Light emitting diode epitaxial wafer and preparation method thereof, and light emitting diode

By introducing a C- and Mg co-doped InGaN layer and an N-polar C- and Mg co-doped AlInGaN layer into the epitaxial wafer of an AlGaN-based light-emitting diode, and performing NH₃ and H₂ treatments, the problem of poor ohmic contact in the P-type layer was solved, and the luminous efficiency was improved.

CN116682902BActive Publication Date: 2026-11-24JIANGXI ZHAO CHI SEMICON CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310695952.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-13
Publication Date
2026-11-24
Estimated Expiration
2043-06-13

AI Technical Summary

Technical Problem

Poor ohmic contact in the P-type layer of an AlGaN-based light-emitting diode epitaxial wafer leads to low luminous efficiency, which is difficult to improve effectively using existing methods.

Method used

The structure and surface properties of the P-type contact layer are optimized by using C and Mg co-doped InGaN layers and N-polar C and Mg co-doped AlInGaN layers, combined with NH₃ and H₂ treatments.

Benefits of technology

This significantly improves the ohmic contact characteristics and light extraction efficiency of the LED epitaxial wafer, thereby increasing luminous efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116682902B_ABST
    Figure CN116682902B_ABST
Patent Text Reader

Abstract

This invention discloses a light-emitting diode (LED) epitaxial wafer and its fabrication method, and the LED itself, relating to the field of semiconductor optoelectronic devices. The LED epitaxial wafer includes a substrate, on which a buffer layer, an undoped AlGaN layer, an N-type AlGaN layer, a multiple quantum well layer, an electron blocking layer, a P-type AlGaN layer, and a P-type contact layer are sequentially stacked. The P-type contact layer includes a C and Mg co-doped InGaN layer, wherein Mg replaces group III elements and C replaces group V elements. Implementing this invention can improve the luminous efficiency of the LED epitaxial wafer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of semiconductor optoelectronic devices, and more particularly to a light-emitting diode epitaxial wafer and its fabrication method, and a light-emitting diode. Background Technology

[0002] In AlGaN-based LED epitaxial wafers, the introduction of Al increases the activation energy of Mg dopant in the P-type layer, resulting in lower activation efficiency. Furthermore, the poor ohmic contact between the P-electrode and the P-type layer after subsequent P-electrode fabrication leads to low luminous efficiency in the AlGaN-based LED epitaxial wafer.

[0003] The commonly used method is to form a heavily doped P-type AlGaN layer on the P-type layer, but its doping concentration is still low, making it difficult to effectively improve the ohmic contact. Therefore, it is necessary to increase its thickness, but increasing the thickness will increase light absorption and reduce luminous efficiency. Summary of the Invention

[0004] The technical problem to be solved by the present invention is to provide a light-emitting diode epitaxial wafer and a method for preparing the same, which can improve the luminous efficiency of the light-emitting diode epitaxial wafer.

[0005] Another technical problem that this invention aims to solve is to provide a light-emitting diode with high luminous efficiency.

[0006] To address the aforementioned problems, this invention discloses a light-emitting diode epitaxial wafer, comprising a substrate, and sequentially stacked on the substrate a buffer layer, an undoped AlGaN layer, an N-type AlGaN layer, a multiple quantum well layer, an electron blocking layer, a P-type AlGaN layer, and a P-type contact layer; wherein the P-type contact layer comprises a C and Mg co-doped InGaN layer, wherein Mg replaces group III elements and C replaces group V elements.

[0007] As an improvement to the above technical solution, the Mg doping concentration in the C and Mg co-doped InGaN layer is 2 × 10⁻⁶. 19 cm -3 -5×10 22 cm -3 The doping concentration of C is 1×10 19 cm -3 -2×10 22 cm -3 ;

[0008] The In component in the C and Mg co-doped InGaN layer is 0.01-0.2%, and its thickness is 2nm-10nm.

[0009] As an improvement to the above technical solution, the C and Mg co-doped InGaN layer is treated with NH3 after growth to form an N polar contact surface.

[0010] As an improvement to the above technical solution, the P-type contact layer further includes an AlInGaN layer co-doped with N-polar C and Mg, wherein Mg replaces group III elements and C replaces group V elements;

[0011] The N-polar C and Mg co-doped AlInGaN layer is disposed on the C and Mg co-doped InGaN layer.

[0012] As an improvement to the above technical solution, the Mg doping concentration in the N-polar C and Mg co-doped AlInGaN layer is 2 × 10⁻⁶. 19 cm -3 -5×10 22 cm -3 The doping concentration of C is 2 × 10⁻⁶. 19 cm -3 -2×10 22 cm -3 ;

[0013] The AlInGaN layer with N polarity C and Mg co-doped has an Al content of 0-0.2% and an In content of 0.01-0.2%, and its thickness is 0.5nm-2nm.

[0014] As an improvement to the above technical solution, the N-polar C and Mg co-doped AlInGaN layer is treated with H2 after growth to form a roughened surface.

[0015] Accordingly, the present invention also discloses a method for preparing a light-emitting diode epitaxial wafer, which includes:

[0016] A substrate is provided on which a buffer layer, an undoped AlGaN layer, an N-type AlGaN layer, a multiple quantum well layer, an electron blocking layer, a P-type AlGaN layer and a P-type contact layer are sequentially formed.

[0017] The P-type contact layer includes a C and Mg co-doped InGaN layer, wherein Mg replaces group III elements and C replaces group V elements.

[0018] As an improvement to the above technical solution, the growth temperature of the C and Mg co-doped InGaN layer is 700℃-900℃, the growth pressure is 10 torr-200 torr, and the V / Ⅲ ratio is 1500-2500.

[0019] As an improvement to the above technical solution, the P-type contact layer further includes an AlInGaN layer co-doped with N polar C and Mg, with a growth temperature of 600℃-900℃, a growth pressure of 10 torr-200 torr, and a V / Ⅲ ratio of 2000-4000.

[0020] Accordingly, the present invention also discloses a light-emitting diode, which includes the light-emitting diode epitaxial wafer as described above.

[0021] Implementing this invention has the following beneficial effects:

[0022] 1. In the epitaxial wafer of the light-emitting diode of the present invention, the P-type contact layer includes an InGaN layer co-doped with C and Mg, wherein Mg replaces group III elements and C replaces group V elements, that is, both are replaced to form a P-type semiconductor, i.e., a composite P-type material, which can effectively improve the ohmic contact characteristics of the epitaxial wafer of the light-emitting diode and improve the luminous efficiency of the epitaxial wafer of the light-emitting diode.

[0023] 2. In the epitaxial wafer of the light-emitting diode of the present invention, the C and Mg co-doped InGaN layer is treated with NH3 after growth to form an N-polar surface. This provides a good foundation for the subsequent N-polar C and Mg co-doped AlInGaN layer, optimizes the combination between the two, reduces the overall thickness of the P-type contact layer, reduces light absorption, improves external quantum efficiency, and improves the luminous efficiency of the epitaxial wafer of the light-emitting diode.

[0024] 3. In the epitaxial wafer of the light-emitting diode of the present invention, the P-type contact layer further includes an N-polarity C and Mg co-doped AlInGaN layer, which is disposed on the C and Mg co-doped InGaN layer. Firstly, the use of composite doping improves the ohmic contact. Secondly, the introduction of Al increases the bandgap, reducing the light absorption loss of the ohmic contact layer material and improving the light extraction efficiency. Thirdly, the use of N-polarity results in a slightly roughened surface structure for this layer, further improving the light extraction efficiency. All three factors combined effectively improve the luminous efficiency of the light-emitting diode epitaxial wafer.

[0025] 4. In the epitaxial wafer of the light-emitting diode of the present invention, after the growth of the N-polarity C and Mg co-doped AlInGaN layer is completed, H2 etching is performed. Firstly, H2 etching can roughen the surface of the layer, improving the light extraction efficiency. Secondly, H2 etching mainly etches In atoms, reducing the number of In atoms, which further increases the bandgap of the layer, reduces light absorption, and improves the light extraction efficiency. Combined, these two factors effectively improve the luminous efficiency of the epitaxial wafer of the light-emitting diode. Attached Figure Description

[0026] Figure 1 This is a schematic diagram of the structure of a light-emitting diode epitaxial wafer in one embodiment of the present invention;

[0027] Figure 2 This is a schematic diagram of the structure of the P-type contact layer in one embodiment of the present invention;

[0028] Figure 3 This is a schematic diagram of the structure of the P-type contact layer in another embodiment of the present invention;

[0029] Figure 4 This is a flowchart of a method for preparing an epitaxial wafer for a light-emitting diode according to an embodiment of the present invention. Detailed Implementation

[0030] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be described in further detail below.

[0031] refer to Figure 1 and Figure 2 This invention discloses a light-emitting diode epitaxial wafer, comprising a substrate 1, and sequentially stacked on the substrate 1 a buffer layer 2, an undoped AlGaN layer 3, an N-type AlGaN layer 4, a multiple quantum well layer 5, an electron blocking layer 6, a P-type AlGaN layer 7, and a P-type contact layer 8. The P-type contact layer 8 comprises a C and Mg co-doped InGaN layer 81, wherein Mg replaces group III elements and C replaces group V elements. Specifically, in one embodiment of this invention, the P-type contact layer 8 is a C and Mg co-doped InGaN layer 81. In another embodiment of this invention, the P-type contact layer 8 is a stacked structure formed by multiple C and Mg co-doped InGaN layers 81, but the invention is not limited thereto.

[0032] In the C and Mg co-doped InGaN layer 81, the Mg doping concentration is 1×10⁻⁶. 19 cm -3 -9×10 22 cm -3 An example is 3×10 19 cm -3 8×10 19 cm -3 2×10 20 cm -3 7×10 20 cm -3 4×10 21 cm -3 6×10 21 cm -3 2×10 22 cm -3 Or 7×10 22 cm -3 However, it is not limited to this. Preferably, the Mg doping concentration is 2 × 10⁻⁶. 19 cm -3 -5×10 22 cm -3 .

[0033] The C doping concentration in the C and Mg co-doped InGaN layer 81 is 5 × 10⁻⁶. 18 cm -3 -5×10 22 cm-3 An example is 7×10 18 cm -3 2×10 19 cm -3 7×10 19 cm -3 3×10 20 cm -3 9×10 20 cm -3 4×10 21 cm -3 8×10 21 cm -3 Or 3×10 22 cm -3 However, it is not limited to this. Preferably, the doping concentration of C is 1×10⁻⁶. 19 cm -3 -2×10 22 cm -3 .

[0034] In the C and Mg co-doped InGaN layer 81, the proportion of In component (i.e., the molar ratio of InN) is 0.01-0.2, for example 0.05, 0.07, 0.1, 0.13, 0.15 or 0.17, but not limited to these.

[0035] The thickness of the C and Mg co-doped InGaN layer 81 is 0.5nm-20nm, with exemplary thicknesses of 1nm, 1.5nm, 3nm, 7nm, 12nm, 14nm, or 18nm, but not limited thereto. Preferably, it is 2nm-10nm.

[0036] Preferably, in one embodiment of the present invention, after the C and Mg co-doped InGaN layer 81 is grown, it is treated with NH3 to form an N polar contact surface. Specifically, it is treated at 700℃-800℃ for 50s-150s in an NH3 atmosphere.

[0037] refer to Figure 3 In one embodiment of the present invention, the P-type contact layer 8 further includes an N-polar C and Mg co-doped AlInGaN layer 82 disposed on a C and Mg co-doped InGaN layer 81, wherein Mg replaces group III elements and C replaces group V elements. Specifically, in one embodiment of the present invention, the P-type contact layer 8 includes only one N-polar C and Mg co-doped AlInGaN layer 82. In another embodiment of the present invention, the P-type contact layer 8 includes a stacked structure formed by multiple N-polar C and Mg co-doped AlInGaN layers 82.

[0038] In the C and Mg co-doped AlInGaN layer 82, the Mg doping concentration is 1×10⁻⁶.19 cm -3 -8×10 22 cm -3 An example is 3×10 19 cm -3 8×10 19 cm -3 2×10 20 cm -3 7×10 20 cm -3 4×10 21 cm -3 6×10 21 cm -3 2×10 22 cm -3 Or 7×10 22 cm -3 However, it is not limited to this. Preferably, the Mg doping concentration is 2 × 10⁻⁶. 19 cm -3 -5×10 22 cm -3 .

[0039] The C doping concentration in the C and Mg co-doped AlInGaN layer 82 is 5 × 10⁻⁶. 18 cm -3 -5×10 22 cm -3 An example is 7×10 18 cm -3 2×10 19 cm -3 7×10 19 cm -3 3×10 20 cm -3 9×10 20 cm -3 4×10 21 cm -3 8×10 21 cm -3 Or 3×10 22 cm -3 However, it is not limited to this. Preferably, the doping concentration of C is 2 × 10⁻⁶. 19 cm -3 -2×10 22 cm -3 .

[0040] In the C and Mg co-doped AlInGaN layer 82, the proportion of Al component (i.e., the molar ratio of AlN) is 0-0.2, with exemplary values ​​of 0.05, 0.07, 0.1, 0.13, 0.15, or 0.17, but not limited to these. The proportion of In component (i.e., the molar ratio of InN) in the C and Mg co-doped AlInGaN layer 82 is 0.01-0.2, with exemplary values ​​of 0.05, 0.07, 0.1, 0.13, 0.15, or 0.17, but not limited to these.

[0041] The thickness of the C and Mg co-doped AlInGaN layer 82 is 0.1 nm-5 nm, with exemplary thicknesses of 0.4 nm, 0.7 nm, 1.3 nm, 2.4 nm, 3.5 nm, 4.2 nm, or 4.6 nm, but not limited thereto. Preferably, it is 0.5 nm-2 nm.

[0042] Preferably, in one embodiment of the present invention, after the C and Mg co-doped AlInGaN layer 82 is grown, it is treated with H2 to form a roughened surface. Specifically, the treatment is carried out in an H2 atmosphere at 950℃-1100℃ for 10s-50s.

[0043] The substrate 1 can be a sapphire substrate, a silicon substrate, a Ga2O3 substrate, a SiC substrate, or a ZnO substrate, but is not limited to these. A sapphire substrate is preferred.

[0044] The buffer layer 2 is an AlN layer, but is not limited to it. The thickness of the buffer layer 2 is 30nm-100nm, with exemplary thicknesses of 42nm, 55nm, 67nm, 74nm, 85nm, or 92nm, but is not limited to it.

[0045] The thickness of the undoped AlGaN layer 3 is 1μm-3μm, with exemplary thicknesses of 1.3μm, 1.5μm, 2.1μm, 2.4μm or 2.7μm, but not limited thereto.

[0046] In this case, the N-type dopant element in the N-type AlGaN layer 4 is Si, but it is not limited to Si. The doping concentration of the N-type element in the N-type AlGaN layer 4 is 5 × 10⁻⁶. 18 cm -3 -1×10 20 cm -3 An example is 6.5 × 10 18 cm -3 8×10 18 cm -3 1.5×10 19 cm -3 5.4×10 19 cm -3 Or 8.5×10 19 cm-3 However, it is not limited to this. Specifically, the thickness of the N-type AlGaN layer 4 is 1μm-3μm, with exemplary thicknesses of 1.2μm, 1.6μm, 2.1μm, 2.4μm or 2.6μm, but it is not limited to this.

[0047] Among them, the multi-quantum well layer 5 consists of multiple Al α Ga 1-α N quantum well layer (α = 0.4-0.6) and Al β Ga 1-β A periodic structure formed by alternating N quantum barrier layers (β = 0.5-0.8) with a period number of 3-15. Among them, a single Al... α Ga 1-α The thickness of the N quantum well layer is 2nm-5nm, and the thickness of a single Al... β Ga 1-β The thickness of the N quantum barrier layer is 5nm-15nm.

[0048] Among them, electron blocking layer 6 is Al γ Ga 1-γ The N-layer (γ = 0.55-0.8) is not limited to this. Specifically, the thickness of the electron blocking layer 6 is 20nm-100nm, exemplarily 25nm, 35nm, 40nm, 55nm, 70nm, 85nm or 97nm, but not limited to this.

[0049] In this case, the P-type dopant in the P-type AlGaN layer 7 is Mg, but it is not limited to this. The doping concentration of the P-type dopant in the P-type AlGaN layer 7 is 1×10⁻⁶. 19 cm -3 -5×10 20 cm -3 An example is 2.5 × 10 19 cm -3 4.5×10 19 cm -3 6×10 19 cm -3 8×10 19 cm -3 Or 3×10 20 cm -3 However, it is not limited to this. Specifically, the thickness of the p-type AlGaN layer 7 is 200nm-500nm, with examples being 230nm, 280nm, 330nm, 350nm, 400nm, or 440nm, but not limited to this.

[0050] Accordingly, refer to Figure 4 The present invention also discloses a method for preparing a light-emitting diode epitaxial wafer, which includes the following steps:

[0051] S1: Provides a substrate;

[0052] S2: A buffer layer, an undoped AlGaN layer, an N-type AlGaN layer, a multiple quantum well layer, an electron blocking layer, a P-type AlGaN layer, and a P-type contact layer are grown sequentially on the substrate.

[0053] Specifically, step S2 includes:

[0054] S21: A buffer layer is grown on the front side of the substrate;

[0055] Specifically, AlN layers can be grown using PVD or MOCVD as buffer layers, but this is not the only option.

[0056] S22: An undoped AlGaN layer is grown on the buffer layer;

[0057] In one embodiment of the present invention, an undoped AlGaN layer is grown using MOCVD at a growth temperature of 1000℃-1200℃ and a growth pressure of 100 torr-500 torr.

[0058] S23: An N-type AlGaN layer is grown on an undoped AlGaN layer;

[0059] In one embodiment of the present invention, an N-type AlGaN layer is grown by MOCVD at a growth temperature of 1100℃-1300℃ and a growth pressure of 300 torr-500 torr.

[0060] S24: Growth of multiple quantum well layers on N-type AlGaN layers;

[0061] In one embodiment of the present invention, multiple Al atoms are periodically grown using MOCVD. α Ga 1-α N quantum well layer and Al β Ga 1-β An N-quantum barrier layer is obtained, which is a multi-quantum well layer. Among them, Al α Ga 1-α The growth temperature of the N quantum well layer is 850℃-950℃, and the growth pressure is 50 torr-300 torr. Al β Ga 1-β The growth temperature of the N quantum barrier layer is 1050℃-1150℃, and the growth pressure is 50 torr-300 torr.

[0062] S25: Growth of an electron blocking layer on a multi-quantum-well layer;

[0063] In one embodiment of the present invention, an electron blocking layer is grown by MOCVD at a growth temperature of 1000℃-1100℃ and a growth pressure of 100 torr-300 torr.

[0064] S26: A P-type AlGaN layer is grown on an electron blocking layer;

[0065] In one embodiment of the present invention, a p-type AlGaN layer is grown using MOCVD at a growth temperature of 1000℃-1100℃ and a growth pressure of 300 torr-500 torr. Higher pressure and growth temperature enhance Al diffusion.

[0066] S27: Grow a P-type contact layer on a P-type AlGaN layer;

[0067] Specifically, in one embodiment of the present invention, step S27 includes:

[0068] S271: Growing a C and Mg co-doped InGaN layer on a P-type AlGaN layer;

[0069] Specifically, one or more C and Mg co-doped InGaN layers are grown by MOCVD at 700℃-900℃, with a growth pressure of 10 torr-200 torr and a V / III ratio of 1500-2500. Based on this low-temperature and low-pressure growth, P-type doping of C and Mg can be achieved.

[0070] Preferably, in one embodiment of the present invention, after the C and Mg co-doped InGaN layer is grown, it is treated with NH3. Specifically, only NH3 is introduced into the MOCVD reaction chamber and the treatment is carried out at 700℃-800℃ for 50s-150s.

[0071] S272: An N-polar C and Mg co-doped AlInGaN layer is grown on a C and Mg co-doped InGaN layer;

[0072] Specifically, one or more C and Mg co-doped AlInGaN layers are grown by MOCVD at a growth temperature of 600℃-900℃, a growth pressure of 10 torr-200 torr, and a V / III ratio of 2000-4000. Based on this low-temperature, low-pressure growth, P-type doping of C and Mg can be achieved; based on the high V / III ratio growth conditions, the N-polar C and Mg co-doped AlInGaN layer can exhibit N-polarity.

[0073] Preferably, in one embodiment of the present invention, the C and Mg co-doped AlInGaN layer is treated with H2 after growth. Specifically, only H2 is introduced into the MOCVD reaction chamber, and the treatment is carried out at 950℃-1100℃ for 10s-50s.

[0074] The present invention will be further described below with reference to specific embodiments:

[0075] Example 1

[0076] refer to Figure 1 , Figure 2 This embodiment provides a light-emitting diode epitaxial wafer, which includes a substrate 1, a buffer layer 2, an undoped AlGaN layer 3, an N-type AlGaN layer 4, a multiple quantum well layer 5, an electron blocking layer 6, a P-type AlGaN layer 7, and a P-type contact layer 8.

[0077] In this design, substrate 1 is a sapphire substrate. Buffer layer 2 is an AlN layer with a thickness of 40 nm. Undoped AlGaN layer 3 has a thickness of 1.2 μm. N-type AlGaN layer 4 has a thickness of 2.2 μm and is doped with Si at a doping concentration of 5.5 × 10⁻⁶. 19 cm -3 .

[0078] Among them, the multi-quantum well layer 5 consists of multiple Al α Ga 1-α N quantum well layer (α = 0.42) and Al β Ga 1-β A periodic structure formed by alternating N quantum barrier layers (β = 0.6) has a period number of 10. Among them, a single Al α Ga 1-α The thickness of the N quantum well layer is 3 nm, and a single Al β Ga 1-β The thickness of the N quantum barrier layer is 10 nm.

[0079] Among them, electron blocking layer 6 is Al γ Ga 1-γ The N-layer (γ = 0.7) has a thickness of 40 nm. The p-type AlGaN layer 7 has a thickness of 320 nm and is doped with Mg at a doping concentration of 8 × 10⁻⁶. 19 cm -3 .

[0080] Among them, the P-type contact layer 8 is an InGaN layer co-doped with C and Mg, and its Mg doping concentration is 6×10⁻⁶. 21 cm -3 The doping concentration of C is 8 × 10⁻⁶. 21 cm -3 The In component accounts for 0.12%, and the thickness is 4.5 nm.

[0081] The method for fabricating the epitaxial wafer of the light-emitting diode in this embodiment includes the following steps:

[0082] (1) Provide a substrate;

[0083] (2) Grow a buffer layer on the substrate;

[0084] Among them, an AlN layer is grown by PVD as a buffer layer.

[0085] (3) An undoped AlGaN layer is grown on the buffer layer;

[0086] Specifically, undoped AlGaN layers were grown by MOCVD at a temperature of 1030℃ and a growth pressure of 200 torr.

[0087] (4) An N-type AlGaN layer is grown on an undoped AlGaN layer;

[0088] Specifically, an N-type AlGaN layer was grown by MOCVD at a growth temperature of 1200℃ and a growth pressure of 200 torr.

[0089] (5) Growth of multiple quantum well layers on N-type AlGaN layers;

[0090] Specifically, multiple Al atoms are periodically grown using MOCVD. α Ga 1-α N quantum well layer and Al β Ga 1-β An N-quantum barrier layer is obtained, which is a multi-quantum well layer. Among them, Al α Ga 1-α The N quantum well layer was grown at a temperature of 930℃ and a growth pressure of 200 torr. Al β Ga 1-β The growth temperature of the N quantum barrier layer is 1080℃, and the growth pressure is 200 torr.

[0091] (6) Grow an electron blocking layer on a multi-quantum-well layer;

[0092] Specifically, an electron blocking layer is grown by MOCVD at a growth temperature of 1080℃ and a growth pressure of 250 torr.

[0093] (7) A P-type AlGaN layer is grown on the electron blocking layer;

[0094] Specifically, a P-type AlGaN layer was grown by MOCVD at a growth temperature of 1050℃ and a growth pressure of 300 torr.

[0095] (8) Grow a P-type contact layer on a P-type AlGaN layer;

[0096] Specifically, C and Mg co-doped InGaN layers were grown by MOCVD at a growth temperature of 740℃, a growth pressure of 50 torr, and a V / Ⅲ ratio of 1800.

[0097] Example 2

[0098] This embodiment provides a light-emitting diode epitaxial wafer, which differs from Embodiment 1 in that: the P-type contact layer 8 further includes an N-polarity C and Mg co-doped AlInGaN layer 82 disposed on a C and Mg co-doped InGaN layer 81. The Mg doping concentration is 2 × 10⁻⁶. 22 cm -3 The doping concentration of C is 1×10 22 cm -3 The composition consists of 0.1% Al and 0.15% In, with a thickness of 1.5 nm. It is grown by MOCVD at a growth temperature of 640℃, a growth pressure of 50 torr, and a V / III ratio of 3300.

[0099] Everything else is the same as in Example 1.

[0100] Example 3

[0101] This embodiment provides a light-emitting diode epitaxial wafer, which differs from Embodiment 2 in that...

[0102] After the C and Mg co-doped InGaN layer 81 was grown, only NH3 was introduced into the MOCVD reaction chamber, and it was treated at 760℃ for 120s.

[0103] Everything else is the same as in Example 2.

[0104] Example 4

[0105] This embodiment provides a light-emitting diode epitaxial wafer, which differs from Embodiment 3 in that...

[0106] After the C and Mg co-doped AlInGaN layer 82 was grown, H2 was introduced into the MOCVD reaction chamber and the mixture was treated at 1020℃ for 35 s.

[0107] Everything else is the same as in Example 3.

[0108] Comparative Example 1

[0109] This comparative example provides a light-emitting diode epitaxial wafer, which differs from Example 1 in that the P-type contact layer 8 is a heavily doped AlGaN layer, with Mg as the dopant element and a doping concentration of 1×10⁻⁶. 22 cm -3 Everything else is the same as in Example 1.

[0110] Comparative Example 2

[0111] This comparative example provides a light-emitting diode epitaxial wafer. The C and Mg co-doped InGaN layer 81 is doped with only C and not Mg, meaning that Cp2Mg is not introduced during its preparation method. Everything else is the same as in Example 1.

[0112] Example 3

[0113] This comparative example provides a light-emitting diode epitaxial wafer, which differs from Example 1 in that the C and Mg co-doped InGaN layer 81 has an N-type C dopant, meaning it substitutes for a group III element. Correspondingly, the growth temperature of this layer is 1120°C, the growth pressure is 350 torr, and the V / III ratio is 1800. All other aspects are the same as in Example 1.

[0114] The LED epitaxial wafers obtained in Examples 1-4 and Comparative Examples 1-3 were used to fabricate chips with a vertical structure of 10mil×24mil. Their luminous brightness was tested, and the improvement rate of their luminous brightness was calculated based on Comparative Example 1.

[0115] The specific results are as follows:

[0116]

[0117]

[0118] As can be seen from the table, when the P-type contact layer of the traditional light-emitting diode epitaxial wafer (Comparative Example 1) is changed to the P-type contact layer structure of the present invention, the luminous brightness is significantly improved.

[0119] The above description is a preferred embodiment of the invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made without departing from the principle of the invention, and these improvements and modifications are also considered to be within the scope of protection of the invention.

Claims

1. A light-emitting diode epitaxial wafer, comprising a substrate, and a buffer layer, an undoped AlGaN layer, an N-type AlGaN layer, a multiple quantum well layer, an electron blocking layer, a P-type AlGaN layer, and a P-type contact layer sequentially stacked on the substrate; characterized in that, The P-type contact layer includes a C and Mg co-doped InGaN layer, wherein Mg replaces group III elements and C replaces group V elements; The Mg doping concentration in the C and Mg co-doped InGaN layer is 2 × 10⁻⁶. 19 cm -3 -5×10 22 cm -3 The doping concentration of C is 1×10 19 cm -3 -2×10 22 cm -3 ; The In component in the C and Mg co-doped InGaN layer is 0.01-0.2%, and its thickness is 2nm-10nm.

2. The light-emitting diode epitaxial wafer as described in claim 1, characterized in that, After the C and Mg co-doped InGaN layer is grown, it is treated with NH3 to form an N polar contact surface.

3. The light-emitting diode epitaxial wafer as described in claim 1 or 2, characterized in that, The P-type contact layer also includes an N-polar C and Mg co-doped AlInGaN layer, wherein Mg replaces group III elements and C replaces group V elements; The N-polar C and Mg co-doped AlInGaN layer is disposed on the C and Mg co-doped InGaN layer.

4. The light-emitting diode epitaxial wafer as described in claim 3, characterized in that, The Mg doping concentration in the N-polar C and Mg co-doped AlInGaN layer is 2 × 10⁻⁶. 19 cm -3 -5×10 22 cm -3 The doping concentration of C is 2 × 10⁻⁶. 19 cm -3 -2×10 22 cm -3 ; The AlInGaN layer with N polarity C and Mg co-doped has an Al content of 0-0.2% and an In content of 0.01-0.2%, and its thickness is 0.5nm-2nm.

5. The light-emitting diode epitaxial wafer as described in claim 4, characterized in that, After the N-polar C and Mg co-doped AlInGaN layer is grown, it is treated with H2 to form a roughened surface.

6. A method for preparing a light-emitting diode epitaxial wafer, used to prepare a light-emitting diode epitaxial wafer as described in any one of claims 1-5, characterized in that, include: A substrate is provided on which a buffer layer, an undoped AlGaN layer, an N-type AlGaN layer, a multiple quantum well layer, an electron blocking layer, a P-type AlGaN layer and a P-type contact layer are sequentially formed. The P-type contact layer includes a C and Mg co-doped InGaN layer, wherein Mg replaces group III elements and C replaces group V elements; The Mg doping concentration in the C and Mg co-doped InGaN layer is 2 × 10⁻⁶. 19 cm -3 -5×10 22 cm -3 The doping concentration of C is 1×10 19 cm -3 -2×10 22 cm -3 ; The In component in the C and Mg co-doped InGaN layer is 0.01-0.2%, and its thickness is 2nm-10nm.

7. The method for fabricating a light-emitting diode epitaxial wafer as described in claim 6, characterized in that, The growth temperature of the C and Mg co-doped InGaN layer is 700℃-900℃, the growth pressure is 10 torr-200 torr, and the V / Ⅲ ratio is 1500-2500.

8. The method for fabricating a light-emitting diode epitaxial wafer as described in claim 6, characterized in that, The P-type contact layer also includes an N-polar C and Mg co-doped AlInGaN layer, with a growth temperature of 600℃-900℃, a growth pressure of 10 torr-200 torr, and a V / Ⅲ ratio of 2000-4000.

9. A light-emitting diode, characterized in that, Includes the light-emitting diode epitaxial wafer as described in any one of claims 1-5.

Citation Information

Patent Citations

  • Light-emitting diode epitaxial wafer, preparation method thereof and light-emitting diode

    CN116130572A

  • Light-emitting diode epitaxial wafer, preparation method thereof and light-emitting diode

    CN116154066A