Adhesive film

By using PEEK-PEoEK copolymer film, the problem of bonding thermoplastic polymer materials has been solved, achieving a bonding effect with high fracture toughness and low melting temperature, improving the chemical resistance and mechanical properties of composite materials, and making them suitable for the aerospace industry.

CN116685469BActive Publication Date: 2026-11-20SOLVAY SPECIALTY POLYMERS USA LLC +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202280009650.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-04-23
Filing Date
2022-01-10
Publication Date
2026-11-20
Estimated Expiration
2042-01-10

AI Technical Summary

Technical Problem

Existing technologies are difficult to effectively bond thermoplastic polymer materials, especially in the aerospace industry, leading to delamination and loss of structural integrity in composite and laminate materials under high-demand environments. Furthermore, existing adhesive materials are insufficient in terms of solvent resistance and mechanical properties.

Method used

Using PEEK-PEoEK copolymer films with molar ratios ranging from 90/10 to 55/45, these films exhibit high fracture toughness and low melting temperature, and are used to bond thermoplastic polymer materials. The chemical and mechanical properties of the materials are ensured by differential scanning calorimetry and FT-IR analysis.

Benefits of technology

It provides a bond with high fracture toughness and excellent mechanical properties, reduces processing temperature, improves the chemical resistance and fluid resistance of materials, is suitable for bonding composite materials, and avoids deformation and structural damage caused by melting and cooling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure QLYQS_2
    Figure QLYQS_2
  • Figure QLYQS_3
    Figure QLYQS_3
Patent Text Reader

Abstract

The adhesive film comprising the PEEK-PEoEK copolymer is chemically compatible with polyaryletherketone, thereby providing a connected polyaryletherketone polymer part with high fracture toughness and overall good mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Related applications

[0002] This application claims priority to Provisional Application No. 63 / 136,227 filed in the United States on January 12, 2021, and Patent Application No. EP 21170100.8 filed in Europe on April 23, 2021, the entire contents of each of these applications are incorporated herein by reference for all purposes. Technical Field

[0003] This invention relates to the use of PEEK-PEoEK copolymers in the manufacture of adhesive films and their use in components such as composites, laminates and the like. Background Technology

[0004] In many industries, particularly the aerospace industry, there is extensive use of laminates, composites, and other components comprising multiple layers of different materials, each with specific properties for the final component. Achieving satisfactory adhesion or bonding directly between different layers that may be used in composites or laminates often proves challenging. Poor compatibility between composite layers can limit the properties exhibited by such components. In particular, certain thermoplastic polymers (especially crystalline and / or high-temperature thermoplastics) exhibit poor adhesion to other materials, leading to delamination and loss of structural integrity when components are used in demanding environments.

[0005] Numerous techniques have been proposed for securing and / or bonding thermoplastic parts together. In particular, many different welding processes, such as ultrasonic welding, induction welding, and hot plate welding, have been proposed for securing first and second thermoplastic parts together. However, localized melting of the first and second parts in the welding area can affect the integrity and / or shape of the parts. This can also lead to deformation due to residual stresses that accumulate in the parts during the melting and / or cooling of the thermoplastic in the welding area.

[0006] To address some issues related to welding processes, it has been proposed to provide films and / or adhesives between parts and / or layers to bond them together.

[0007] WO 11 / 001103A2 describes the use of amorphous polyether ketone ketone (PEKK) membranes as adhesive layers in components such as composites and laminates. However, given the amorphous nature of the membrane, it is considered unsuitable for structural applications in the aerospace industry. In general, using amorphous materials as adhesive layers in composites may represent the weakest point of the structure, where properties such as solvent resistance are relatively low. Therefore, the joints can be easily eroded by fluids, leading to premature structural failure.

[0008] WO 2015 / 198063A1 discloses the use of polymeric materials comprising a PEEK-PEDEK polymer having repeating units of the following formula.

[0009] -O-Ph-O-Ph-CO-Ph- I

[0010] and the repeating unit of the following formula

[0011] -O-Ph-Ph-O-Ph-CO-Ph- II

[0012] Ph represents the phenylene moiety, which acts as an adhesive between the first and second parts comprising a polyaryletherketone polymer (particularly PEEK). However, the mechanical properties of the PEEK-PEDEK polymer are inferior to those of other polyaryletherketone polymers.

[0013] Therefore, there is still a need to provide films and / or layers that can bond together parts made of polyaryletherketone polymers with good chemical resistance and mechanical properties.

[0014] To reduce the processing temperature for manufacturing composite parts, it is advantageous to use polyaryletherketone polymers with melting temperatures lower than those currently used. Therefore, there is a need for adhesive films containing semi-crystalline polymers with melting temperatures below 310°C to allow for proper bonding of parts based on low-melting-point polyaryletherketone polymers. Summary of the Invention

[0015] It has now been found that films containing PEEK-PEoEK copolymers, especially (R... PEEK ) / (R PEoEK The molar ratios in the range of 90 / 10 to 55 / 45, preferably from 85 / 15 to 60 / 40, are chemically compatible with polyaryletherketones, thereby providing polyaryletherketone polymer parts with high fracture toughness and a minimum crystallinity level of 4 J / g when measured by DSC (cooling rate of 10 °C / min), thus providing composite materials with excellent mechanical properties.

[0016] Therefore, the first object of the present invention is a film comprising a PEEK-PEoEK copolymer. This film is suitable for use as an adhesive film, and in the remainder of the specification, the terms "film" and "adhesive film" are used interchangeably.

[0017] For the purposes of this instruction manual:

[0018] - The use of parentheses before and after symbols or numbers that identify a compound, chemical formula or part of a formula serves only to better distinguish those symbols or numbers from the rest of the text, and therefore the parentheses may be omitted;

[0019] - When indicating a numerical range, the range endpoints are included;

[0020] The term "containing PEEK-PEoEK copolymer" means that the composition contains one or more PEEK-PEoEK copolymers.

[0021] PEEK-PEoEK copolymer

[0022] As used herein, the term "PEEK-PEoEK copolymer" refers to a copolymer containing at least 50 mol.% repeating units (R) relative to the total molar number of repeating units in the PEEK-PEoEK copolymer. PEEK ) and repeating unit (R) PEoEK ), its molar ratio (R PEEK ) / (R PEoEK The range is from 95 / 5 to 5 / 95. In some embodiments, the PEEK-PEoEK copolymer comprises at least 60 mol.%, at least 70 mol.%, at least 80 mol.%, at least 90 mol.%, at least 95 mol.%, and most preferably at least 99 mol.%, of repeating units (R) relative to the total molar number of repeating units in the PEEK-PEoEK copolymer. PEEK ) and (R PEoEK ).

[0023] Repeating unit (R) PEEK ) and (R PEoEK ) in molar ratios ranging from 90 / 10 to 55 / 45 (R PEEK ) / (R PEoEK ) is present in the PEEK-PEoEK copolymer. However, it should generally be understood that the preferred PEEK-PEoEK copolymer for the film of the present invention is one in which the molar ratio (R) is [missing information]. PEEK ) / (R PEoEK The copolymer is preferably in the range of 85 / 15 to greater than 55 / 45, more preferably in the range of 85 / 15 to 60 / 40, and even more preferably in the range of 80 / 20 to 65 / 35.

[0024] Repeating unit (R) PEEK It can be expressed by the following formula:

[0025] and

[0026] Repeating unit (R) PEoEK It can be expressed by the following formula:

[0027]

[0028] Each R 1 and R 2They may be the same as or different from each other, and each time they appear, they are independently selected from the group consisting of: halogens, alkyl, alkenyl, alkynyl, aryl, ether, thioether, carboxylic acid, ester, amide, imide, alkali metal or alkaline earth metal sulfonates, alkyl sulfonates, alkali metal or alkaline earth metal phosphonates, alkyl phosphonates, amines, and quaternary ammonium.

[0029] Each a and b is independently selected from a group of integers ranging from 0 to 4.

[0030] In some preferred embodiments, in equation (A), each a is zero, such that the repeating unit (R) PEEK ) is a repeating unit with the following formula:

[0031]

[0032] In some preferred embodiments, in equation (B), each b is zero, such that the repeating unit (R) PEoEK ) is a repeating unit with the following formula:

[0033]

[0034] Preferably, the repeating unit (R) PEEK ) is a repeating unit with equation (A-1), and the repeating unit (R) PEoEK ) is a repeating unit with equation (B-1).

[0035] The PEEK-PEoEK copolymer of the present invention may additionally contain repeating units (R) different from those detailed above. PEEK ) and (R PEoEK The repeating unit (R) PAEK In this case, the repeating unit (R) PAEK The amount of ) can be included relative to the total number of repeating units of the PEEK-PEoEK copolymer between 0.1 and less than 50 mol.%, preferably less than 10 mol.%, more preferably less than 5 mol.%, and most preferably less than 2 mol.%.

[0036] When different from the repeating unit (R) PEEK ) and (R PEoEK The repeating unit (R) PAEK When present in the PEEK-PEoEK copolymer of the present invention, it differs from the repeating unit (R) described above. PEEK ) and (R PEoEK These repeating units (R) PAEK It usually conforms to any one of the following formulas (KA) to (KM):

[0037]

[0038]

[0039] In each of the formulas (KA) to (KM) above, each R' may be the same as or different from each other, and is independently selected each time from a C1-C12 alkyl, alkenyl, alkynyl, or aryl group that optionally contains one or more heteroatoms; sulfonic acid and sulfonate / ester groups; phosphonic acid and phosphonate / ester groups; amine and quaternary ammonium groups; and each j' may be the same as or different from each other, and is independently selected each time from an integer from 0 to 4, preferably j' equal to zero. In the repeating unit (R PAEK In ), the corresponding phenylene moiety can independently have 1,2-, 1,4-, or 1,3- bonds to other moiety in the repeating unit that are different from R'.

[0040] Preferably, the PEEK-PEoEK copolymer in the membrane used in the present invention is substantially composed of repeating units (R) as detailed above. PEEK ) and (R PEoEK Therefore, in some preferred embodiments, the PEEK-PEoEK copolymer is essentially composed of repeating units (R). PEEK ) and (R PEoEK It consists of ) . As used in this paper, the expression "basically composed of repeating units (R) PEEK ) and (R PEoEK "Composition" refers to a different type of repeating unit (R) as detailed above. PEEK ) and (R PEoEK Any additional repeating unit may be present in the PEEK-PEoEK copolymer in an amount of up to 2 mol.%, up to 1 mol.%, or up to 0.5 mol.%, relative to the total molar number of repeating units in the PEEK-PEoEK copolymer, and so as not to substantially alter the advantageous properties of the PEEK-PEoEK copolymer.

[0041] When measured at 150°C or lower, the preferred PEEK-PEoEK copolymers typically have a solubility of less than 0.2% wt in N-methylpyrrolidone (NMP), N,N-dimethylacetamide (DMAc), and N,N-dimethylformamide (DMF). In some embodiments, the PEEK-PEoEK copolymers used in conjunction with adhesive films are advantageously substantially insoluble in the solvents listed above, making them particularly suitable for applications requiring improved chemical resistance and / or, in some cases, fluid resistance.

[0042] In some embodiments, the PEEK-PEoEK copolymer has a melt temperature (Tm) of less than or equal to 320°C, preferably less than or equal to 315°C, as measured by differential scanning calorimetry (DSC) according to ASTM D3418-03, E1356-03, and E794-06. m).

[0043] Melting temperature Tm, glass transition temperature Tg, and heat of fusion (ΔH) were measured by differential scanning calorimetry (DSC) according to ASTM D3418-03, E1356-03, E793-06, and E794-06 standards, with a heating and cooling rate of 10 °C / min, scanning from 30 °C to 400 °C.

[0044] Advantageous adhesive films are prepared from PEEK-PEoEK copolymers with a melt temperature (Tm) of less than or equal to 320°C, preferably less than or equal to 310°C and / or at least 270°C.

[0045] In some embodiments, the PEEK-PEoEK copolymer has a heat of fusion (ΔH) of at least 4 J / g, preferably at least 5 J / g, or at least 10 J / g, more preferably at least 15 J / g. In some aspects, the PEEK-PEoEK copolymer may have a heat of fusion (ΔH) of up to 75 J / g, preferably up to 65 J / g.

[0046] In some embodiments, the PEEK-PEoEK copolymer has a glass transition temperature (Tg) of less than or equal to 165°C, preferably less than or equal to 160°C, less than or equal to 155°C, or less than or equal to 150°C, as measured by differential scanning calorimetry (DSC) according to ASTM D3418-03 and E1356-03. g In some embodiments, the PEEK-PEoEK copolymer has a glass transition temperature (Tg) of 130°C or higher, preferably 135°C or higher, as measured in a differential scanning calorimeter (DSC) according to ASTM D3418-03 and E1356-03.

[0047] Depending on requirements, PEEK-PEoEK copolymers can be manufactured at higher or lower molecular weights to allow for adjustment of the melt copolymer viscosity over a very wide range. In some embodiments, the PEEK-PEoEK copolymer can have a viscosity as specified in ASTM D3835 at 410°C and 46.3s. -1 The measured value is at least 0.10 kN / m. 2 More preferably at least 0.20 kN / m 2 And the optimal value is at least 0.25 kN / m. 2 The melt viscosity (MV). In some embodiments, the PEEK-PEoEK copolymer may have the following characteristics according to ASTM D3835 at 410°C and 46.3s. -1 The measured value is at most 1.50 kN / m. 2 More preferably at least 1.30 kN / m 2And the optimal value is at least 1.10 kN / m. 2 Melt viscosity (MV).

[0048] The stability of the PEEK-PEoEK copolymer in the melt phase was determined to be 46.3 s at 410 °C. -1 The melt viscosity is determined by comparing the melt viscosity at a shear rate after a residence time of 40 minutes with the melt viscosity at the same temperature and shear rate after a residence time of 10 minutes, wherein the melt viscosity is determined using a capillary rheometer according to ASTM D3835 using a conical die (diameter = 1.016 mm, length = 20.32 mm, cone angle = 120°). The melt stability of the PEEK-PEoEK copolymer is preferably less than 1.23, more preferably less than 1.22, and more preferably less than 1.21. Preferably, the melt stability is greater than 0.60, more preferably greater than 0.65, and most preferably greater than 0.70.

[0049] FT-IR analysis of PEEK-PEoEK copolymers can provide valuable information about the copolymer's microstructure, including the linkage of various monomers, the characteristics of end groups, and the presence or absence of defects. According to certain preferred embodiments, the PEEK-PEoEK copolymer possesses a microstructure that allows for the visualization of its FT-IR spectra on polymer powder at 600 and 1000 cm⁻¹. -1 When records are made in ATR mode, the following inequality must be satisfied:

[0050] (i) in It is at 700cm -1 The absorbance at that point, and It is at 704cm -1 Absorbance at that location;

[0051] (ii) in It is 816cm -1 absorbance at the location and It is at 835cm -1 Absorbance at that location;

[0052] (iii) in It is 623cm -1 absorbance at the location and It is 557cm -1 Absorbance at that location;

[0053] (iv) in It is at 928cm -1 absorbance at the location and It is at 924cm-1 The absorbance at that location.

[0054] PEEK-PEoEK copolymers with specific microstructures (including monomer linkages, end groups, and defects) (characterized by the aforementioned spectral features) can provide improved chemical and mechanical properties.

[0055] The PEEK-PEoEK copolymer can have a calcium content of less than 5 ppm, which is measured by inductively coupled plasma optical emission spectrometry (ICP-OES) using standards with known calcium contents. According to these preferred embodiments, the PEEK-PEoEK copolymer can have a calcium content of less than 4 ppm, less than 3 ppm, or even more preferably less than 2.5 ppm.

[0056] In these preferred embodiments, the PEEK-PEoEK copolymer may also have a sodium content of less than 1,000 ppm, which is measured by inductively coupled plasma optical emission spectrometry (ICP-OES) using standards with known sodium contents. Preferably, the PEEK-PEoEK copolymer may have a sodium content of less than 900 ppm, less than 800 ppm, or even more preferably less than 500 ppm.

[0057] In some embodiments, the PEEK-PEoEK copolymer may have a phosphorus content of at least 6 ppm, which is measured by inductively coupled plasma optical emission spectrometry (ICP-OES) using standards with known phosphorus contents. Preferably, the PEEK-PEoEK copolymer has a phosphorus content of at least 10 ppm, at least 15 ppm, or even more preferably at least 20 ppm.

[0058] In the adhesive film of the present invention, it may be advantageous to select a PEEK-PEoEK copolymer with increased thermal stability, which may be particularly advantageous when the parts to be joined by the adhesive film are high melt temperature polymers and / or the final parts must withstand high operating temperatures. Therefore, in some embodiments, the PEEK-PEoEK copolymer has a peak degradation temperature of at least 550°C, more preferably at least 551°C, and even more preferably at least 552°C, as measured by TGA according to ASTM D3850.

[0059] Methods suitable for manufacturing PEEK-PEoEK copolymers are generally known in the art. In general, the PEEK-PEoEK copolymers used herein are manufactured by a method comprising reacting at least one difluorinated compound having formula (C):

[0060]

[0061] A mixture of dihydroxy compounds having formulas (D) and (E) reacts in a polar organic solvent in the presence of a base (such as Na₂CO₃, K₂CO₃, or combinations thereof):

[0062]

[0063] The molar ratio (D) / (E) ranges from 90 / 10 to 55 / 45, where R 3 R 4 and R 5 With the meanings specified above, c, d, and e are each independently selected from a group of integers ranging from 0 to 4. Preferably, each of c, d, and e is zero.

[0064] In the embodiments, the PEEK-PEoEK copolymer used in the membrane of the present invention is prepared as described in WO 2020 / 254097A1, the entire contents of which are incorporated herein by reference.

[0065] Membrane composition and method for making membrane

[0066] In some embodiments, the membrane of the present invention comprises at least one additive that is different from the PEEK-PEoEK copolymer. Suitable additives include, but are not limited to: (i) colorants, such as dyes; (ii) pigments, such as titanium dioxide, zinc sulfide, and zinc oxide; (iii) light stabilizers, such as UV stabilizers; (iv) heat stabilizers; (v) antioxidants, such as organophosphites and phosphonites; (vi) acid scavengers; (vii) processing aids; (viii) nucleating agents; (ix) internal and / or external lubricants; (x) flame retardants; (xi) smoke suppressants; (x) antistatic agents; (xi) anti-caking agents; (xii) conductive additives, such as carbon black and carbon nanofibers; (xiii) plasticizers; (xiv) flow modifiers; (xv) fillers; (xvi) metal deactivators; and (xvii) flow aids, such as silica.

[0067] According to some embodiments, the membrane of the present invention further comprises at least one nucleating agent. This nucleating agent can be selected from the group consisting of: boron-containing compounds (e.g., boron nitride, sodium tetraborate, potassium tetraborate, calcium tetraborate, etc.), alkaline earth metal carbonates (e.g., calcium magnesium carbonate), oxides (e.g., titanium oxide, aluminum oxide, magnesium oxide, zinc oxide, antimony trioxide, etc.), silicates (e.g., talc, sodium aluminum silicate, calcium silicate, magnesium silicate, etc.), salts of alkaline earth metals (e.g., calcium carbonate, calcium sulfate, etc.), nitrides, etc. The nucleating agent can also be carbon-based. Nucleating agents in this category include graphite, graphene, graphite nanosheets, and graphene oxide. It can also be carbon black and other forms of carbon. Particularly good results have been obtained when the nucleating agent is boron nitride.

[0068] Typically, the membrane contains less than 20 wt.% of additives, preferably less than 10 wt.%, more preferably less than 5 wt.%, and even more preferably less than 2 wt.%, most preferably less than 1 wt.%.

[0069] In a preferred embodiment, the membrane is free of any reinforcing fibers, i.e., it contains less than 0.5 wt.%, preferably less than 0.1 wt.%, of any reinforcing fibers. The term "fiber" has its common meaning as known to those skilled in the art and may include one or more fibrous materials suitable for reinforcing composite structures, i.e., "reinforcing fibers." As used herein, the term "fiber" refers to organic and / or inorganic fibers having a length of at least 0.5 mm.

[0070] In some embodiments, the film may comprise a blend of more than one polymer, one of which is a PEEK-PEoEK copolymer. According to these embodiments, the adhesive film may comprise 40 wt.% or less (based on the total weight of the polymer matrix) of at least one additional polymer component different from the PEEK-PEoEK copolymer. Such an additional polymer component is advantageously selected from the group consisting of poly(arylene ether sulfone) (PAES) polymers and poly(arylene ether ketone) (PAEK) polymers. When the additional polymer component is a PAES polymer, it may be advantageously selected from the group consisting of polysulfone (PSU), polyphenylene sulfone (PPSU), and poly(ether sulfone) (PES). When the additional polymer component is a PAEK polymer, it may be advantageously selected from the group consisting of poly(ether ether ketone) (PEEK) polymers, poly(ether ketone ketone) (PEKK) polymers, polyether ketone (PEK), polyether ketone ether ketone ketone (PEKEKK), and PEEK-PEDEK copolymers. The additional polymer component may also include polyimides, such as polyetherimide (PEI) or polyamide imide.

[0071] In alternative embodiments, the PEEK-PEoEK copolymer, as detailed above, is the sole polymeric component in the adhesive film. As used herein, the term "polymeric component" means a compound having repeating units and a molecular weight of at least 2,000 g / mol. In some embodiments, the adhesive film comprises less than 3 wt.%, 2 wt.%, 1 wt.%, or 0.5 wt.% of a polymeric component in addition to the PEEK-PEoEK copolymer.

[0072] In some embodiments, the adhesive film comprises at least 90 wt.% of a PEEK-PEoEK copolymer and at least one additive and / or at least one additional polymer component different from the PEEK-PEoEK copolymer. Most preferably, the adhesive film comprises at least 95 wt.%, preferably at least 98 wt.% of a PEEK-PEoEK copolymer and at least one additive.

[0073] The membrane of the present invention may have a thickness of 15 to 800 μm, or even 25 to 600 μm, preferably 30 to 500 μm, more preferably 40 to 300 μm, and most preferably 50 to 250 μm.

[0074] The membrane of the present invention can be prepared by any conventional method known in the field of polymer processing.

[0075] The components of adhesive films are typically processed in film form by cast extrusion, optionally with uniaxial or biaxial orientation. As used herein, the term "film components" includes PEEK-PEoEK copolymers and optionally: at least one additive, at least one additional polymer component other than the PEEK-PEoEK copolymer, or a combination thereof.

[0076] In some embodiments, the method of manufacturing the film includes melt-blending a physical mixture of the film components. Conventional melt-blending equipment can be used, such as co-rotating and counter-rotating extruders, single-screw extruders, co-kneaders, disc extruders, and a variety of other types of extrusion equipment. Preferably, an extruder, more preferably a twin-screw extruder, can be used.

[0077] In some embodiments, the physical mixture is compounded in an extruder and then shredded into granules or pellets. The granules or pellets can then be further processed to manufacture the film of the present invention.

[0078] Alternatively, the physical mixture is compounded in an extruder and then directly formed into a film. A technique particularly suitable for manufacturing the adhesive film of the present invention involves extruding a molten composition through a die having an elongated shape to obtain an extruded strip and casting / calendering the extruded strip to obtain a film. The strip can be calendered into a film by passing it through suitable rollers that can be maintained at a suitable temperature and whose speed can be adjusted to obtain the desired thickness. The thickness of the film is adjusted at the die orifice. Depending on the cooling temperature used to cure the film, the film can be amorphous or semi-crystalline in finished (extruded) form.

[0079] In an advantageous embodiment, the membrane is a single-layer membrane, i.e., it consists of only one layer comprising a PEEK-PEoEK copolymer.

[0080] Methods for manufacturing components

[0081] A second object of the present invention is a method for manufacturing an assembly using a membrane according to the first object of the invention. The method includes the steps of: arranging a membrane according to the first object of the invention between a first component comprising a polymer (P1) and a second component comprising a polymer (P2); and subjecting the membrane to a temperature (T0) suitable for melting the membrane but not melting the polymers (P1) and (P2). m x ).

[0082] Temperature (T) m x Typically, this is greater than the melting temperature of the adhesive film. Temperature (T) m x The temperature can be below 330°C, preferably below 320°C, and more preferably below 310°C. The temperature can be above 270°C. The temperature can be in the range of 270°C to 330°C, preferably in the range of 280°C to 315°C.

[0083] Temperature (T) m x It is preferred to use a temperature lower than that of polymers (P1) and (P2).

[0084] The method preferably includes the following steps: arranging a membrane between a first component containing polymer (P1) and a second component containing polymer (P2); and placing the membrane at a temperature (T) in the range of 280°C to 315°C. m x At this temperature, the melting temperature is suitable for melting films, but not for melting polymers (P1) and polymers (P2).

[0085] Preferably, when the membrane and the polymers (P1) and (P2) are subjected to temperature (T) m x The method includes applying pressure to solidify the components and produce the assembly. Therefore, the method also includes subjecting the membrane to a temperature (T...) m x At the same time, pressure is applied to the first and second components.

[0086] In this method, it is preferable to control the cooling of the adhesive film after melting, so that the PEEK-PEoEK copolymer in the adhesive film develops crystallinity (i.e., it is not amorphous). After cooling, the film preferably has a crystallinity of at least 5%, preferably at least 15%, more preferably at least 20%, and especially at least 23%, as measured herein.

[0087] As used herein, the expression "first component comprising polymer (P1)" refers to a component comprising polymer (P1) having at least one surface (particularly the surface in contact with the adhesive film). The first component may be composed of said polymer (P1). Alternatively, the first component comprises a surface comprising polymer (P1). The surface comprising polymer (P1) typically has a thickness suitable for forming an adhesion with the adhesive film. The thickness may suitably be equal to or greater than 5 μm.

[0088] As used herein, the term "second component containing polymer (P2)" refers to a component containing polymer (P2) having at least one surface (particularly the surface in contact with the adhesive film).

[0089] The second component may be composed of the polymer (P2). Alternatively, the second component includes a surface containing the polymer (P2). The surface containing the polymer (P2) typically has a thickness suitable for forming an adhesive film. The thickness may preferably be equal to or greater than 5 μm.

[0090] Polymer (P1) and polymer (P2) can be the same or different.

[0091] Polymer (P1) and polymer (P2) may be independently selected from crystalline and / or high-temperature thermoplastic polymers. Notable non-limiting examples include, but are not limited to, poly(aryl ether ketone), polyetherimide, polyamide imide, polysulfone, polyethersulfone, polyaryl ether, polycarbonate, liquid crystal polymer, polyphenylene sulfide, polyarylene (polyphenylene oxide), polyamide, polyphthalamide, polyarylene ester, and blends thereof.

[0092] In a preferred embodiment, polymers (P1) and (P2) are independently selected from the group consisting of polyaryletherketones, hereinafter referred to as "PAEK", and blends of polyaryletherketones.

[0093] A suitable PAEK is one containing at least 50 wt.% of repeating units (R) represented by a group consisting of formulas (A) and (KA) to (KM) as defined above. PAEK Those polymers. In some embodiments, the PAEK has at least 60 wt.%, at least 80 wt.%, at least 90 wt.%, at least 95 wt.%, or at least 98 wt.% repeating units (R). PAEK ).

[0094] The PAEK polymer can be a homopolymer, a random, alternating, or block copolymer. When the PAEK polymer is a copolymer, it can contain (i) repeating units (R) of at least two different formulas selected from (A) and (KA) to (KM). PAEK ).

[0095] According to some embodiments, these repeating units (R) PAEK Select a group consisting of units having formulas (J'-A) to (J'-D):

[0096]

[0097] PAEK polymers can be polyetheretherketone (“PEEK”) polymers. As used herein, the term “PEEK polymer” refers to a polymer in which at least 50 wt.% of the repeating units are repeating units of formula J'-A (R PAEK ), especially the repeating unit (R) of equation (A-1) as defined above. PAEKAny polymer of formula J'-A. In some embodiments, at least 75 wt.%, at least 85 wt.%, at least 95 wt.%, or at least 99 wt.% of the repeating units of the PEEK polymer are repeating units of formula J'-A. In some embodiments, 99.99 wt.% of the PEEK polymer are repeating units of formula J'-A, particularly repeating units (R) of formula (A-1). PAEK ).

[0098] PAEK polymers can be polyetherketoneketone (“PEKK”) polymers.

[0099] As used herein, the term "PEKK polymer" refers to a polymer containing repeating units (R... T ) and repeating unit (R) I Any polymer of the PEKK polymer, wherein the combined amount of these repeating units is based on a total molar number of at least 50 mol.% in the PEKK polymer, wherein the repeating units (R) T The expression (T) represents:

[0100]

[0101] And repeating unit (R) I Equation (I) represents:

[0102]

[0103] in:

[0104] - In each of equations (T) and (I), R 1 and R 2 In each case, each is independently selected from the group consisting of: alkyl, alkenyl, alkynyl, aryl, ether, thioether, carboxylic acid, ester, amide, imide, alkali metal sulfonate or alkaline earth metal sulfonate, alkyl sulfonate, alkali metal phosphonate or alkaline earth metal phosphonate, alkyl phosphonate, amine, and quaternary ammonium; and

[0105] -i and j are each an independent integer selected from 0 to 4 in each case.

[0106] To avoid ambiguity, repeating unit (R) T The molar content of ) is defined as:

[0107]

[0108] Repeating unit (R) I The molar content of ) is defined as:

[0109] and

[0110] Therefore, the T / I ratio is defined as:

[0111] According to one embodiment, for each R 1 and R 2 Groups i and j are zero. In other words, repeating units (R) T ) and (R I Both are unreplaced. According to this embodiment, the repeating unit (R) T ) and (R I The following are represented by equations (T') and (I'), respectively:

[0112]

[0113] In some embodiments, polymers (P1) and (P2) are independently selected from PEKK polymers as defined above, with a T / I ratio in the range of 55 / 45 to 85 / 15, preferably from 57 / 43 to 80 / 20, and more preferably from 58 / 42 to 75 / 25.

[0114] In other embodiments, polymers (P1) and (P2) may be independently selected from compositions comprising first and second PEKK polymers, each PEKK polymer characterized by a T / I ratio, wherein the T / I ratio of the first PEKK polymer differs from that of the second PEKK polymer, particularly those compositions having a melt temperature less than or equal to 330°C. In one aspect of the embodiments, the first PEKK polymer preferably has a (T / I) ratio of at least 50 / 50, preferably at least 54 / 46, more preferably at least 56 / 44; most preferably at least 57 / 43 and / or at most 64 / 36, preferably at most 63 / 37, more preferably at most 62 / 38. The second PEKK polymer preferably has a (T / I) ratio of at least 65 / 35, more preferably at least 66 / 34, and more preferably at least 67 / 33; and / or a (T / I) ratio of at most 85 / 15, more preferably at most 83 / 17, and more preferably at most 82 / 18.

[0115] In another aspect of the embodiment, the following inequality is satisfied: (repeating unit (R) in the second PEKK polymer) T (molar content) - (repeating unit (R) in the first PEKK polymer) T The molar content of () is ≤20 mol.%, preferably ≤17 mol.%, more preferably ≤15 mol.%. Typically, the following inequality is also satisfied: (the repeating unit (R) in the second PEKK polymer T (molar content) - (repeating unit (R) in the first PEKK polymer) T The molar content of the substance is ≥3 mol.%, preferably ≥4 mol.%, and more preferably ≥5 mol.%.

[0116] In embodiments of the present invention, polymer PEKK is nucleophilic PEKK, which means that polymer PEKK is produced by polycondensation of aromatic compounds containing dihydroxy and difluorobenzoyl groups and / or aromatic compounds containing hydroxy-fluorobenzoyl groups.

[0117] In an alternative embodiment, the polymer PEKK is nucleophilic PEKK.

[0118] In other embodiments, the polymer (PAEK) is poly(ether ketone) [polymer (PEK)]. As used herein, the expressions "poly(ether ketone)" and "polymer (PEK)" refer to a greater than 50% molar repeating unit (R) therein. PAEK ) is any polymer having repeating units of the formula (K'-C):

[0119]

[0120] % moles are based on the total number of repeating units in the polymer (PEK).

[0121] According to these embodiments, at least 60% mole, at least 70% mole, at least 80% mole, at least 90% mole, at least 95% mole, at least 99% mole, or even substantially all of the repeating units (R) PAEK ) is a repeating unit (K'-C). Preferred polymers (PEK) are those in which substantially all repeating units are units having the formula (K'-C), and it should be understood that end groups, defects, and small amounts of impurities may be present.

[0122] In some embodiments, the polymer (PAEK) is poly(ether diphenyl ether ketone) [polymer (PEDEK)]. As used herein, the expressions "poly(ether diphenyl ether ketone)" or "polymer (PEDEK)" indicate that more than 50% molar repeating units (R) are present therein. K (K'-D) is any polymer having repeating units of the formula (K'-D).

[0123]

[0124] % moles are based on the total number of repeating units in the polymer (PEDEK).

[0125] According to these embodiments, at least 60% mole, at least 70% mole, at least 80% mole, at least 90% mole, at least 95% mole, at least 99% mole, or even substantially all repeating units (R) K The repeating unit (K'-D) is as detailed above. Preferred polymers (PEDEK) are those in which substantially all repeating units are units having the formula (K'-D), and it should be understood that end groups, defects, and small amounts of impurities may be present.

[0126] In some other embodiments, the polymer (PAEK) is a poly(ether diphenyl ether ketone)-poly(ether ether ketone) copolymer [polymer (PEEK-PEDEK)]. As used herein, the expression "poly(ether diphenyl ether ketone)-poly(ether ether ketone) copolymer" or "polymer (PEEK-PEDEK)" means that more than 50% molar repeating units (R) are present therein. K (K'-A) is any polymer having a mixture of repeating units of the formula (K'-A) and (K'-D) in a relative molar ratio of (K'-A):(K'-D) of 95:5 to 5:95, preferably 80:20 to 20:80.

[0127] In some embodiments, the polymer (P1) may be part of a first composition, which may include the polymer (P1) and a filler. The filler may include fibrous fillers or non-fibrous fillers. Alternatively, the filler may include both fibrous and non-fibrous fillers.

[0128] Alternatively, the polymer (P2) may be part of a second composition, which may include the polymer (P2) and a filler. The filler may include fibrous fillers or non-fibrous fillers. Alternatively, the filler may include both fibrous and non-fibrous fillers.

[0129] Suitable fiber fillers include, for example, carbon fibers, graphite fibers, glass fibers such as E-glass fibers, ceramic fibers such as silicon carbide fibers, synthetic polymer fibers such as aramid fibers, polyimide fibers, high-modulus polyethylene (PE) fibers, polyester fibers, and polybenzoxazole fibers such as poly(p-phenylene-benzobisoxazole) (PBO) fibers, aramid fibers, boron fibers, basalt fibers, quartz fibers, alumina fibers, zirconia fibers, and mixtures thereof. The fibers can be continuous or discontinuous, and can be aligned or randomly oriented.

[0130] In some embodiments, the fiber comprises at least one carbon fiber. As used herein, the term "carbon fiber" is intended to include graphitized, partially graphitized, and ungraphitized carbon-reinforced fibers, and mixtures thereof. Carbon fibers can be obtained by heat treatment and pyrolysis of various polymer precursors, such as synthetic fibers, polyacrylonitrile (PAN), aromatic polyamides, or phenolic resins; carbon fibers can also be obtained from pitch materials. The term "graphite fiber" is intended to refer to carbon fibers obtained by high-temperature pyrolysis (above 2000°C) of carbon fibers, wherein the carbon atoms are arranged in a manner similar to that of graphite. Carbon fibers are preferably selected from the group consisting of PAN-based carbon fibers, pitch-based carbon fibers, graphite fibers, and mixtures thereof.

[0131] In some embodiments, the fiber comprises at least one glass fiber. The glass fiber may have a circular or non-circular cross-section (such as an elliptical or rectangular cross-section). When the glass fiber used has a circular cross-section, it preferably has an average glass fiber diameter of 3 to 30 μm, particularly preferably 5 to 12 μm. Depending on the type of glass from which they are made, different types of glass fibers with circular cross-sections are commercially available. Notably, glass fibers made of E- or S-glass can be cited as examples. In some embodiments, the glass fiber is a standard E-glass material with a non-circular cross-section. In some embodiments, the polymer composition comprises S-glass fibers with a circular cross-section.

[0132] In embodiments, the composite material of the present invention comprises continuous fibers. As referred to herein, "continuous fibers" means fibers having a length of 3 mm or more typically 10 mm and an aspect ratio of 500 or more typically 5000.

[0133] In one embodiment of the invention, the first component is a composite material comprising one or more layers containing fibers and a polymer (P1). The polymer (P1) is impregnated, coated, or laminated onto the fibers.

[0134] In another embodiment of the invention, the second component is a composite material comprising one or more layers containing fibers and a polymer (P2). The polymer (P2) is impregnated, coated, or laminated onto the fibers.

[0135] Another object of the present invention is a component comprising a first component containing a polymer (P1), a second component containing a polymer (P2), and a membrane of the present invention located between and bonded to the first and second components.

[0136] The term “adhesion” in this article means the attachment of materials to each other, preferably a permanent attachment.

[0137] This component can be part of a component or part used in the aerospace and automotive industries. For example, a component that includes or is composed of components of the present invention can include, but is not limited to, brackets, clips, reinforcing ribs, and other similar types of parts.

[0138] It should be understood that any description (even one relating to a particular embodiment) is applicable to other embodiments of this disclosure and may be interchanged with it.

[0139] The present invention will be described in more detail below by way of non-limiting examples.

[0140] If any patent, patent application, or publication incorporated herein by reference conflicts with the description of this application to the extent that it may lead to ambiguity in terminology, this description shall take precedence.

[0141] Example

[0142] raw material

[0143] 1,2-Dichlorobenzene, terephthaloyl chloride, isophthaloyl chloride, 3,5-dichlorobenzoyl chloride, aluminum chloride (AlCl3), and methanol were purchased from Sigma Aldrich.

[0144] 1,4-Bis(4-phenoxybenzoyl)benzene is prepared according to IN patent 193687 (filed on June 21, 1999 and incorporated herein by reference).

[0145] Hydroquinone, optical grade, is obtained from Eastman Chemical Company, USA. It contains 0.38 wt% moisture, which is used to adjust the feed weight. All indicated weights include moisture.

[0146] Resorcinol, ACS reagent grade, is obtained from Aldrich, Inc.

[0147] 4,4'-Biphenyl, polymer grade, was obtained from SI Corporation (SI, USA).

[0148] Catechol, in flakes, is obtained from Solvay USA. Its purity, determined by GC, is 99.85%. It contains 680 ppm water, which is used to adjust the feed weight. All indicated weights include water.

[0149] 4,4'-Difluorobenzophenone, polymer grade (99.8%+), was obtained from Malwa Company, India.

[0150] Diphenyl sulfone (polymer grade) was obtained from Proviron (99.8% pure).

[0151] Sodium carbonate, light soda ash, was obtained from Solvay SA, France.

[0152] Potassium carbonate, has d 90 <45μm, obtained from Armand Products.

[0153] The lithium chloride (anhydrous grade) was obtained from Acros.

[0154] 1,4-bis(4'-fluorobenzoyl)benzene (1,4-DFDK) and 1,3-bis(4'-fluorobenzoyl)benzene (1,3-DFDK) were prepared by Friedel-Crafts acylation of fluorobenzene according to Example 1 of U.S. Patent No. 5,300,693 (incorporated herein by reference in its entirety). A fraction of 1,4-DFDK was purified by recrystallization in chlorobenzene as described in U.S. Patent No. 5,300,693, and another fraction was purified by recrystallization in DMSO / ethanol. The 1,4-DFDK purified by recrystallization in DMSO / ethanol was used as 1,4-DFDK in the polymerization reaction to produce PEKK as described below, while the 1,4-DFDK recrystallized in chlorobenzene was used as a precursor for 1,4-bis(4'-hydroxybenzoyl)benzene (1,4-BHBB).

[0155] 1,4-BHBB and 1,3-bis(4'-hydroxybenzoyl)benzene (1,3-BHBB) were produced by hydrolyzing 1,4-DFDK and 1,3-DFDK, respectively, following the procedure described in Example 1 of U.S. Patent No. 5,250,738 to Hackenbruch et al. (incorporated herein by reference in its entirety). They were purified by recrystallization in DMF / ethanol.

[0156] Melting temperature (T) m Determination of crystallization temperature (Tc) and heat of fusion

[0157] Melting temperature T m The peak temperature of melting endothermic reaction during the second heating scan in a differential scanning calorimeter (DSC) was determined according to ASTM D3418-03, E1356-03, E793-06, and E794-06. Details of the procedure used in this invention are as follows: A TA instrument DSC Q20 was used, with nitrogen (99.998% purity, 50 mL / min) as the carrier gas. Temperature and heat flow rate calibration was performed using indium. Sample sizes ranged from 5 to 7 mg. Weights were recorded as ±0.01 mg.

[0158] The heating cycle is:

[0159] - First heating cycle: 10.00℃ / min, from 30.00℃ to 400.00℃, isothermal at 400.00℃ for 1 min;

[0160] - First cooling cycle: 10.00℃ / min, from 400.00℃ to 30.00℃, isothermal for 1 min;

[0161] - Second heating cycle: 10.00℃ / min, from 30.00℃ to 400.00℃, isothermal at 400.00℃ for 1 min.

[0162] Melting temperature T m The peak temperature at which melting endotherm was determined during the second thermal scan was also determined. The enthalpy of melting was determined during the second thermal scan. The melting of the composition was considered as the area above a linear baseline drawn from 220°C to temperatures above the last endothermic curve. When evaluating the crystallinity of the film in an adhesive structure (part), the heat of melting was determined during the first thermal scan.

[0163] Crystallization temperature T c The peak temperature of the exothermic crystallization curve was determined during the first cooling scan.

[0164] Determination of melt viscosity

[0165] Melt viscosity was measured using a capillary rheometer according to ASTM D3835. A mold with the following characteristics was used at 380°C or 410°C (as shown) and for 46.3 seconds. -1 Readings were obtained at the following shear rates after 10 minutes (reported in Table 2) and 40 minutes of residence time: diameter = 1.016 mm, length = 20.32 mm, cone angle = 120°. Melt stability VR40 was measured by the ratio of viscosity at 40 minutes to viscosity at 10 minutes.

[0166] Determination of tensile properties

[0167] A substrate measuring 762mm × 762mm × 3.2mm was prepared from a polymer by compression molding of 30g of polymer under the following conditions:

[0168] Preheat at T1

[0169] T1 / 20 minutes, 2000 kg-f

[0170] T1 / 2 minute, 2700 kg-f

[0171] Cool to 30°C within 40 minutes, 2000 kg-f

[0172] The results table indicates the T1 value used for the polymer. The substrate was then annealed at 200°C for 3 hours.

[0173] A 762mm × 762mm × 3.2mm compression-molded substrate was machined into a Type V ASTM tensile specimen, and specimens of these different polymer compositions were subjected to tensile testing at room temperature (i.e., 23°C) at a speed of 0.05 inches / minute (0.127 cm / min) on three samples according to ASTM Method D638. The mean of the three specimens is expressed as the standard deviation in parentheses.

[0174] Synthesis Example

[0175] Comparative Example 1: PEKK with a T / I ratio of 60 / 40

[0176] In a 500 mL 4-necked reaction flask equipped with a stirrer, an N2 inlet tube, a Claisen adapter with a thermocouple inserted into the reaction medium, and a Dean-Stark trap with a condenser and dry ice trap, 112.50 g of diphenyl sulfone, 33.390 g of 1,3-BHBB, 6.372 g of 1,4-BHBB, and 41.051 g of 1,4-DFDK were introduced. The contents of the flask were evacuated under vacuum and then filled with high-purity nitrogen (containing less than 10 ppm of O2). The reaction mixture was then placed under constant nitrogen purging (60 mL / min).

[0177] The reaction mixture was slowly heated to 270°C. At 270°C, 13.725 g of Na₂CO₃ and 0.086 g of K₂CO₃ were added to the reaction mixture over 60 minutes using a powder dispenser. At the end of the addition, the reaction mixture was heated to 320°C at 1°C / min. After 2 minutes at 320°C, 1.207 g of 1,4-DFDK was added to the reaction mixture while the reactor was purged with nitrogen. After 5 minutes, 0.529 g of lithium chloride was added to the reaction mixture. After 10 minutes, an additional 0.503 g of 1,4-DFDK was added to the reactor and the reaction mixture was maintained at the temperature for 15 minutes. An additional 25 g of diphenyl sulfone was added to the reaction mixture and it was maintained with stirring for 15 minutes. The reactor contents were then poured from the reactor into a stainless steel pan and cooled. The solids were crushed and ground in a grinder (through a 2 mm sieve). Diphenyl sulfones and their salts were extracted from the mixture using acetone and water at pH values ​​between 1 and 12. 0.67 g of NaH₂PO₄·2H₂O and 0.62 g of Na₂HPO₄ were dissolved in 1200 mL of deionized water for final washing. The powder was then removed from the reactor and dried under vacuum at 120 °C for 12 hours, yielding 72 g of a yellow powder. The properties of the final polymer are detailed in Table 2.

[0178] Comparative Example 2: Preparation of PEEK-PEDEK 75 / 25 copolymer

[0179] In a 500 mL 4-necked reaction flask equipped with a stirrer, an N2 inlet tube, a Claisen adapter with a thermocouple inserted into the reaction medium, and a Dean-Stark water separator with a condenser and dry ice trap, 128.21 g of diphenyl sulfone, 20.297 g of hydroquinone, 11.411 g of 4,4'-biphenol, and 54.377 g of 4,4'-difluorobenzophenone were introduced. The contents of the flask were evacuated under vacuum and then filled with high-purity nitrogen (containing less than 10 ppm of O2). The reaction mixture was then subjected to a constant nitrogen purging (60 mL / min).

[0180] The reaction mixture was slowly heated to 150°C. At 150°C, a mixture of 26.955 g of Na₂CO₃ and 0.169 g of K₂CO₃ was added to the reaction mixture over 30 minutes using a powder dispenser. At the end of the addition, the reaction mixture was heated to 320°C at a rate of 1°C / min. After 13 minutes at 320°C, 3.742 g of 4,4'-difluorobenzophenone was added to the reaction mixture while the reactor was purged with nitrogen. After 5 minutes, 1.039 g of lithium chloride was added to the reaction mixture. After 10 minutes, an additional 2.138 g of 4,4'-difluorobenzophenone was added to the reactor and the reaction mixture was maintained at this temperature for 15 minutes.

[0181] The reactor contents were then poured into an SS pan and cooled. The solids were crushed and ground in a grinder (through a 2 mm sieve). Diphenyl sulfones and the salt were extracted from the mixture with acetone and water at a pH between 1 and 12. The powder was then removed from the reactor and dried under vacuum at 120°C for 12 hours, yielding 74 g of white powder.

[0182] At 410℃, for 46 seconds -1 The melt viscosity, measured by capillary rheology, is 0.28 kN-s / m. 2 .

[0183] The properties of the final polymer are detailed in Table 2.

[0184] Comparative Example 3: Preparation of PEEK-PEmEK 70 / 30 copolymer

[0185] In a 1000 mL 4-necked reaction flask equipped with a stirrer, an N2 inlet tube, a Clayson adapter with a thermocouple inserted into the reaction medium, and a Dean-Stark water separator with a condenser and dry ice trap, 330.00 g of diphenyl sulfone, 37.949 g of hydroquinone, 16.234 g of resorcinol, and 109.875 g of 4,4'-difluorobenzophenone were introduced. The contents of the flask were purged under vacuum and then filled with high-purity nitrogen (containing less than 10 ppm of O2). The reaction mixture was then subjected to a constant nitrogen purging (60 mL / min).

[0186] The reaction mixture was slowly heated to 150°C. At 150°C, a mixture of 54.099 g of Na₂CO₃ and 0.170 g of K₂CO₃ was added to the reaction mixture over 30 minutes using a powder dispenser. At the end of the addition, the reaction mixture was heated to 300°C at a rate of 1°C / min. After 57 minutes at 300°C, 17.135 g of 4,4'-difluorobenzophenone was added to the reaction mixture while the reactor was purged with nitrogen. After 5 minutes, 2.081 g of lithium chloride was added to the reaction mixture. After 10 minutes, an additional 4.284 g of 4,4'-difluorobenzophenone was added to the reactor and the reaction mixture was maintained at this temperature for 15 minutes.

[0187] The reactor contents were then poured into an SS pan and cooled. The solids were crushed and ground in a grinder (through a 2 mm sieve). Diphenyl sulfones and the salt were extracted from the mixture with acetone and water at a pH between 1 and 12. The powder was then removed from the reactor and dried under vacuum at 100°C for 12 hours, yielding 125 g of light brown powder.

[0188] At 410℃, for 46 seconds -1 The melt viscosity, measured by capillary rheology, is 0.70 kN-s / m. 2 The properties of the final polymer are detailed in Table 2.

[0189] Example 4: Preparation of PEEK-PEoEK 80 / 20 copolymer

[0190] In a 1000 mL 4-necked reaction flask equipped with a stirrer, an N2 inlet tube, a Clayson adapter with a thermocouple inserted into the reaction medium, and a Dean-Stark water separator with a condenser and dry ice trap, 343.63 g of diphenyl sulfone, 61.852 g of hydroquinone, 15.426 g of catechol, and 154.573 g of 4,4'-difluorobenzophenone were introduced. The contents of the flask were evacuated under vacuum and then filled with high-purity nitrogen (containing less than 10 ppm of O2). The reaction mixture was then subjected to a constant nitrogen purging (60 mL / min).

[0191] The reaction mixture was slowly heated to 150°C. At 150°C, a mixture of 76.938 g of Na₂CO₃ and 0.484 g of K₂CO₃ was added to the reaction mixture over 30 minutes using a powder dispenser. At the end of the addition, the reaction mixture was heated to 320°C at a rate of 1°C / min. After 1 minute at 320°C, the reaction was terminated in three stages: 18.329 g of 4,4'-difluorobenzophenone was added to the reaction mixture while the reactor was purged with nitrogen. After 5 minutes, 2.338 g of lithium chloride was added to the reaction mixture. After 10 minutes, an additional 6.110 g of 4,4'-difluorobenzophenone was added to the reactor and the reaction mixture was maintained at the temperature for 15 minutes.

[0192] The reactor contents were then poured into an SS pan and cooled. The solids were crushed and ground in a grinder (through a 2 mm sieve). Diphenyl sulfones and the salt were extracted from the mixture with acetone and water at a pH between 1 and 12. The powder was then dried under vacuum at 120°C for 12 hours, yielding 174 g of white powder.

[0193] The melt viscosity, measured by capillary rheology at 410℃ and 46 s⁻¹, was 1.50 kN⁻¹ / m. 2 The properties of the polymer are disclosed in Table 2 below.

[0194] Example 5-7: Preparation of PEEK-PEoEK 75 / 25 and 70 / 30 copolymers

[0195] The same procedure as in Example 4 was followed, but the following amounts of reagents were used as shown in Table 1. The properties of the resulting polymer are shown in Table 2.

[0196] Table 1: Reagents used to prepare reagents for Examples 5-7

[0197] reagents unit Example 5 Example 6 Example 7 PEEK / PEoEK 75 / 25 75 / 25 70 / 30 diphenyl sulfone g 340.54 343.63 343.63 hydroquinone g 57.500 57.987 54.121 catechol g 19.109 19.282 23.139 4,4'-Difluorobenzophenone g 153.181 154.573 153.351 <![CDATA[Na2CO3]]> g 76.245 76.938 76.938 <![CDATA[K2CO3]]> g 0.479 0.484 0.484 Time at 320℃ minute 33 16 73 4,4'-Difluorobenzophenone (in the first termination) g 10.596 18.329 18.329 Lithium chloride (in the second termination) g 2.941 2.388 2.388 4,4'-Difluorobenzophenone (in the third termination) g 6.055 343.63 6.110 polymer weight g 185 188 188 <![CDATA[Na2HPO4]]> g 1.86 1.86 1.86

[0198] Table 2 presents the characteristics of the samples prepared according to Examples 1-7.

[0199] Table 2

[0200]

[0201]

[0202] The data presented in Table 2 indicate that PEEK-PEoEK copolymers are characterized by typically low Tg. m Compared to known low-Tm PAEK, it has the following advantages:

[0203] -As shown by the calorific value, compared to PEKK for the same T m Increased crystallinity (CE1 vs E4);

[0204] - Higher Tg compared to PEEK-PEmEK, resulting in higher continuous operating temperatures;

[0205] -Compared to PEEK-PEDEK for the same T m Improved mechanical properties (CE2 vs E4)

[0206] - Achieves lower T compared to PEEK-PEDEK m Possibility (T) m <295℃).

[0207] Examples 10-11 - General Procedures for Preparing Adhesive Films from Polymers of Examples 5 and CE 3

[0208] Using 26mm with an L / D ratio of 48:1 The ZSK-26 type twin-screw extruder, with its co-rotating, intermeshing sections, converts coarse polymer powder into granules through melt compounding. The powder is fed by gravity into the feed hopper of extruder barrel section 1 at a rate of 37 lbs / hr (16.8 kg / hr). The extruder has 12 barrel sections, with sections 2 through 12, and the die, all heated under a temperature profile set at 350°C. The melt temperature of the extrudate is measured using a handheld pyrometer as it exits the die.

[0209] Throughout the compounding run, the extrudate melt temperature was approximately 380°C. The screw speed was set at 200 rpm, and the extruder torque reading was approximately 50% throughout the production run. Vacuum ventilation (at a vacuum level of 26 inches Hg) was applied at barrel section 10 during compounding to remove moisture and any possible residual volatiles from the compound. The extrudate from this run was stretched and cooled in a water bath, and then granulated into pellets with a diameter of approximately 2.7 mm and a length of 3.0 mm.

[0210] The blended pellets were processed into a film with a nominal thickness of 140 micrometers and a width of 8.5 to 9 cm using melt extrusion on a single-screw extruder. An OCS (Optical Control System, GmbH) extruder was used for this purpose. This extruder had a single-stage, non-vented screw with a diameter of 20 mm and an L / D ratio of 30. It was fitted with a 125 mm wide die with a gap thickness of 0.5 mm. The extruder barrel had four heating sections, operated from back to front, with temperatures set to approximately: 335°C, 360°C, 360°C, and 370°C. The die was set to 390°C. Before extrusion into a film, the pellets were dried overnight (approximately 16 hours) in a dry air convection oven set to 150°C. The blend was extruded using a screw speed of 28 rpm and a productivity of approximately 4 lb / hr (1.8 kg / hr). The film was formed and stretched on two cooling rollers, with the first (top) and second (bottom) rollers set at 140 and 145°C, respectively.

[0211] Example 11: Component fabrication and fracture toughness testing

[0212] The fracture toughness (G1c) is as follows: a laminate (305mm × 305mm size) is manufactured, wherein the layer in the crack plane is a fusion-bonded film fused to the surface of a fiber-reinforced composite substrate. APC (polymer of Example 8) / AS4D unitape with a nominal fiber area weight of 145 gsm and a resin content of 34 wt.% was cut and stacked to form a 16-layer quasi-isotropic (+45° / 0° / -45° / 90° 02s) stack. On top of this stack, a layer of type 108 glass fiber fabric was placed to cover the entire surface, followed by a 280 mm × 305 mm × 0.125 mm membrane from Example 10, with three edges aligned with the edges of the stack. The other edge had a 305 mm × 25 mm × 0.05 mm thick anti-stick coating, Kapton film, which would act as a crack initiator once the board was bonded. The remainder of the stack was formed by reversing the order of material placement, starting with the type 108 glass fiber fabric and then the 16 layers of quasi-isotropic material.

[0213] The laminate was then placed on a flat steel tool and vacuum-packed (710-730 mm Hg vacuum) for treatment in a high-temperature autoclave. The hot-pressing cycle involved a linear temperature rise to 375°C, at which point a pressure of 6.7 bar was applied and held for 15 minutes, followed by cooling the laminate at 6.7 bar (670 kPa) pressure and 711 mm Hg. Before removal from the autoclave, the pressure was released at 93°C and the laminate was cooled to room temperature. The thickness of the resulting plate was measured, and the laminate was then machined into 1 inch × 12 inch (2.5 cm × 30.5 cm) specimens for G1c fracture toughness measurements.

[0214] Table 3: G1c results during RTA

[0215]

[0216] Data shows that the use of the adhesive film according to the invention (Example 5) provides an improved bond to the laminated material, as demonstrated by the high fracture toughness strength.

Claims

1. A component comprising a first part comprising a polymer (P1), a second part comprising a polymer (P2), and a film comprising at least one PEEK-PEoEK copolymer, the PEEK-PEoEK copolymer comprising at least 50 mol.% of repeating units (R) relative to the total molar number of repeating units in the PEEK-PEoEK copolymer. PEEK ) and repeating unit (R) PEoEK ),in: - Repeating unit (R) PEEK ) is a repeating unit with the following formula: ,and - Repeating unit (R) PEoEK ) is a repeating unit with the following formula: , Each R 1 and R 2 They may be the same as or different from each other, and each time they appear, they are independently selected from the group consisting of: halogens, alkyl, alkenyl, alkynyl, aryl, ether, thioether, carboxylic acid, ester, amide, imide, alkali metal or alkaline earth metal sulfonates, alkyl sulfonates, alkali metal or alkaline earth metal phosphonates, alkyl phosphonates, amines, and quaternary ammonium. Each a and b is independently selected from a group of integers ranging from 0 to 4; and The PEEK-PEoEK copolymer contains a molar ratio (R) PEEK ) / (R PEoEK Repeating units (R) ranging from 95 / 5 to 5 / 95 PEEK ) and (R PEoEK ); The membrane is located between and bonded to the first and second components, wherein the melting temperatures of polymers (P1) and (P2) are higher than the melting temperature of the membrane containing the PEEK-PEoEK copolymer.

2. The component as claimed in claim 1, wherein, These repeating units (R) PEEK ) is a repeating unit with the following formula: and / or these repeating units (R) PEoEK ) is a repeating unit with the following formula: 。 3. The component as claimed in claim 1 or 2, wherein, The PEEK-PEoEK copolymer has a molar ratio (R) ranging from 90 / 10 to 55 / 45. PEEK ) / (R PEoEK ).

4. The component as claimed in claim 1 or 2, wherein, The PEEK-PEoEK copolymer has a molar ratio (R) ranging from 85 / 15 to 60 / 40. PEEK ) / (R PEoEK ).

5. The component as claimed in claim 1 or 2, wherein, The PEEK-PEoEK copolymer has a molar ratio (R) ranging from 80 / 20 to 65 / 35. PEEK ) / (R PEoEK ).

6. The component as claimed in claim 1 or 2, wherein, The PEEK-PEoEK copolymer has a melting temperature of less than or equal to 320°C (T0). m ).

7. The component of claim 6, wherein, The PEEK-PEoEK copolymer has a melting temperature of less than or equal to 315°C (T0). m ).

8. The component as claimed in claim 1 or 2, wherein, When measured at 150°C or lower, the solubility of this PEEK-PEoEK copolymer in N-methylpyrrolidone (NMP), N,N-dimethylacetamide (DMAc), and N,N-dimethylformamide (DMF) is less than 0.2% wt.

9. The component of claim 1 or 2, wherein the thickness of the membrane is from 15 to 800 µm.

10. The component as claimed in claim 1 or 2, wherein, Polymer (P1) and polymer (P2) are liquid crystal polymers.

11. The component as claimed in claim 1 or 2, wherein, Polymer (P1) and polymer (P2) are independently selected from the group consisting of polyaryletherketone, polyamide, polyetherimide, polyamideimide, polysulfone, polyethersulfone, polyarylether, polycarbonate, polyphenylene sulfide, polyarylene (polyphenylene oxide), polyphthalamide, polyarylate and blends thereof.

12. The component of claim 11, wherein, Polymer (P1) and polymer (P2) are independently selected from the group consisting of polyaryletherketone, polyetherimide, polyamideimide, polysulfone, polyethersulfone, polyphenylene sulfide, polyphthalamide and blends thereof.

13. The component of claim 11, wherein, Polymer (P1) and polymer (P2) are independently selected from PEKK polymers and mixtures thereof with a T / I ratio ranging from 55 / 45 to 85 / 15.

14. The component of claim 13, wherein, Polymer (P1) and polymer (P2) are independently selected from PEKK polymers and mixtures thereof with a T / I ratio ranging from 57 / 43 to 80 / 20.

15. The component of claim 13, wherein, Polymer (P1) and polymer (P2) are independently selected from PEKK polymers and mixtures thereof with a T / I ratio ranging from 58 / 42 to 75 / 25.

16. The component of claim 11, wherein, The first component is a composite material comprising one or more layers containing fibers and polymers (P1), and / or the second component is a composite material comprising one or more layers containing fibers and polymers (P2).

17. The component of claim 16, wherein, The fiber is either carbon fiber or glass fiber.

18. The component of claim 17, wherein, The fiber is a continuous carbon fiber or glass fiber.

19. A method of manufacturing a component as claimed in any one of claims 1 to 18, the method comprising the following steps: The membrane is disposed between a first component containing polymer (P1) and a second component containing polymer (P2); and the membrane is subjected to a temperature (T) suitable for melting the membrane but not melting the polymer (P1) and polymer (P2). m x ).

20. The method of claim 19, wherein, Temperature (T) m x () higher than the melting temperature of the film.

21. The method of claim 20, wherein, Temperature (T) m x It is lower than the melting temperature of polymers (P1) and (P2).

22. The method of any one of claims 19 to 21, the method comprising the following steps: The membrane is arranged between a first component containing polymer (P1) and a second component containing polymer (P2); And subjecting the membrane to temperatures ranging from 280°C to 315°C (T m x ).

23. The method according to any one of claims 19 to 21, wherein, When the membrane is subjected to the temperature (T) m x When pressure is applied, these components are secured.

Citation Information

Patent Citations

  • Process for purification of 1,4-bis(4-phenoxybenzoyl)benzene

    IN193687B

  • Process for the preparation of 1,4-bis(4-hydroxybenzoyl)-benzene

    US5250738A

  • Process for the preparation of 1,4-bis(4-fluorobenzoyl)-benzene

    US5300693A

  • Polyarylene ether ketone composition for induction welding

    WO2011001103A2

  • Polymeric materials

    WO2015198063A1