A method for in-situ preparation of two-dimensional MXene materials

By using a gradient heating method and glucose as a carbon source, the preparation process of two-dimensional MXene materials was simplified, energy consumption was reduced, etching efficiency and material dispersibility were improved, and the problems of complex processes and high energy consumption in existing technologies were solved, enabling efficient mass production.

CN116692863BActive Publication Date: 2026-11-24SUZHOU BEIKE NANO TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202310759099.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-26
Publication Date
2026-11-24
Estimated Expiration
2043-06-26

AI Technical Summary

Technical Problem

The existing fabrication process for two-dimensional MXene materials is complex and energy-intensive, making it difficult to achieve mass production. Furthermore, metallic impurities are easily introduced during the etching process.

Method used

Two-dimensional MXene materials were prepared in situ in an oxygen-free environment using a gradient heating method. Glucose was used as the carbon source, and the process was simplified and energy consumption was reduced by gradient heating and etching gas reaction.

Benefits of technology

It shortens the synthesis time, reduces energy consumption, improves etching efficiency and material dispersibility, simplifies the operation process, and increases the yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116692863B_ABST
    Figure CN116692863B_ABST
Patent Text Reader

Abstract

This invention belongs to the field of functional materials preparation, specifically relating to a method for in-situ preparation of two-dimensional MXene materials. The method mainly involves using glucose as a carbon source, first employing a gradient heating approach to induce a reaction in the raw materials, followed by in-situ etching. This method can achieve uniform and refined material structure, increase the contact area between the material and the etching gas, improve etching efficiency and effect, and is simple and safe to operate, shortening the synthesis time while avoiding the energy consumption caused by secondary heating, thus reducing costs.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of functional materials preparation, specifically relating to a method for in-situ preparation of two-dimensional MXene materials. Background Technology

[0002] Two-dimensional MXene materials possess rich surface functional groups, outstanding electromechanical properties, and magnetic properties, attracting widespread research in electrochemical energy storage, electromagnetic shielding, superconductors, and other fields. MXene materials are typically prepared by selective etching of precursors, with the most common method being liquid-phase etching using strong acids. However, this method suffers from low processing efficiency and complex waste disposal. Therefore, researchers are actively exploring new processes for MXene material preparation and promoting its mass production. For example, CN114620728A discloses a method and system for preparing two-dimensional materials using a gas-phase method. This method employs a gas-phase approach, introducing an etching gas, which avoids the complex post-processing required in MXene material preparation and simplifies the preparation process.

[0003] Furthermore, considering the precursors required for etching, they are currently mainly prepared by sintering elemental powders. This reaction process introduces a large number of metallic impurities, and the purification and salt recovery processes are complex, which also limits the scale of production and the application prospects of MXene materials. Therefore, considering the overall process of obtaining MXene materials, simplifying the preparation process and reducing energy consumption are urgent problems to be solved. Summary of the Invention

[0004] The purpose of this invention is to overcome the shortcomings of the prior art and provide a method for in-situ preparation of two-dimensional MXene materials, which can simplify the preparation process and reduce energy consumption.

[0005] The technical solution of the present invention is as follows: This invention provides a method for in-situ preparation of two-dimensional MXene materials, comprising the following steps: First, the transition metal element raw material, the group III or group IV element raw material, the carbon source and / or nitrogen source raw material are mixed evenly. Then, in an oxygen-free environment, the temperature is gradually increased to the first predetermined temperature for reaction. After the reaction is completed, the temperature is adjusted to the second predetermined temperature, and an etching gas is introduced to carry out the reaction, thereby obtaining a two-dimensional MXene material.

[0006] The gradient heating described in this invention is performed under the following conditions: heating at 7-10℃ / min to 300-350℃ and holding for 20-40 min, then heating at 4-6℃ / min to 800-1000℃ and holding for 1-2 h, and finally heating at 2-5℃ / min to the first predetermined temperature and holding for 0.5-5 h.

[0007] The transition metal element raw materials, Group III or Group IV element raw materials, carbon source and / or nitrogen source raw materials of the present invention have a molar ratio of 3:1 to 1.2:0.5 to 1.5. The transition metal element powder is scandium powder, titanium powder, zirconium powder, hafnium powder, vanadium powder, niobium powder, tantalum powder, chromium powder, molybdenum powder, and manganese powder. The Group III or Group IV element powder is aluminum powder, gallium powder, thallium powder, silicon powder, germanium powder, tin powder, and lead powder.

[0008] The carbon source described in this invention is glucose.

[0009] The gradient heating described in this invention is performed under the following conditions: heating at 7°C / min to 350°C and holding for 20 min, then heating at 4°C / min to 1000°C and holding for 1 h, and finally heating at 3°C / min to the first predetermined temperature and holding for 0.5 h.

[0010] The first predetermined temperature of the present invention is 1100-1600℃, the second predetermined temperature is 600-1000℃, the holding temperature is 20-50min, and the temperature adjustment has a cooling rate of 2-4℃ / min.

[0011] The oxygen-free environment described in this invention is a vacuum environment, a nitrogen environment, or an inert gas environment.

[0012] In this invention, an etching gas is introduced to carry out a reaction. The etching gas is mixed with a carrier gas to obtain a mixed gas. The mixed gas containing the etching gas is introduced to carry out the reaction. The gas flow rate is 70-100 sccm. The carrier gas accounts for 20%-50% of the total volume of the mixed gas. The etching gas described in this invention is HF gas or HCl gas, and the carrier gas is one or more of helium, argon, and nitrogen.

[0013] The first predetermined temperature of the present invention is 1600℃, and the second predetermined temperature is 600℃, with a holding time of 40 minutes.

[0014] The gas flow rate of the present invention is 80 sccm, and the carrier gas is 20% of the total volume of the mixed gas.

[0015] Beneficial effects Compared with conventional methods, this invention uses in-situ preparation of two-dimensional MXene materials, which shortens the synthesis time and avoids the energy consumption caused by secondary heating, thus reducing costs. This invention selects glucose as a carbon source, which provides a large number of nucleation substrates during the carbonization process, ensuring that no violent reaction occurs between raw materials, thereby making the material structure uniform and refined. This invention employs a gradient heating method to ensure that the carbon source glucose is fully carbonized, that the raw materials are in uniform contact and react completely, and that the dispersion, gas permeability and specific surface area of ​​the obtained material are improved, thereby increasing the contact area between the material and the etching gas, and improving the etching efficiency and etching effect. This invention employs a one-step method to prepare two-dimensional MXene materials from raw materials, avoiding secondary feeding at high temperatures, and the entire reaction takes place in a gaseous environment. The operation is simple and safe, and the yield is high. Attached Figure Description

[0016] Figure 1 XRD pattern of Ti3C2 MXene material; Figure 2 SEM images of Ti3C2 MXene material prepared by etching at 600℃; Figure 3 SEM images of Ti3C2 MXene material prepared by etching at 750℃; Figure 4 SEM images of Ti3C2 MXene material prepared by etching at 800℃; Figure 5 SEM image of Ti3C2 MXene material prepared by etching at 950℃. Detailed Implementation

[0017] The following examples are intended to illustrate the present invention, and not to further limit the invention.

[0018] This invention provides a method for in-situ preparation of two-dimensional MXene materials, comprising the following steps: First, the transition metal element raw material, the group III or group IV element raw material, the carbon source and / or nitrogen source raw material are mixed evenly. Then, in an oxygen-free environment, the temperature is gradually increased to the first predetermined temperature for reaction. After the reaction is completed, the temperature is adjusted to the second predetermined temperature, and an etching gas is introduced to carry out the reaction, thereby obtaining a two-dimensional MXene material.

[0019] The transition metal element raw materials, Group III or Group IV element raw materials, carbon source and / or nitrogen source raw materials of the present invention have a molar ratio of 3:1 to 1.2:0.5 to 1.5. The transition metal element powders are scandium powder, titanium powder, zirconium powder, hafnium powder, vanadium powder, niobium powder, tantalum powder, chromium powder, molybdenum powder, and manganese powder. The Group III or Group IV element powders are aluminum powder, gallium powder, thallium powder, silicon powder, germanium powder, tin powder, and lead powder. Preferably, the carbon source is glucose.

[0020] This invention uses glucose as a carbon source, which provides a large number of nucleation substrates during the carbonization process, ensuring that no violent reaction occurs between the raw materials, and making the material structure uniform and refined.

[0021] The oxygen-free environment described in this invention is a vacuum environment, a nitrogen environment, or an inert gas environment.

[0022] This invention raises the temperature in an oxygen-free environment to prevent oxidation of the raw materials during the reaction process, thereby ensuring that the raw materials react fully and improving utilization.

[0023] The gradient heating described in this invention is performed under the following conditions: heating at 7–10°C / min to 300–350°C, holding at this temperature for 20–40 min; then heating at 4–6°C / min to 800–1000°C, holding at this temperature for 1–2 h; and finally heating at 2–5°C / min to the first predetermined temperature, holding at this temperature for 0.5–5 h. Preferably, the gradient heating conditions are as follows: heating at 7℃ / min to 350℃ and holding for 20 min, then heating at 4℃ / min to 1000℃ and holding for 1 h, and finally heating at 3℃ / min to the first predetermined temperature and holding for 0.5 h.

[0024] This invention employs a gradient heating method to ensure that the carbon source glucose is fully carbonized, that the raw materials are in uniform contact and react completely, and that the dispersion, gas permeability and specific surface area of ​​the obtained material are improved, thereby increasing the contact area between the material and the etching gas, and improving the etching efficiency and etching effect.

[0025] The first predetermined temperature described in this invention is 1100–1600℃, the second predetermined temperature is 600–1000℃, the holding temperature is 20–50 min, and the temperature adjustment has a cooling rate of 2–4℃ / min. Preferably, the first predetermined temperature is 1300–1600°C, and the second predetermined temperature is 600–800°C. Preferably, the first predetermined temperature is 1600℃, the second predetermined temperature is 600℃, and the temperature is maintained for 40 minutes.

[0026] In this invention, the second predetermined temperature for the etching reaction is lower than the first predetermined temperature, thus avoiding energy consumption caused by secondary heating and reducing costs.

[0027] In this invention, an etching gas is introduced to carry out a reaction. The etching gas is mixed with a carrier gas to obtain a mixed gas. The mixed gas containing the etching gas is introduced to carry out the reaction. The gas flow rate is 70-100 sccm. The carrier gas accounts for 20%-50% of the total volume of the mixed gas. Preferably, the etching gas is HF or HCl, and the carrier gas is one or more of helium, argon, and nitrogen. Preferably, the gas flow rate is 80 sccm, and the carrier gas is 20% of the total volume of the mixed gas.

[0028] This invention etches materials by introducing an etching gas to obtain two-dimensional MXene materials. The carrier gas can dilute the content of the etching gas in the mixed gas, thereby controlling the rate of the gas phase etching reaction.

[0029] Example 1 This embodiment discloses a method for in-situ preparation of two-dimensional MXene material Ti3CN, the specific process of which is as follows: S1: Raw material pretreatment: Mix titanium powder, aluminum powder, glucose and nitrogen powder evenly in a molar ratio of 3:1.2:0.2:1.

[0030] S2: High-temperature reaction: The pretreated raw materials are placed in a high-temperature tube furnace under argon atmosphere and reacted by gradient heating to the first predetermined temperature. The gradient heating conditions are as follows: heating to 300℃ at 10℃ / min and holding for 30min, then heating to 800℃ at 5℃ / min and holding for 2h, and finally heating to the first predetermined temperature of 1500℃ at 2℃ / min and holding for 3h.

[0031] S3: Etching: After the reaction is completed at the first predetermined temperature, the temperature is lowered to the second predetermined temperature of 1000℃ at a cooling rate of 3℃ / min and held for 20min. The etching gas HCl is mixed with the carrier gas argon to obtain a mixed gas. The mixed gas containing the etching gas is introduced to carry out the reaction. The gas flow rate is 70sccm to obtain the two-dimensional MXene material Ti3CN. The carrier gas argon accounts for 50% of the total volume of the mixed gas.

[0032] Example 2 This embodiment discloses a method for in-situ preparation of two-dimensional MXene material Ti3C2, the specific process of which is as follows: S1: Raw material pretreatment: Mix titanium powder, aluminum powder and glucose in a molar ratio of 3:1.1:0.5 until homogeneous.

[0033] S2: High-temperature reaction: The pretreated raw materials are placed in a high-temperature tube furnace under nitrogen atmosphere and reacted by gradient heating to the first predetermined temperature. The gradient heating conditions are as follows: heating to 350℃ at 7℃ / min and holding for 20min, then heating to 1000℃ at 4℃ / min and holding for 1h, and finally heating to the first predetermined temperature of 1600℃ at 3℃ / min and holding for 0.5h.

[0034] S3: Etching: After the reaction is completed at the first predetermined temperature, the temperature is lowered to the second predetermined temperature of 600℃ at a cooling rate of 2℃ / min and held for 40min. The etching gas HCl is mixed with the carrier gas nitrogen to obtain a mixed gas. The mixed gas containing the etching gas is introduced to carry out the reaction. The gas flow rate is 80sccm to obtain the two-dimensional MXene material Ti3C2. The carrier gas nitrogen accounts for 20% of the total volume of the mixed gas.

[0035] X-ray diffraction (XRD) analysis was performed on the final product obtained in Example 2, and the results are as follows: Figure 1 As shown, the product is Ti3C2. Scanning electron microscopy (SEM) was performed on the product, and the results are as follows. Figure 2 As shown, the product has an accordion-like morphology and a distinct stacked layered structure.

[0036] Example 3 This embodiment discloses a method for in-situ preparation of two-dimensional MXene material Ti2N, the specific process of which is as follows: S1: Raw material pretreatment: Mix titanium powder, aluminum powder and nitrogen powder evenly in a molar ratio of 3:1:1.5.

[0037] S2: High-temperature reaction: The pretreated raw materials are placed in a high-temperature tube furnace and reacted under vacuum by gradient heating to the first predetermined temperature. The gradient heating conditions are as follows: heating to 320℃ at 8℃ / min and holding for 40min, then heating to 900℃ at 6℃ / min and holding for 1.5h, and finally heating to the first predetermined temperature of 1100℃ at 5℃ / min and holding for 5h.

[0038] S3: Etching: After the reaction is completed at the first predetermined temperature, the temperature is lowered to the second predetermined temperature of 800℃ at a cooling rate of 4℃ / min and held for 50min. The etching gas HF is mixed with the carrier gas helium to obtain a mixed gas. The mixed gas containing the etching gas is introduced to carry out the reaction. The gas flow rate is 100sccm to obtain the two-dimensional MXene material Ti3C2. Among them, the carrier gas helium accounts for 30% of the total volume of the mixed gas.

[0039] Example 4 This embodiment discloses a method for in-situ preparation of two-dimensional MXene material Ti3C2, the specific process of which is as follows: S1: Raw material pretreatment: Mix titanium powder, aluminum powder and glucose in a molar ratio of 3:1.1:0.5 until homogeneous.

[0040] S2: High-temperature reaction: The pretreated raw materials are placed in a high-temperature tube furnace under argon atmosphere and reacted by gradient heating to the first predetermined temperature. The gradient heating conditions are as follows: heating to 300℃ at 10℃ / min and holding for 30min, then heating to 800℃ at 5℃ / min and holding for 2h, and finally heating to the first predetermined temperature of 1300℃ at 2℃ / min and holding for 4h.

[0041] S3: Etching: After the reaction is completed at the first predetermined temperature, the temperature is lowered to the second predetermined temperature of 700℃ at a cooling rate of 3℃ / min and held for 20min. The etching gas HCl is mixed with the carrier gas argon to obtain a mixed gas. The mixed gas containing the etching gas is introduced to carry out the reaction. The gas flow rate is 70sccm to obtain the two-dimensional MXene material Ti3C2. The carrier gas argon accounts for 50% of the total volume of the mixed gas.

[0042] Example 5 Example 5 provides a method for in-situ preparation of two-dimensional MXene materials that is basically the same as that in Example 2, except that the second predetermined temperature in the S3 etching step is 750°C.

[0043] The product was subjected to SEM testing, and the results are as follows: Figure 3 As shown, the product has an accordion-like morphology and a distinct stacked layered structure.

[0044] Example 6 Example 6 provides a method for in-situ preparation of two-dimensional MXene materials that is basically the same as that in Example 2, except that the second predetermined temperature in the S3 etching step is 800°C.

[0045] The product was subjected to SEM testing, and the results are as follows: Figure 4 As shown, the product has an accordion-like morphology and a distinct stacked layered structure.

[0046] Example 7 Example 7 provides a method for in-situ preparation of two-dimensional MXene materials that is basically the same as that in Example 2, except that the second predetermined temperature in the S3 etching step is 950°C.

[0047] The product was subjected to SEM testing, and the results are as follows: Figure 5 As shown, the product has an accordion-like morphology and a distinct stacked layered structure.

[0048] Comparative Example 1 The method for in-situ preparation of two-dimensional MXene materials provided in Comparative Example 1 is basically the same as that in Example 2, except that the high-temperature reaction step S2 does not involve gradient heating, but instead directly heats to the first predetermined temperature at a rate of 2℃ / min, while the other conditions are the same.

[0049] Comparative Example 2 Comparative Example 2 provides a method for in-situ preparation of two-dimensional MXene materials that is basically the same as that in Example 2, except that the carbon source in the raw material pretreatment step S1 is carbon powder, while the other conditions are the same.

[0050] The specific surface area and pore volume of the material after reaction at the first predetermined temperature were tested using a specific surface area measuring instrument. The test results are as follows: .

Claims

1. A method of in-situ preparation of two-dimensional MXene material, characterized in that, Includes the following steps: First, titanium powder, aluminum powder, carbon source and / or nitrogen source raw materials are mixed evenly. Then, in an oxygen-free environment, the temperature is gradually increased to the first predetermined temperature for reaction. After the reaction is completed, the temperature is adjusted to the second predetermined temperature, and etching gas is introduced to carry out the reaction to obtain two-dimensional MXene material. The carbon source is glucose; The gradient heating conditions are as follows: heating at 7-10℃ / min to 300-350℃, holding at that temperature for 20-40 min, then heating at 4-6℃ / min to 800-1000℃, holding at that temperature for 1-2 h, and finally heating at 2-5℃ / min to the first predetermined temperature, holding at that temperature for 0.5-5 h. The first predetermined temperature is 1100-1600℃, the second predetermined temperature is 600-1000℃, the holding temperature is 20-50 min, and the temperature adjustment has a cooling rate of 2-4℃ / min.

2. The method of claim 1, wherein, The molar ratio of the titanium powder, aluminum powder, carbon source and / or nitrogen source raw materials is 3:1 to 1.2:0.5 to 1.

5.

3. The method of claim 1, wherein the method is characterized by, The gradient heating conditions are as follows: heat up to 350℃ at 7℃ / min and hold for 20min, then heat up to 1000℃ at 4℃ / min and hold for 2h, and finally heat up to the first predetermined temperature at 3℃ / min and hold for 0.5h.

4. The method of claim 1, wherein the method is characterized by, The oxygen-free environment refers to a vacuum environment, a nitrogen environment, or an inert gas environment.

5. The method of claim 1, wherein the method is characterized by, The etching gas is introduced to carry out the reaction. The etching gas is mixed with the carrier gas to obtain a mixed gas. The mixed gas containing the etching gas is introduced to carry out the reaction. The gas flow rate is 70-100 sccm. The carrier gas accounts for 20%-50% of the total volume of the mixed gas.

6. The method of claim 5, wherein the method is characterized by, The etching gas is HF or HCl, and the carrier gas is one or more of helium, argon, and nitrogen.

7. The method of claim 1, wherein the method is characterized by, The first predetermined temperature is 1600℃, the second predetermined temperature is 600℃, and the temperature is maintained for 40 minutes.

8. The method of claim 5, wherein the method is characterized by, The gas flow rate is 80 sccm, and the carrier gas is 20% of the total volume of the mixed gas.

Citation Information

Patent Citations

  • Ti3AlC2 powder and preparation method thereof

    CN110817875A

  • Method for preparing MXene material

    CN112794328A