs of deviation from the control process. Optical images indicated the absence of large voids. Therefore, the introduction of 1 wt.% pNIPAM did not significantly alter the preferred solidification window in the baseline method.

[0155] However, SEM revealed significant differences in the fibrous structures at the submicron scale. For example, samples removed from the coagulation bath showed filaments with a smooth skin and an internal core structure, the latter being porous across the entire cross-section. Surprisingly, the skin surface remained intact without any signs of surface defects. Compared to standard coagulated samples, the core structure appeared more open and spongy, and in particular, the network included numerous small cavities, as previously observed in membrane structures. It was unexpected that the coagulated samples would exhibit such pronounced porosity when the bath concentration was 65 wt.% DMSO (beyond the solubility of pNIPAM), but this suggests that pNIPAM precipitates at a different rate than PAN-based polymers and undergoes phase separation upon coagulation.

[0156] The coagulated filaments were drawn, and the porous structure remained intact. When the fiber was drawn, the spongy core became denser and the skin roughened. The pore size decreased, but the core still retained many small indentations on the order of 100 nm within the structure. A higher concentration of pNIPAM in the fiber was found in the coagulation bath compared to the washing bath, and this concentration decreased after the washing step, indicating that pNIPAM was removed from the fiber during washing.

[0157] Another difference found between the pNIPAM blended fibers and the control fibers was their swelling behavior. The degree of swelling of the pNIPAM blended fibers and the control fibers was determined according to the following procedure: Samples were taken and first centrifuged at 3000 rpm for 15 minutes to remove any adhering liquid from the filament surface. The collected samples were then immersed in a glass beaker / flask containing deionized water and washed for at least 15 minutes. This washing step was then repeated at least twice with fresh deionized water to ensure complete solidification of the sample and removal of solvent. Once the final washing was complete, the samples were centrifuged again at 3000 rpm for 15 minutes and weighed to obtain the post-wash weight or W. a The sample was then placed in an air-circulating oven at 110°C for 3 hours. After drying, the sample was removed from the oven and placed in a desiccator for at least ten minutes. The dried and desiccated sample was reweighed, and the final weight was recorded as W. f Then, the degree of swelling is calculated using the following formula:

[0158] Swelling degree (%) = (W a -W f )×(100 / W f )

[0159] This method correlates fiber porosity with liquid absorption.

[0160] The swelling of the pNIPAM blend sample (183%) was much lower than that of the control sample (192%), and the same was true for the solidified sample and the first drawn sample (163% vs. 181%). This difference suggests that pNIPAM may affect the reverse diffusion kinetics of solvent entering and exiting the fiber.

[0161] Interestingly, despite noting structural differences (i.e., the presence of porosity and swelling behavior), the mechanical properties of the pNIPAM blended fibers appeared unaffected by the coagulation bath and first drawing bath conditions. Toughness, elongation, and Young's modulus remained within the range of measurements and process errors during these runs.

[0162] Example 3. Carbon fiber made from PAN / pNIPAM white fibers

[0163] PAN / pNIPAM white fibers prepared according to the procedure described in Example 2 were oxidized and carbonized to form carbon fibers. White fibers made from PAN-based polymers that do not contain pNIPAM were oxidized and carbonized to form carbon fibers. It was observed that the addition of pNIPAM did not significantly affect the mechanical properties. For six carbonization runs forming control fibers, the average tensile strength was 482 + / - 32 ksi and the average tensile strength was 39.1 + / - 0.4 Msi, while the carbon fibers made from PAN / pNIPAM white fibers exhibited tensile strengths exceeding 500 ksi and moduli exceeding 38.3 Msi. This result indicates that the presence of 1% pNIPAM does not impair the mechanical load-bearing capacity of carbon fibers made from PAN / pNIPAM blends. The density of the carbon fibers was typically 1.74 to 1.79 g / cm³. 3 .

[0164] Interestingly, cross-sectional microscopy of the carbon fibers of this invention revealed very fine pores in the fiber cross-section. These pores are all less than 100 nanometers in size and are mostly concentrated near the fiber sheath surface. This indicates that the porosity generated during spinning is retained through carbonization.

[0165] Example 4. PAN / PVOH white fiber

[0166] The spinning solution was prepared according to the procedure described in Example 2, except that pNIPAM was replaced with polyvinyl alcohol (PVOH; available from Sigma-Aldrich). The final spinning solution contained approximately 17.5 wt% solids (PAN-based polymer + pNIPAM) and approximately 5 wt.% PVOH (relative to the PAN-based polymer). The zero-shear viscosity at 45°C was approximately 56 Pa*sec.

[0167] As in Example 2, the spinning solution is spun to form PAN / PVOH white fibers, wherein the coagulation bath is set at 50°C.

[0168] Fiber samples were retrieved after solidification and after the first drawing bath. The swelling degree of the sample collected after solidification was 241%, which is significantly higher than the typical swelling degree of fibers made alone from the same PAN-based polymer (typically around 190%–200%). The swelling degree of the sample after the first drawing was 174%, which is also significantly higher than the typical swelling degree of fibers made alone from the same PAN-based polymer (typically around 120%–140%). This difference, due to the presence of pNIPAM, suggests that PVOH may influence the reverse diffusion kinetics of solvent ingress and egress from the fiber. Furthermore, compared to Example 2, the fiber sample extracted after the washing step showed fibers with even greater pore concentration and cavities throughout the fiber core, due to the higher concentration of PVOH relative to the PAN-based polymer. This significantly demonstrates that pore density and pore volume can be controlled by polymer blend concentration and polymer blend characteristics.

[0169] Example 5. Carbon fibers made from PAN / PVOH white fibers

[0170] The PAN / PVOH white fibers prepared according to the procedure described in Example 4 were oxidized and carbonized to successfully form carbon fibers.

[0171] The tensile strength is 340 + / - 12 ksi and the tensile modulus is 31 + / - 2.5 Msi (according to ASTM methods). The carbon fiber made from PAN / PVOH has a density typically between 1.70 and 1.77 g / cm³. 3 .

[0172] It will be apparent to those skilled in the art that the conditions for carrying out the methods of the present invention described herein can be optimized based on the intended application and circumstances without departing from the spirit of this disclosure.

Claims

1. A method for producing polyacrylonitrile-based fibers having a controlled morphology, the method comprising: a) Forming a homogeneous solution comprising: Polymer A based on polyacrylonitrile, Unlike polymer B, which is based on polyacrylonitrile, polymer B is poly(N-isopropylacrylamide), and A first liquid containing a solvent for polymer A. Polymer B is soluble in the first liquid; b) Spinning or incorporating the homogeneous solution into a coagulation bath containing a solvent for polymer A and a non-solvent for polymer A. Polymer B is insoluble in the second liquid, thereby forming a polyacrylonitrile-based material comprising polymer A and polymer B; and c) Contacting the polyacrylonitrile-based material leaving the coagulation bath with a bath containing a third liquid consisting of water, selectively removing polymer B from the polyacrylonitrile-based material. Polymer B is soluble in the third liquid, and the temperature of the bath is 0-30°C. This results in a polyacrylonitrile-based fiber with a controlled morphology.

2. The method according to claim 1, wherein, The solvent used for polymer A in the first liquid and the solvent used for polymer A in the second liquid are the same.

3. The method according to claim 1, wherein, The solvent used for polymer A in the first liquid and the solvent used for polymer A in the second liquid are each selected from the group consisting of: dimethyl sulfoxide (DMSO), dimethylformamide (DMF), dimethylacetamide (DMAc), ethylene carbonate (EC), N-methyl-2-pyrrolidone (NMP), zinc chloride (ZnCl2) / water, sodium thiocyanate (NaSCN) / water, and mixtures thereof.

4. The method according to claim 3, wherein, The solvent used for polymer A in the first liquid and the solvent used for polymer A in the second liquid are each selected from the group consisting of: dimethyl sulfoxide (DMSO), dimethylformamide (DMF), dimethylacetamide (DMAc), ethylene carbonate (EC), and N-methyl-2-pyrrolidone (NMP).

5. The method according to any one of claims 1-4, wherein, The non-solvent used for polymer A in the second liquid and the non-solvent used for polymer A in the third liquid are the same.

6. The method according to any one of claims 1-4, wherein, The non-solvent used for polymer A in the second liquid is water.

7. The method according to any one of claims 1-4, wherein, The first liquid is composed of the solvent used for polymer A.

8. The method according to any one of claims 1-4, wherein, The second liquid consists of the solvent used for polymer A and the non-solvent used for polymer A.

9. The method according to any one of claims 1-4, wherein, Polymer A comprises repeating units derived from acrylonitrile and at least one comonomer selected from the group consisting of: methacrylic acid (MAA), acrylic acid (AA), itaconic acid (ITA), methacrylate (MA), ethyl acrylate (EA), butyl acrylate (BA), methyl methacrylate (MMA), ethyl methacrylate (EMA), propyl methacrylate, butyl methacrylate, β-hydroxyethyl methacrylate, dimethylaminoethyl methacrylate, 2-ethylhexyl acrylate, isopropyl acetate, vinyl acetate (VA), vinyl propionate, vinylimidazolium (VIM), acrylamide (AAm), diacetone acrylamide (DAAm), allyl chloride, vinyl bromide, vinyl chloride, vinylidene chloride, sodium vinyl sulfonate, sodium p-styrene sulfonate (SSS), sodium methyl allyl sulfonate (SMS), sodium 2-acrylamido-2-methylpropane sulfonate (SAMPS), and mixtures thereof.

10. The method according to any one of claims 1-4, wherein, Step b) includes spinning or incorporating the homogeneous solution formed in step a) into a coagulation bath containing the second liquid to form a polyacrylonitrile-based material as one or more fibers, the second liquid containing a solvent for polymer A and a non-solvent for polymer A.

11. The method according to claim 10, wherein, Step c) includes drawing the one or more fibers by one or more drawing and washing baths, wherein at least one bath contains the third liquid containing a non-solvent for polymer A.

12. The method according to any one of claims 1-4, wherein, The second liquid contains less than or equal to 85 wt% of the solvent used for polymer A and more than or equal to 15 wt% of the non-solvent used for polymer A, relative to the total weight of the second liquid.

13. The method according to any one of claims 1-4, wherein, In step a), the homogeneous solution contains less than or equal to 50 wt% of polymer B relative to the total weight of the homogeneous solution.

14. The method according to claim 13, wherein, In step a), the homogeneous solution contains less than or equal to 20 wt% of polymer B relative to the total weight of the homogeneous solution.

15. The method according to claim 14, wherein, In step a), the homogeneous solution contains less than or equal to 10 wt% of polymer B relative to the total weight of the homogeneous solution.

16. The method according to any one of claims 1-4, further comprising step d) drying the polyacrylonitrile-based fiber produced in step c).

17. The method according to any one of claims 1-4, further comprising step e) at least partially recovering polymer B.

18. A polyacrylonitrile-based fiber, produced by the method according to any one of claims 1-17.

19. A method for producing carbon fiber, the method comprising: (i) Producing polyacrylonitrile-based fibers by the method according to any one of claims 1-17; (ii) The polyacrylonitrile-based fiber produced in step (i) is oxidized to form a stabilized carbon fiber precursor fiber and then the stabilized carbon fiber precursor fiber is carbonized to produce the carbon fiber.

20. A carbon fiber produced by the method according to claim 19.

21. The carbon fiber according to claim 20, wherein, Density less than or equal to 1.80 g / cm³.

22. The carbon fiber according to claim 21, wherein, The density is less than or equal to 1.79 g / cm³.

23. The carbon fiber according to claim 22, wherein, The density is less than or equal to 1.78 g / cm³.

24. The carbon fiber according to any one of claims 20-23, wherein, The density ranges from 1.50 to 1.77 g / cm³.

25. The carbon fiber according to any one of claims 20-23, wherein, The density ranges from 1.70 to 1.77 g / cm³ or from 1.74 to 1.79 g / cm³.

26. A composite material comprising carbon fibers produced by the method according to claim 19 or carbon fibers according to any one of claims 20-23; and a matrix resin.

27. A composite article obtained by curing the composite material according to claim 26.

Citation Information

Patent Citations

  • Composite materials comprising conductive NANO-fillers

    WO2013141916A2

  • Composite materials with electrically conductive and delamination resistant properties

    WO2015130368A2

  • Composite materials with high z-direction electrical conductivity

    WO2016048885A1

  • Method for manufacturing adsorption transfer fiber

    CN101696517A

  • Porous carbon fiber and composite microwave-absorbing material based thereon and preparation method of composite microwave-absorbing material

    CN102168325A