Light emitting diode epitaxial wafer and preparation method thereof, and light emitting diode
By introducing a C and Mg co-doped AlInGaN layer and a back-well protective layer into GaN-based LEDs, the problem of electron-hole concentration mismatch was solved, thereby improving the luminous efficiency of the LEDs.
Patent Information
- Application Number
- CN202310696356.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-13
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-06-13
AI Technical Summary
The mismatch between electron and hole concentrations in GaN-based LEDs leads to low luminous efficiency and severe electron leakage, which affects the luminous efficiency of hole injection into the active region.
A composite P-type layer is introduced between the electron blocking layer and the multi-quantum well layer. An AlInGaN layer co-doped with C and Mg is used, and a back-well protection layer is set between the composite P-type layer and the multi-quantum well layer to optimize the doping concentration and composition ratio.
The increased hole injection concentration into the multi-quantum well layer enhances the radiative recombination efficiency of electrons and holes, thereby improving the luminous efficiency of the light-emitting diode.
Smart Images

Figure CN116682903B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of semiconductor optoelectronic devices, and more particularly to a light-emitting diode epitaxial wafer and its fabrication method, and a light-emitting diode. Background Technology
[0002] Light-emitting diodes (LEDs) are a type of energy-saving and environmentally friendly light source. Currently, various types of LEDs are widely used in indicators, displays, backlighting, and projection. These achievements in semiconductor lighting are mainly due to advancements in GaN-based LED technology. Compared to other material systems, GaN-based LEDs have significant advantages in both efficiency and reliability.
[0003] For GaN materials, electrons have higher mobility and lower effective mass compared to holes. Electrons are also easier to activate and have a higher concentration, leading to a significant electron-hole mismatch in the active region. Quantum wells near the N-type GaN layer emit almost no light, while electrons can easily be injected into the active region and even into the P-type GaN layer, causing electron leakage. Furthermore, the electron blocking layer, as the main functional layer of the LED, not only blocks electron injection into the P-type layer for light emission but also blocks hole injection into the active region, further reducing the hole concentration and exacerbating the electron-hole mismatch problem, severely impacting the LED's luminous efficiency. Therefore, to improve the luminous efficiency of GaN-based LEDs, increasing the hole concentration injected into the active region and improving the electron-hole matching degree is essential. Summary of the Invention
[0004] The technical problem to be solved by the present invention is to provide an epitaxial wafer for a light-emitting diode and a method for preparing the same, which can improve the luminous efficiency of the light-emitting diode.
[0005] Another technical problem that this invention aims to solve is to provide a light-emitting diode with high luminous efficiency.
[0006] To address the aforementioned problems, this invention discloses a light-emitting diode epitaxial wafer, comprising a substrate and an N-type GaN layer, a stress-relieving layer, a multiple quantum well layer, a composite P-type layer, an electron blocking layer, and a P-type GaN layer sequentially disposed on the substrate; the composite P-type layer comprises a C and Mg co-doped AlInGaN layer, wherein Mg replaces group III elements and C replaces group V elements.
[0007] As an improvement to the above technical solution, the Mg doping concentration in the C and Mg co-doped AlInGaN layer is 2 × 10⁻⁶. 18 cm -3 -5×1021 cm -3 The doping concentration of C is 1×10 18 cm -3 -2×10 21 cm -3 ;
[0008] The Al component in the C and Mg co-doped AlInGaN layer is 0-0.2%, the In component is 0.01-0.2%, and its thickness is 20nm-2000nm.
[0009] As an improvement to the above technical solution, the composite P-type layer is a C and Mg co-doped AlInGaN layer, or
[0010] The composite P-type layer is a stacked structure composed of multiple C and Mg co-doped AlInGaN layers.
[0011] As an improvement to the above technical solution, a back-well protection layer is also included, which is disposed between the multi-quantum well layer and the composite P-type layer;
[0012] The back-well protective layer is an AlGaN layer, or
[0013] The back-well protective layer is a stacked structure composed of multiple AlGaN layers.
[0014] As an improvement to the above technical solution, the Al composition in the AlGaN layer is 0.4-0.9%, and its thickness is 1nm-50nm.
[0015] As an improvement to the above technical solution, it also includes a buffer layer and an intrinsic GaN layer sequentially stacked between the substrate and the N-type GaN layer.
[0016] Accordingly, the present invention also discloses a method for preparing a light-emitting diode epitaxial wafer, which includes:
[0017] A substrate is provided on which an N-type GaN layer, a stress-relieving layer, a multiple quantum well layer, a composite P-type layer, an electron blocking layer, and a P-type GaN layer are sequentially grown; the composite P-type layer includes a C and Mg co-doped AlInGaN layer, wherein Mg replaces group III elements and C replaces group V elements.
[0018] As an improvement to the above technical solution, the growth temperature of the C and Mg co-doped AlInGaN layer is 600℃-900℃, and the growth pressure is 10 torr-200 torr.
[0019] As an improvement to the above technical solution, the light-emitting diode epitaxial wafer further includes a back-well protection layer, which includes an AlGaN layer;
[0020] The growth temperature of the AlGaN layer is 950℃-1100℃, and the growth pressure is 100 torr-500 torr.
[0021] Accordingly, the present invention also discloses a light-emitting diode, which includes the above-mentioned light-emitting diode epitaxial wafer.
[0022] Implementing this invention has the following beneficial effects:
[0023] 1. In the light-emitting diode epitaxial wafer of the present invention, a composite P-type layer is introduced between the electron blocking layer and the multiple quantum well layer. This composite P-type layer comprises a C- and Mg-doped AlInGaN layer, wherein Mg replaces group III elements and C replaces group V elements, i.e., both are substituted to form a P-type semiconductor, thus obtaining the composite P-type layer. This layer can weaken the blocking effect of the electron blocking layer on hole injection in the P-type GaN layer, increase the hole concentration injected from the P-type GaN layer into the multiple quantum well light-emitting layer, improve the radiative recombination efficiency of electrons and holes in the multiple quantum well layer, and improve the luminous efficiency of the light-emitting diode epitaxial wafer.
[0024] 2. In the epitaxial wafer of the light-emitting diode of the present invention, a back-well protection layer is provided between the composite P-type layer and the multi-quantum-well layer. The back-well protection layer is made of AlGaN material, which can protect the high-quality multi-quantum-well light-emitting layer from damage and ultimately achieve the purpose of improving the luminous efficiency of the light-emitting diode. Attached Figure Description
[0025] Figure 1 This is a schematic diagram of the structure of a light-emitting diode epitaxial wafer in one embodiment of the present invention;
[0026] Figure 2 This is a schematic diagram of the structure of the light-emitting diode epitaxial wafer in another embodiment of the present invention;
[0027] Figure 3 This is a flowchart of a method for preparing an epitaxial wafer for a light-emitting diode according to an embodiment of the present invention. Detailed Implementation
[0028] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be described in further detail below.
[0029] refer to Figure 1 The present invention discloses a light-emitting diode epitaxial wafer, comprising a substrate 1 and an N-type GaN layer 2, a stress relief layer 3, a multiple quantum well layer 4, a composite P-type layer 5, an electron blocking layer 6 and a P-type GaN layer 7 sequentially disposed on the substrate 1.
[0030] The composite P-type layer 5 comprises a C and Mg co-doped AlInGaN layer, wherein Mg substitutes for group III elements and C substitutes for group V elements. This substitution forms a composite P-type semiconductor. Specifically, in one embodiment of the invention, the composite P-type layer 5 is a C and Mg co-doped AlInGaN layer. In another embodiment of the invention, the composite P-type layer 5 is a stacked structure formed by multiple C and Mg co-doped AlInGaN layers, but the invention is not limited thereto.
[0031] In the C and Mg co-doped AlInGaN layer, the Mg doping concentration is 1×10⁻⁶. 18 cm -3 -8×10 21 cm -3 An example is 2×10 18 cm -3 6×10 18 cm -3 1×10 19 cm -3 9×10 19 cm -3 2×10 20 cm -3 Or 7×10 21 cm -3 However, it is not limited to this. Preferably, the Mg doping concentration is 2 × 10⁻⁶. 18 cm -3 -5×10 21 cm -3 .
[0032] The C doping concentration in the C and Mg co-doped AlInGaN layer is 8 × 10⁻⁶. 17 cm -3 -5×10 21 cm -3 An example is 9×10 17 cm -3 3×10 18 cm -3 8×10 18 cm -3 2×10 19 cm -3 7×10 19 cm -3 3×10 20 cm -3 9×10 20 cm -3 Or 2×10 21 cm -3 However, it is not limited to this. Preferably, the doping concentration of C is 1×10⁻⁶. 18 cm -3-2×10 21 cm -3 .
[0033] In the C and Mg co-doped AlInGaN layer, the proportion of Al component (i.e., the molar ratio of AlN) is 0-0.2, with examples of 0.05, 0.07, 0.1, 0.13, 0.15, or 0.17, but not limited to these. In the C and Mg co-doped AlInGaN layer, the proportion of In component (i.e., the molar ratio of InN) is 0.01-0.2, with examples of 0.05, 0.07, 0.1, 0.13, 0.15, or 0.17, but not limited to these.
[0034] The thickness of the composite P-type layer 5 is 20nm-2000nm, with examples of 25nm, 100nm, 400nm, 800nm, 1200nm, 1400nm or 1600nm, but not limited to these.
[0035] Preferred, Reference Figure 2 In one embodiment of the present invention, the light-emitting diode epitaxial wafer further includes a back-well protection layer 8, which is disposed between the multi-quantum-well layer 4 and the composite P-type layer 5. This back-well protection layer effectively prevents the composite P-type layer from affecting the multi-quantum-well layer 4 due to excessively high doping concentration. Specifically, in one embodiment of the present invention, the back-well protection layer 8 is an AlGaN layer. In another embodiment of the present invention, the back-well protection layer 8 is a stacked structure composed of multiple AlGaN layers.
[0036] The proportion of Al component in the AlGaN layer (i.e., the molar ratio of AlN) is 0.3-0.95, with exemplary values of 0.35, 0.4, 0.55, 0.6, 0.7, 0.78, or 0.85, but not limited thereto. A preferred proportion is 0.4-0.9.
[0037] The thickness of the AlGaN layer is 1nm-50nm, with examples of 4nm, 10nm, 16nm, 30nm, 40nm or 45nm, but not limited to these.
[0038] The substrate 1 may be a sapphire substrate, a silicon substrate, a silicon carbide substrate, a gallium oxide substrate, or a zinc oxide substrate, but is not limited to these.
[0039] The N-type GaN layer 2 is doped with Si, but is not limited to Si. The doping concentration of the N-type GaN layer 2 is 5 × 10⁻⁶. 18 cm -3 -1×10 19 cm -3 The thickness is 1μm-3μm.
[0040] The stress relief layer 3 is a periodic structure formed by overlapping InGaN and lightly doped N-GaN layers, with a period number of 3-10. The thickness of a single InGaN layer is 2nm-6nm, and the thickness of a single lightly doped N-GaN layer is 5nm-10nm. The dopant element in the lightly doped N-GaN layer is Si, but not limited to Si. The doping concentration of the lightly doped N-GaN layer is 1×10⁻⁶. 15 cm -3 -4×10 17 cm -3 .
[0041] Among them, the multiple quantum well layer 4 consists of alternating stacked InGaN quantum well layers and GaN quantum barrier layers, with a stacking period of 3-15. The thickness of a single InGaN quantum well layer is 2nm-5nm. The thickness of a single GaN quantum barrier layer is 6nm-15nm.
[0042] Among them, electron blocking layer 6 is Al x Ga 1-x N layers and In y Ga 1-y A periodic structure with N alternating layers, the number of periods being 3-15; where x is 0.05-0.2 and y is 0.1-0.5. A single Al x Ga 1-x The thickness of the N layer is 1nm-5nm, and a single In... y Ga 1-y The thickness of layer N is 1nm-5nm. The total thickness of electron blocking layer 6 is 5nm-100nm.
[0043] The doping element in the p-type GaN layer 7 is Mg, but it is not limited to this. The doping concentration of Mg in the p-type GaN layer 7 is 5 × 10⁻⁶. 18 cm -3 -1×10 20 cm -3 The thickness of the p-type GaN layer 7 is 20nm-200nm.
[0044] Preferably, in one embodiment of the present invention, the light-emitting diode epitaxial wafer further includes a buffer layer 9 and an intrinsic GaN layer 10 sequentially stacked between the substrate 1 and the N-type GaN layer 2. The buffer layer 9 may be an AlN layer and / or an AlGaN layer, but is not limited thereto. The thickness of the buffer layer 9 is 20 nm-100 nm. The thickness of the intrinsic GaN layer 10 is 1 μm-3 μm.
[0045] Accordingly, refer to Figure 3 The present invention also discloses a method for preparing a light-emitting diode epitaxial wafer, which is used to prepare the above-mentioned light-emitting diode epitaxial wafer, and includes the following steps:
[0046] S1: Provides a substrate;
[0047] Specifically, the substrate can be a sapphire substrate, a silicon substrate, or a silicon carbide substrate, but is not limited to these. A sapphire substrate is preferred.
[0048] S2: An N-type GaN layer, a stress relief layer, a multi-quantum well layer, a composite P-type layer, an electron blocking layer, and a P-type GaN layer are sequentially grown on the substrate.
[0049] Preferably, in one embodiment of the present invention, S2 includes sequentially growing a buffer layer, an intrinsic GaN layer, an N-type GaN layer, a stress relief layer, a multiple quantum well layer, a composite P-type layer, an electron blocking layer, and a P-type GaN layer on a substrate.
[0050] Specifically, in this embodiment, step S2 includes:
[0051] S21: Grow a buffer layer on the substrate;
[0052] Specifically, an AlGaN layer grown by MOCVD or an AlN layer grown by PVD can be used as a buffer layer, but it is not limited to these. Preferably, an AlN layer grown by PVD is used as a buffer layer.
[0053] S22: Grow an intrinsic GaN layer on the buffer layer;
[0054] Specifically, intrinsic GaN layers were grown in MOCVD at a temperature of 1100℃-1150℃ and a pressure of 100 torr-500 torr. During growth, NH3 was introduced into the MOCVD reaction chamber as the N source; H2 and N2 were used as carrier gases, and TMGa was introduced as the Ga source.
[0055] S23: Growing an N-type GaN layer on an intrinsic GaN layer;
[0056] Specifically, an N-type GaN layer is grown in MOCVD at a temperature of 1100℃-1150℃ and a pressure of 100 torr-500 torr. During growth, NH3 is introduced into the MOCVD reaction chamber as the N source, and SiH4 is introduced as the N-type doping source; H2 and N2 are used as carrier gases, and TMGa is introduced as the Ga source.
[0057] S24: Growing a stress-relieving layer on an N-type GaN layer;
[0058] Specifically, InGaN layers and lightly doped N-GaN layers are periodically grown in MOCVD until a stress-relieved layer is obtained. The InGaN layer is grown at a temperature of 750℃-850℃ and a growth pressure of 100 torr-200 torr. During growth, NH3 is introduced into the MOCVD reaction chamber as the N source, N2 as the carrier gas, TMIn as the In source, and TMGa as the Ga source. The lightly doped N-GaN layer is grown at a temperature of 850℃-900℃ and a growth pressure of 100 torr-200 torr. During growth, NH3 is introduced into the MOCVD reaction chamber as the N source, SiH4 as the N-type dopant source, H2 and N2 as the carrier gas, and TMGa as the Ga source.
[0059] S25: Growth of multiple quantum well layers on stress buffer layers;
[0060] Specifically, InGaN quantum well layers and GaN quantum barrier layers are periodically grown in MOCVD to form a multi-quantum well layer. The InGaN quantum well layer is grown at a temperature of 700℃-800℃ and a growth pressure of 100 torr-500 torr. During growth, NH3 is introduced as the N source, N2 as the carrier gas, TEGa as the Ga source, and TMIn as the In source in the MOCVD reaction chamber. The GaN quantum barrier layer is grown at a temperature of 800℃-900℃ and a growth pressure of 100 torr-500 torr. During growth, NH3 is introduced as the N source, H2 and N2 as the carrier gases, and TEGa as the Ga source in the MOCVD reaction chamber.
[0061] S26: Growing a back-end protective layer on a multi-quantum-well layer;
[0062] Specifically, one or more AlGaN layers are grown by MOCVD as a back-well protective layer at a growth temperature of 950℃-1100℃ and a growth pressure of 100 torr-500 torr. During growth, NH3 is introduced into the MOCVD reaction chamber as the N source, H2 and N2 are used as carrier gases, TEGa is introduced as the Ga source, and TMAl is introduced as the Al source.
[0063] S27: A composite P-type layer is grown on the back protective layer of the well;
[0064] Specifically, one or more C and Mg co-doped AlInGaN layers are grown via MOCVD as composite P-type layers at a growth temperature of 600℃-900℃ and a growth pressure of 10 torr-200 torr. Based on this low-temperature, low-pressure growth, C and Mg P-type doping can be achieved. Specifically, during growth, NH3 is introduced into the MOCVD reaction chamber as the N source, H2 and N2 are used as carrier gases, TEGa is introduced as the Ga and C sources, TMAl is introduced as the Al source, and TMIn is introduced as the In source.
[0065] S28: An electron blocking layer is grown on a composite P-type layer;
[0066] Specifically, Al is periodically grown in MOCVD. x Ga 1-x N layers and In y Ga 1-y The N-layer acts as an electron-blocking layer. Al x Ga 1-x The N-layer is grown at a temperature of 900℃-1000℃ and a growth pressure of 100 torr-500 torr. During growth, NH3 is introduced into the MOCVD reaction chamber as the N source, N2 and H2 are used as carrier gases, TMAl is introduced as the Al source, and TMGa is introduced as the Ga source. y Ga 1-y The N-layer is grown at a temperature of 900℃-1000℃ and a growth pressure of 100 torr-500 torr. During growth, NH3 is introduced into the MOCVD reaction chamber as the N source, N2 and H2 are used as carrier gases, TMIn is introduced as the In source, and TMGa is introduced as the Ga source.
[0067] S29: Grow a P-type GaN layer on the electron blocking layer;
[0068] Specifically, a P-type GaN layer is grown in MOCVD at a temperature of 800℃-1000℃ and a pressure of 100 torr-300 torr. During growth, NH3 is introduced into the MOCVD reaction chamber as the N source, and Cp2Mg is introduced as the P-type doping source; H2 and N2 are used as carrier gases, and TMGa is introduced as the Ga source.
[0069] The present invention will be further described below with reference to specific embodiments:
[0070] Example 1
[0071] This embodiment provides a light-emitting diode epitaxial wafer, referenced... Figure 1 It includes a substrate 1 and a buffer layer 9, an intrinsic GaN layer 10, an N-type GaN layer 2, a stress relief layer 3, a multiple quantum well layer 4, a composite P-type layer 5, an electron blocking layer 6, and a P-type GaN layer 7 sequentially disposed on the substrate 1.
[0072] In this design, substrate 1 is a sapphire substrate; buffer layer 9 is an AlN layer with a thickness of 50 nm; intrinsic GaN layer 10 has a thickness of 1.4 μm; and the Si doping concentration in N-type GaN layer 2 is 7 × 10⁻⁶. 18 cm -3 Its thickness is 2μm.
[0073] The stress relief layer 3 has a periodic structure with 5 periods. Each period consists of sequentially stacked InGaN and low-doped N-GaN layers. The thickness of a single InGaN layer is 4 nm, and the thickness of a single low-doped N-GaN layer is 8 nm. The low-doped N-GaN layer is doped with Si at a concentration of 6 × 10⁻⁶. 15 cm -3 .
[0074] Among them, the multiple quantum well layer 4 consists of alternating stacked InGaN quantum well layers and GaN quantum barrier layers, with a stacking period of 10. The thickness of a single InGaN quantum well layer is 3nm, and the thickness of a single GaN quantum barrier layer is 10nm.
[0075] Among them, the composite p-type layer 5 is a C and Mg co-doped AlInGaN layer, wherein the C doping concentration is 3 × 10⁻⁶. 18 cm -3 The Mg doping concentration is 8 × 10⁻⁶. 18 cm -3 The Al component accounts for 0.1%, the In component accounts for 0.05%, and its thickness is 50nm.
[0076] Among them, electron blocking layer 6 is Al x Ga 1-x Layer N (x = 0.12) and In y Ga 1-y A periodic structure with N alternating layers (y = 0.3) and a period number of 8, where a single Al... x Ga 1-x The thickness of the N layer is 3nm, and a single In... y Ga 1-y The thickness of the N-layer is 3 nm. The dopant element of the p-type GaN layer 7 is Mg, with a doping concentration of 3.5 × 10⁻⁶. 19 cm -3 The thickness is 40nm.
[0077] The method for fabricating the epitaxial wafer of the light-emitting diode in this embodiment includes the following steps:
[0078] (1) Provide a substrate;
[0079] (2) Grow a buffer layer on the substrate;
[0080] Specifically, an AlN layer is grown using PVD as a buffer layer.
[0081] (3) Grow an intrinsic GaN layer on the buffer layer;
[0082] Specifically, intrinsic GaN layers were grown using MOCVD at a growth temperature of 1120℃ and a growth pressure of 250 tor. During growth, NH3 was introduced into the MOCVD reaction chamber as the N source, and H2 and N2 were used as carrier gases, while TMGa was introduced as the Ga source.
[0083] (4) Growing an N-type GaN layer on the intrinsic GaN layer;
[0084] Specifically, an N-type GaN layer was grown using MOCVD at a growth temperature of 1130℃ and a growth pressure of 150 torr. During growth, NH3 was introduced into the MOCVD reaction chamber as an N source and SiH4 was introduced as an N-type doping source. H2 and N2 were used as carrier gases, and TMGa was introduced as a Ga source.
[0085] (5) A stress-relieving layer is grown on the N-type GaN layer;
[0086] Specifically, InGaN layers and lightly doped N-GaN layers are periodically grown in MOCVD until a stress-relieved layer is obtained. The InGaN layer is grown at a temperature of 780℃ and a growth pressure of 120 torr. During growth, NH3 is introduced into the MOCVD reaction chamber as the N source, N2 as the carrier gas, TMIn as the In source, and TMGa as the Ga source. The lightly doped N-GaN layer is grown at a temperature of 940℃ and a growth pressure of 120 torr. During growth, NH3 is introduced into the MOCVD reaction chamber as the N source, SiH4 as the N-type dopant source, H2 and N2 as the carrier gas, and TMGa as the Ga source.
[0087] (6) Grow a multi-quantum well layer on the stress relief layer;
[0088] Specifically, InGaN quantum well layers and GaN quantum barrier layers are periodically grown in MOCVD to obtain multiple quantum well layers;
[0089] The InGaN quantum well layer was grown at a temperature of 750℃ and a growth pressure of 300 torr. During growth, NH3 was introduced as the N source, N2 as the carrier gas, TEGa as the Ga source, and TMIn as the In source in the MOCVD reaction chamber. The GaN quantum barrier layer was grown at a temperature of 820℃ and a growth pressure of 300 torr. During growth, NH3 was introduced as the N source, H2 and N2 as the carrier gases, and TEGa as the Ga source in the MOCVD reaction chamber.
[0090] (7) Growth of composite P-type layers on multi-quantum-well layers;
[0091] Specifically, one or more C and Mg co-doped AlInGaN layers are grown by MOCVD as composite P-type layers at a growth temperature of 660℃ and a growth pressure of 50 torr. During growth, NH3 is introduced into the MOCVD reaction chamber as the N source, H2 and N2 are used as carrier gases, TEGa is introduced as the Ga and C sources, TMAl is introduced as the Al source, and TMIn is introduced as the In source.
[0092] (8) An electron blocking layer is grown on the composite P-type layer;
[0093] Specifically, Al is periodically grown in MOCVD. x Ga 1-x N layers and In y Ga 1-y The N-layer acts as an electron-blocking layer. Al x Ga 1-x The N-layer was grown at a temperature of 950℃ and a growth pressure of 250 torr. During growth, NH3 was introduced into the MOCVD reaction chamber as the N source, N2 and H2 were used as carrier gases, TMAl was introduced as the Al source, and TMGa was introduced as the Ga source. y Ga 1-y The N-layer was grown at a temperature of 950℃ and a growth pressure of 250 torr. During growth, NH3 was introduced into the MOCVD reaction chamber as the N source, N2 and H2 were used as carrier gases, TMIn was introduced as the In source, and TMGa was introduced as the Ga source.
[0094] (9) Grow a P-type GaN layer on the electron blocking layer;
[0095] Specifically, a P-type GaN layer was grown in MOCVD at a temperature of 900℃ and a pressure of 200 torr. During growth, NH3 was introduced into the MOCVD reaction chamber as the N source, and Cp2Mg was introduced as the P-type doping source; H2 and N2 were used as carrier gases, and TMGa was introduced as the Ga source.
[0096] Example 2
[0097] This embodiment provides a light-emitting diode epitaxial wafer, referenced... Figure 2 It includes a substrate 1 and a buffer layer 9, an intrinsic GaN layer 10, an N-type GaN layer 2, a stress relief layer 3, a multi-quantum well layer 4, a weather protection layer 8, a composite P-type layer 5, an electron blocking layer 6, and a P-type GaN layer 7 sequentially disposed on the substrate 1.
[0098] In this design, substrate 1 is a sapphire substrate; buffer layer 9 is an AlN layer with a thickness of 50 nm; intrinsic GaN layer 10 has a thickness of 1.4 μm; and the Si doping concentration in N-type GaN layer 2 is 7 × 10⁻⁶. 18 cm -3 Its thickness is 2μm.
[0099] The stress relief layer 3 has a periodic structure with 5 periods. Each period consists of sequentially stacked InGaN and low-doped N-GaN layers. The thickness of a single InGaN layer is 4 nm, and the thickness of a single low-doped N-GaN layer is 8 nm. The low-doped N-GaN layer is doped with Si at a concentration of 6 × 10⁻⁶. 15 cm -3 .
[0100] Among them, the multiple quantum well layer 4 consists of alternating stacked InGaN quantum well layers and GaN quantum barrier layers, with a stacking period of 10. The thickness of a single InGaN quantum well layer is 3nm, and the thickness of a single GaN quantum barrier layer is 10nm.
[0101] Among them, the back protective layer 8 is an AlGaN layer with an Al composition ratio of 0.6 and a thickness of 15nm.
[0102] Among them, the composite p-type layer 5 is a C and Mg co-doped AlInGaN layer, wherein the C doping concentration is 3 × 10⁻⁶. 18 cm -3 The Mg doping concentration is 8 × 10⁻⁶. 18 cm -3 The Al component accounts for 0.1%, the In component accounts for 0.05%, and its thickness is 50nm.
[0103] Among them, electron blocking layer 6 is Al x Ga 1-x Layer N (x = 0.12) and In y Ga 1-y A periodic structure with N alternating layers (y = 0.3) and a period number of 8, where a single Al... x Ga 1-x The thickness of the N layer is 3nm, and a single In... y Ga 1-y The thickness of the N-layer is 3 nm. The dopant element of the p-type GaN layer 7 is Mg, with a doping concentration of 3.5 × 10⁻⁶. 19 cm -3 The thickness is 40nm.
[0104] The method for fabricating the epitaxial wafer of the light-emitting diode in this embodiment includes the following steps:
[0105] (1) Provide a substrate;
[0106] (2) Grow a buffer layer on the substrate;
[0107] Specifically, an AlN layer is grown using PVD as a buffer layer.
[0108] (3) Grow an intrinsic GaN layer on the buffer layer;
[0109] Specifically, intrinsic GaN layers were grown using MOCVD at a growth temperature of 1120℃ and a growth pressure of 250 tor. During growth, NH3 was introduced into the MOCVD reaction chamber as the N source, and H2 and N2 were used as carrier gases, while TMGa was introduced as the Ga source.
[0110] (4) Growing an N-type GaN layer on the intrinsic GaN layer;
[0111] Specifically, an N-type GaN layer was grown using MOCVD at a growth temperature of 1130℃ and a growth pressure of 150 torr. During growth, NH3 was introduced into the MOCVD reaction chamber as an N source and SiH4 was introduced as an N-type doping source. H2 and N2 were used as carrier gases, and TMGa was introduced as a Ga source.
[0112] (5) A stress-relieving layer is grown on the N-type GaN layer;
[0113] Specifically, InGaN layers and lightly doped N-GaN layers are periodically grown in MOCVD until a stress-relieved layer is obtained. The InGaN layer is grown at a temperature of 780℃ and a growth pressure of 120 torr. During growth, NH3 is introduced into the MOCVD reaction chamber as the N source, N2 as the carrier gas, TMIn as the In source, and TMGa as the Ga source. The lightly doped N-GaN layer is grown at a temperature of 940℃ and a growth pressure of 120 torr. During growth, NH3 is introduced into the MOCVD reaction chamber as the N source, SiH4 as the N-type dopant source, H2 and N2 as the carrier gas, and TMGa as the Ga source.
[0114] (6) Grow a multi-quantum well layer on the stress relief layer;
[0115] Specifically, InGaN quantum well layers and GaN quantum barrier layers are periodically grown in MOCVD to obtain multiple quantum well layers;
[0116] The InGaN quantum well layer was grown at a temperature of 750℃ and a growth pressure of 300 torr. During growth, NH3 was introduced as the N source, N2 as the carrier gas, TEGa as the Ga source, and TMIn as the In source in the MOCVD reaction chamber. The GaN quantum barrier layer was grown at a temperature of 820℃ and a growth pressure of 300 torr. During growth, NH3 was introduced as the N source, H2 and N2 as the carrier gases, and TEGa as the Ga source in the MOCVD reaction chamber.
[0117] (7) Grow a back-end protective layer on the multi-quantum-well layer;
[0118] Specifically, an AlGaN layer was grown by MOCVD as a back-well protective layer at a growth temperature of 1000℃ and a growth pressure of 300 torr. During growth, NH3 was introduced into the MOCVD reaction chamber as the N source, H2 and N2 were used as carrier gases, TEGa was introduced as the Ga source, and TMAl was introduced as the Al source.
[0119] (8) A composite P-type layer is grown on the back protective layer of the well;
[0120] Specifically, one or more C and Mg co-doped AlInGaN layers are grown by MOCVD as composite P-type layers at a growth temperature of 660℃ and a growth pressure of 50 torr. During growth, NH3 is introduced into the MOCVD reaction chamber as the N source, H2 and N2 are used as carrier gases, TEGa is introduced as the Ga and C sources, TMAl is introduced as the Al source, and TMIn is introduced as the In source.
[0121] (9) An electron blocking layer is grown on the composite P-type layer;
[0122] Specifically, Al is periodically grown in MOCVD. x Ga 1-x N layers and In y Ga 1-y The N-layer acts as an electron-blocking layer. Al x Ga 1-x The N-layer was grown at a temperature of 950℃ and a growth pressure of 250 torr. During growth, NH3 was introduced into the MOCVD reaction chamber as the N source, N2 and H2 were used as carrier gases, TMAl was introduced as the Al source, and TMGa was introduced as the Ga source. y Ga 1-y The N-layer was grown at a temperature of 950℃ and a growth pressure of 250 torr. During growth, NH3 was introduced into the MOCVD reaction chamber as the N source, N2 and H2 were used as carrier gases, TMIn was introduced as the In source, and TMGa was introduced as the Ga source.
[0123] (10) Grow a P-type GaN layer on an electron blocking layer;
[0124] Specifically, a P-type GaN layer was grown in MOCVD at a temperature of 900℃ and a pressure of 200 torr. During growth, NH3 was introduced into the MOCVD reaction chamber as the N source, and Cp2Mg was introduced as the P-type doping source; H2 and N2 were used as carrier gases, and TMGa was introduced as the Ga source.
[0125] Comparative Example 1
[0126] This comparative example provides a light-emitting diode epitaxial wafer, which differs from Example 1 in that it does not include a composite P-type layer. Correspondingly, the fabrication method for this layer also omits the fabrication step; all other aspects are the same as in Example 1.
[0127] Comparative Example 2
[0128] This comparative example provides a light-emitting diode epitaxial wafer, which differs from Example 1 in that the composite P-type layer 5 is not doped with Mg, but only with C. That is, Cp₂Mg is not introduced in its preparation method. Everything else is the same as in Example 1.
[0129] Comparative Example 3
[0130] This comparative example provides a light-emitting diode epitaxial wafer, which differs from Example 1 in that the carbon in the composite P-type layer 5 is N-type doped, i.e., it replaces a group III element. Correspondingly, the growth temperature of this layer in the fabrication method is 1120°C, and the growth pressure is 350 torr. All other aspects are the same as in Example 1.
[0131] The LED epitaxial wafers obtained in Examples 1-2 and Comparative Examples 1-3 were fabricated into chips with a vertical structure of 10mil×24mil. Their luminous brightness was tested, and the improvement rate of their luminous brightness was calculated based on Comparative Example 1.
[0132] The specific results are as follows:
[0133] Luminous brightness improvement rate / % Example 1 1.53±0.08 Example 2 2.34±0.11 Comparative Example 1 - Comparative Example 2 0.32±0.13 Comparative Example 3 (-0.55)±0.09
[0134] As can be seen from the table, when the traditional LED epitaxial wafer (Comparative Example 1) is replaced with the LED epitaxial wafer structure of this invention, the luminous brightness is significantly improved.
[0135] The above description is a preferred embodiment of the invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made without departing from the principle of the invention, and these improvements and modifications are also considered to be within the scope of protection of the invention.
Claims
1. A light-emitting diode epitaxial wafer, characterized in that, The system includes a substrate and an N-type GaN layer, a stress relief layer, a multiple quantum well layer, a composite P-type layer, an electron blocking layer, and a P-type GaN layer sequentially disposed on the substrate; the composite P-type layer includes a C and Mg co-doped AlInGaN layer, wherein Mg replaces group III elements and C replaces group V elements; The Mg doping concentration in the C and Mg co-doped AlInGaN layer is 2 × 10⁻⁶. 18 cm -3 -5×10 21 cm -3 The doping concentration of C is 1×10 18 cm -3 -2×10 21 cm -3 ; The Al component in the C and Mg co-doped AlInGaN layer is 0-0.2%, the In component is 0.01-0.2%, and its thickness is 20nm-2000nm.
2. The light-emitting diode epitaxial wafer as described in claim 1, characterized in that, The composite P-type layer is a C and Mg co-doped AlInGaN layer, or The composite P-type layer is a stacked structure composed of multiple C and Mg co-doped AlInGaN layers.
3. The light-emitting diode epitaxial wafer as described in claim 1 or 2, characterized in that, It also includes a back-well protection layer disposed between the multi-quantum-well layer and the composite P-type layer; The back-well protective layer is an AlGaN layer, or The back-well protective layer is a stacked structure composed of multiple AlGaN layers.
4. The light-emitting diode epitaxial wafer as described in claim 3, characterized in that, The Al component in the AlGaN layer is 0.4-0.9%, and its thickness is 1nm-50nm.
5. The light-emitting diode epitaxial wafer as described in claim 3, characterized in that, It also includes a buffer layer and an intrinsic GaN layer sequentially stacked between the substrate and the N-type GaN layer.
6. A method for preparing a light-emitting diode epitaxial wafer, used to prepare a light-emitting diode epitaxial wafer as described in any one of claims 1-5, characterized in that, include: A substrate is provided on which an N-type GaN layer, a stress-relieving layer, a multiple quantum well layer, a composite P-type layer, an electron blocking layer, and a P-type GaN layer are sequentially grown; the composite P-type layer includes a C and Mg co-doped AlInGaN layer, wherein Mg replaces group III elements and C replaces group V elements.
7. The method for fabricating a light-emitting diode epitaxial wafer as described in claim 6, characterized in that, The growth temperature of the C and Mg co-doped AlInGaN layer is 600℃-900℃, and the growth pressure is 10 torr-200 torr.
8. The method for fabricating a light-emitting diode epitaxial wafer as described in claim 6, characterized in that, The light-emitting diode epitaxial wafer also includes a back-well protection layer, which includes an AlGaN layer. The growth temperature of the AlGaN layer is 950℃-1100℃, and the growth pressure is 100 torr-500 torr.
9. A light-emitting diode, characterized in that, Includes the light-emitting diode epitaxial wafer as described in any one of claims 1-5.
Citation Information
Patent Citations
Optoelectronic semiconductor chip
CN102664223A
Light-emitting diode chip manufacturing method and light-emitting diode chip
JP2018029110A