A short-period low-energy consumption post-forging heat treatment method for backup rolls
By using a segmented cooling and high-temperature heat treatment method for support rolls after forging, spheroidizing annealing and high-temperature tempering are eliminated, solving the problems of long production cycle and high cost of support rolls, and realizing the manufacturing of support rolls with high efficiency and low energy consumption.
Patent Information
- Application Number
- CN202210192582.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-02-28
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2042-02-28
AI Technical Summary
The existing heat treatment process after forging of support rolls is time-consuming and costly, resulting in low production efficiency.
By employing segmented cooling and high-temperature holding methods, the spheroidizing annealing and high-temperature tempering processes are eliminated. By controlling the cooling rate and recrystallization conditions, a microstructure dominated by granular pearlite is obtained, thus shortening the heat treatment cycle.
This significantly shortened the production cycle of heat treatment after forging of support rolls, reduced production costs, enabled efficient manufacturing of support rolls, and promoted the green manufacturing process.
Smart Images

Figure CN116694907B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of heat treatment technology for support rolls, and in particular to a short-cycle, low-energy-consumption heat treatment method for support rolls after forging. Background Technology
[0002] Support rolls are important tools and consumable parts of steel rolling equipment, with a large annual consumption. The domestic demand for support rolls for strip mills is approximately 1,600 units per year. Due to the special performance requirements of support rolls, the working layer of the roll body is required to have high wear resistance and fatigue resistance, while the core is required to have good strength and toughness.
[0003] Generally, support rollers require three heat treatments: post-forging heat treatment, preliminary heat treatment (quenching and tempering), and differential temperature heat treatment (final heat treatment). The performance of the roller neck and core can be ensured through preliminary heat treatment (quenching and tempering), while the surface microstructure (working layer) of the roller body is completed by the final heat treatment process. Post-forging heat treatment mainly originates from the previous traditional process, which uses "normalizing + spheroidizing annealing + high-temperature tempering," with a cycle of 15-25 days, long equipment occupation time, and low production efficiency.
[0004] The existing traditional post-forging heat treatment process for continuous rolling mill support rolls has the problems of long processing time and high cost. Summary of the Invention
[0005] Based on the above analysis, the present invention aims to provide a short-cycle, low-energy-consumption heat treatment method for support rolls after forging, in order to solve the technical problems of long heat treatment process cycle and high cost in the production of existing support rolls.
[0006] The objective of this invention is mainly achieved through the following technical solutions:
[0007] This invention provides a short-cycle, low-energy-consumption heat treatment method for support rolls after forging, comprising the following steps:
[0008] Step 1: Prepare and heat the support rollers;
[0009] Step 2: Cool the support rollers processed in Step 1 by sealing the furnace;
[0010] Step 3: Maintain the temperature at 300-400℃;
[0011] Step 4: After heat preservation, raise the temperature of the support roller to 650-670℃;
[0012] Step 5: Maintain the temperature at 650-670℃;
[0013] Step 6: Increase the temperature to 880-950℃ at a rate of less than or equal to 50℃ / h, and the process takes 7-10 hours.
[0014] Step 7: Keep warm at 880-950℃ for 20-45 hours;
[0015] Step 8: Cool down to 640-740℃ at a rate of less than or equal to 10℃ / h, with a process time of 20-35h.
[0016] Furthermore, it also includes step 9;
[0017] Step 9: Cool down to 400℃ at a rate of less than or equal to 20℃ / h, with a process time of 15-20h.
[0018] Furthermore, it also includes step 10;
[0019] Step 10: Cool down to 150℃ at a rate of less than or equal to 10℃ / h, with a process time of 25-30h.
[0020] Furthermore, in step 9, the temperature is reduced to 400°C at a rate of less than or equal to 18°C / h, and the process takes 17-20 hours.
[0021] Furthermore, in step 1, the support roller is subjected to material preparation and heat preservation at 600-650℃ for a total duration of 20-40 hours.
[0022] Furthermore, in step 2, the support rollers processed in step 1 are cooled in a sealed furnace to 300-400°C for 20-30 hours.
[0023] Furthermore, in step 3, the heat preservation time is 10-30 hours.
[0024] Furthermore, in step 4, after heat preservation, the support roller is heated to 650-670℃ at a rate of less than or equal to 30℃ / h, and the process takes 7-10h.
[0025] Furthermore, in step 5, the heat preservation time is 10-30 hours.
[0026] Furthermore, in step 1, the [H] content of the support roller is controlled to be below 1 PPM.
[0027] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects:
[0028] (1) This invention greatly shortens the production cycle of heat treatment after forging of support rolls, and solves the contradiction between the large production volume of support rolls, the long heat treatment process cycle and the shortage of equipment; while ensuring the quality of forgings, it achieves the goal of shortening the production cycle and reducing production costs.
[0029] (2) The total time for the post-forging heat treatment method of the support roll of the present invention is 160-275 hours, i.e., 7-12 days; the total time for the traditional process is 340-565 hours, i.e., 15-25 days. The present invention reduces the time by more than 50% compared with the traditional process, and the resulting labor, equipment losses, and time effects are immeasurable, achieving short-process manufacturing with guaranteed quality, increased efficiency, and energy saving. The post-forging heat treatment method of the support roll provided by the present invention is equivalent to an innovation in the heat treatment system of support rolls, which strongly promotes the green manufacturing process of large forgings of support rolls.
[0030] In this invention, the above-described technical solutions can be combined with each other to achieve more preferred combinations. Other features and advantages of this invention will be set forth in the following description, and some advantages may become apparent from the description or be learned by practicing the invention. The objects and other advantages of this invention can be realized and obtained through the embodiments described and the accompanying drawings, which are particularly pointed out. Attached Figure Description
[0031] The accompanying drawings are for illustrative purposes only and are not intended to limit the invention. Throughout the drawings, the same reference numerals denote the same parts.
[0032] Figure 1 The traditional post-forging heat treatment process curves for continuous rolling mill support rolls (Cr3\Cr4\Cr5);
[0033] Figure 2 The heat treatment curves of the continuous rolling mill support rolls (Cr3\Cr4\Cr5) after forging are shown in the present invention.
[0034] Figure 3 Microstructure of the surface of the support roll (Cr3) of the continuous rolling mill after high-temperature annealing;
[0035] Figure 4 Microstructure of the body of the support roll (Cr3) of the continuous rolling mill after high-temperature annealing.
[0036] Figure 5 Microstructure of the surface of the support roll (Cr5) of the continuous rolling mill after high-temperature annealing;
[0037] Figure 6 Microstructure of the body and core of the continuous rolling mill support roll (Cr5) after high-temperature annealing;
[0038] Figure 7 The flaw detection report for the continuous rolling mill support roll (Cr3) after high-temperature annealing;
[0039] Figure 8 This is a flaw detection report for the support rolls (Cr5) of the continuous rolling mill after high-temperature annealing. Detailed Implementation
[0040] The preferred embodiments of the present invention will now be described in detail with reference to the accompanying drawings, which constitute a part of the present invention and are used together with the embodiments of the present invention to illustrate the principles of the present invention, but are not intended to limit the scope of the present invention.
[0041] The post-forging heat treatment of the support roll is carried out immediately after the forging process is completed. Its main purposes or functions are: first, to eliminate forging stress, reduce the surface hardness of the forging, and improve its machinability; second, to adjust and improve the overheated or coarse structure formed during the forging process of large forgings, refine the austenite grains of the support roll, eliminate grass-like waves, and improve the ultrasonic flaw detection performance of the support roll forging; and third, to prevent and eliminate white spots.
[0042] With the improvement of my country's smelting level, the [H] content of the support rolls can be controlled below 1 PPM (less than the hydrogen content at the white point and hydrogen embrittlement limits). Therefore, the issue of [H] content of the support rolls does not need to be considered when formulating post-forging heat treatment processes. Thus, under the premise of ensuring workpiece quality and safety, and to achieve the goals of "eliminating forging stress, refining the overall structure, and facilitating machining," the post-forging heat treatment process is adjusted. The performance of the roll neck is ensured through pre-heat treatment (quenching and tempering), while the microstructure of the roll body surface (working layer) is completed by the final heat treatment process.
[0043] The theoretical basis of this invention is that granular pearlite has low hardness, and one way to obtain granular pearlite is through "slowly obtaining supercooled austenite under specific conditions". The steel used for the support roll is a high-alloy tool steel, and a large amount of alloy carbides exist when the high temperature holding temperature is less than or equal to 950°C, resulting in a low carbon content in the austenite. Therefore, network carbides will not form during the slow cooling process. This invention promotes the recrystallization process by appropriately extending the high temperature holding time, and appropriately reduces the high temperature holding temperature on the basis of achieving the recrystallization effect, as shown in step 7 of this invention. By controlling the cooling rate in steps 8 to 10, the support roll forging can obtain a microstructure with low hardness and mainly composed of granular pearlite inside and outside.
[0044] This invention, starting from the microstructure transformation mechanism during the post-forging heat treatment of support roll materials, and disregarding the dehydrogenation factor, formulates a post-forging heat treatment method: It eliminates the spheroidizing annealing and high-temperature tempering processes in the traditional support roll heat treatment process, i.e., steps 10 to 21 in curve 1 are eliminated; the time of step 1 is extended to ensure the elimination of forging stress; and the austenitizing conditions and cooling rate are modified to meet the objectives of "eliminating forging stress, refining the overall microstructure, and facilitating machining." The post-forging heat treatment curve of this invention is shown in [reference needed]. Figure 2 As shown.
[0045] It is important to note that in existing technologies, the main functions of the spheroidizing annealing process are, on the one hand, to reduce the surface hardness of the support roller, making it easier to machine; and on the other hand, to obtain a high-toughness spheroidized structure (granular pearlite) in the core of the support roller. High-temperature tempering mainly considers hydrogen diffusion to ensure that the [H] content is controlled at a low level.
[0046] By controlling the cooling rate and austenitizing conditions for recrystallization, this invention allows the workpiece to acquire a predominantly granular pearlite structure under slow cooling conditions. This ensures high toughness in the core while maintaining low surface hardness, facilitating machining and replacing the spheroidizing annealing step. With improved smelting techniques, the [H] content can be controlled at lower levels. The [H] content in the forgings used in this invention is controlled below 1 PPM, eliminating the need to consider hydrogen diffusion in the 650℃ tempering stage after forging heat treatment, thus eliminating the high-temperature tempering stage. In other words, existing processes use a "normalizing + spheroidizing annealing + high-temperature tempering" technical route for post-forging heat treatment of support rolls, while this invention only uses a high-temperature annealing process, shortening the process flow while ensuring the quality of the support rolls.
[0047] This invention provides a short-cycle, low-energy-consumption heat treatment method for support rolls after forging, comprising the following steps:
[0048] Step 1: Waiting and holding the material at 600-650℃ for a total of 20-40 hours. The purpose is to eliminate the forging stress of the support rollers and to transform the forging from austenite to ferrite-carbide structure.
[0049] Step 2: After heat preservation, seal the support roller in the furnace and cool it to 300-400℃. The process takes 20-30 hours.
[0050] Step 3: Hold at 300-400℃ for 10-30 hours. This stage allows the core of the forging to fully transform from austenite to ferrite-carbide structure, which is beneficial for adjusting and refining the grain structure of the steel through subsequent phase transformation recrystallization.
[0051] Step 4: Heat to 650-670℃ at a rate of less than or equal to 30℃ / h, with a process time of 7-10h; This stage adopts a rate-limited heating method to minimize the internal and external temperature difference and instantaneous internal stress in the support roll forging.
[0052] Step 5: Keep warm at 650-670℃ for 10-30 hours;
[0053] Step 6: Increase the temperature to 880-950℃ at a rate of less than or equal to 50℃ / h, with a process time of 7-10 hours;
[0054] Step 7: Hold at 880-950℃ for 20-45 hours, then heat to the austenitizing temperature for recrystallization to refine the austenite grains, improve the microstructure, and enhance the properties.
[0055] Step 8: Cool down to 640-740℃ at a rate of less than or equal to 10℃ / h, with a process time of 20-35h; in this stage, the support roll forging is slowly cooled to between the material transformation critical point Ar1 and Ar3, and close to the Ar1 point, so that granular pearlite is obtained from the surface of the support roll to the core area.
[0056] Step 9: Cool down to 400℃ at a rate of less than or equal to 20℃ / h, with a process time of 15-20h. The purpose of controlling the process conditions is to slowly reduce the temperature of the core of the support roller, so that the austenite in the core of the support roller gradually transforms into granular pearlite, thereby obtaining a microstructure dominated by granular pearlite.
[0057] Step 10: Cool down to 150℃ at a rate of 10℃ / h or less, taking 25-30 hours. Controlling these process conditions ensures that the core of the support roller undergoes a phase transformation, completely converting the austenite in the core into a microstructure dominated by granular pearlite. Additionally, it reduces the temperature difference between the core and the surface of the support roller, thereby reducing the thermal stress caused by the temperature difference.
[0058] Compared with existing technologies, this invention reduces the number of temperature changes experienced by the rolls by eliminating the supercooling and intermediate-temperature holding processes after normalizing. This ensures a core stress reduction while maintaining a microstructure free of austenite residue. Furthermore, it guarantees significant grain refinement after recrystallization, both on the roll surface and in the roll core. Benefits: Reduced cycle time while maintaining quality.
[0059] It should be noted that the diameter of the support roller of the present invention is 1000mm-1700mm.
[0060] Compared with the prior art, the present invention achieves the goal of the core of the support roller being granular pearlite (granular carbide) with low surface hardness and easy machining, that is, to achieve the process condition setting made by "eliminating spheroidizing annealing and high temperature tempering".
[0061] The total time for the post-forging heat treatment method of the support rolls of this invention is 160-275 hours, or 7-12 days; the total time for the traditional process is 340-565 hours, or 15-25 days. This invention reduces the time by more than 50% compared to the traditional process, and the resulting reduction in labor, equipment losses, and time efficiency is immeasurable, achieving short-process manufacturing that ensures quality, improves efficiency, and saves energy. The post-forging heat treatment method for support rolls provided by this invention represents a revolution in the heat treatment system for support rolls, powerfully promoting the green manufacturing process of large support roll forgings.
[0062] It should be noted that the method of the present invention is applicable to continuous rolling mill support rolls with a roll body forging diameter <1700mm and material of Cr3, Cr4 or Cr5. After being treated by the above-mentioned post-forging heat treatment method, the quality of the support roll is stable.
[0063] Table 1. Components and contents of Cr3, Cr4, and Cr5 in the support rolls of continuous rolling mills.
[0064]
[0065] Example 1
[0066] In this embodiment, the above-mentioned heat treatment method for support roll forging was used to conduct production tests on support roll forgings made of Cr3 with a roll body diameter of 1000mm. The internal and external microstructure and hardness of the workpiece were dissected and tested to verify the feasibility of the process.
[0067] The support roll forging has a roll body diameter of 1000mm and is manufactured using a high-temperature annealing process. The specific process is as follows:
[0068] Step 1: Wait for the material at 640℃ and keep it warm for 20 hours;
[0069] Step 2: Seal the furnace and cool it to 310℃. The process takes 25 hours.
[0070] Step 3: Keep warm at 310℃ for 10 hours;
[0071] Step 4: Increase the temperature to 660℃ at a rate of 30℃ / h, with a process time of 11.7h;
[0072] Step 5: Keep warm at 660℃ for 10 hours;
[0073] Step 6: Increase the temperature to 910℃ at a rate of 50℃ / h, with a process time of 5 hours;
[0074] Step 7: Hold at 910℃ for 22 hours to refine the austenite grains inside and outside the workpiece and achieve recrystallization.
[0075] Step 8: Cool down to 700℃ at a rate of 9℃ / h. The process takes 23.3h. The process conditions at this stage should be controlled to achieve the austenitization conditions that facilitate the formation of particulate pearlite, i.e., a slow cooling rate.
[0076] Step 9: Cool down to 400℃ at a rate of 20℃ / h, with a process time of 15h; controlling these process conditions enables the transformation from austenite to pearlite to be completed in the phase transformation zone of the support roller.
[0077] Step 10: Cool down to 150℃ at a rate of 10℃ / h, with a process time of 25h. The purpose of controlling these process conditions is to ensure that the core of the support roller completes the phase transformation, and that the austenite in the core is completely transformed into a microstructure dominated by granular pearlite. In addition, cooling down to 150℃ at a slow rate reduces the thermal stress caused by the temperature difference between the inside and outside, and prevents the support roller from cracking.
[0078] The test forging of the support roll with Cr3 and a roll body diameter of 1000mm takes about 15 days to complete using the traditional post-forging heat treatment process; however, the optimized process reduces the cycle to 7 days (167h), greatly shortening the production cycle.
[0079] After the above-mentioned post-forging heat treatment, the support roll forging was subjected to overall flaw detection and dissection analysis. The test results of the internal and external microstructure of the roll body, the surface hardness of the roll, and flaw detection are as follows:
[0080] I. In terms of microstructure, Figure 3 The microstructure of the roller body surface. Figure 4 The microstructure of the roller body consists entirely of granular pearlite and a small amount of lamellar pearlite. Traditional heat treatment, spheroidizing annealing, corresponds to a microstructure of granular spheroidized pearlite. Therefore, it can be concluded that the heat treatment method of this invention can obtain the same microstructure as traditional heat treatment methods, thereby ensuring the performance and quality of the support roller.
[0081] II. Regarding mechanical properties, the mechanical properties of the support roll forgings are shown in Table 2.
[0082] Table 2 Mechanical properties of Cr5 support rollers
[0083]
[0084] The surface hardness of the roll workpiece fully meets the requirements of rough machining, and the core impact energy of the support roll forging is ≥60J, ensuring high safety performance.
[0085] III. In terms of flaw detection
[0086] In this embodiment, the processed support rollers were subjected to flaw detection. The results showed that no recordable defects were found, and the bottom wave was clearly visible. The flaw detection was qualified, and the flaw detection report can be found here. Figure 8 .
[0087] The test results show that the heat treatment of the support roll after forging adopts a segmented cooling method, which can achieve the goal of "eliminating forging stress, refining the overall structure, and meeting the requirements of machining". All performance indicators fully meet the requirements and the flaw detection is qualified.
[0088] Example 2
[0089] This embodiment uses the above-mentioned heat treatment method after forging of support rolls to conduct production tests on support roll forgings made of Cr5 with a roll body diameter of 1680mm. The internal and external microstructure and hardness of the workpiece are dissected and tested to verify the feasibility of the process.
[0090] Support roll forging roll body diameter The process employs high-temperature annealing, and the specific steps are as follows:
[0091] Step 1: Prepare and heat the material at 650℃ for 38 hours;
[0092] Step 2: Seal the furnace and cool it to 350℃. The process takes 25 hours.
[0093] Step 3: Keep warm at 350℃ for 30 hours;
[0094] Step 4: Increase the temperature to 660℃ at a rate of 30℃ / h, with a process time of 10.3h;
[0095] Step 5: Keep warm at 660℃ for 30 hours;
[0096] Step 6: Increase the temperature to 930℃ at a rate of 50℃ / h, with a process time of 5.4h;
[0097] Step 7: Hold at 930℃ for 45 hours to refine the austenite grains inside and outside the workpiece and achieve recrystallization.
[0098] Step 8: Cool down to 735℃ at a rate of 7℃ / h. The process takes 27.8h. The process conditions at this stage should be controlled to achieve austenitization conditions that facilitate the formation of particulate pearlite, i.e., a slow cooling rate.
[0099] Step 9: Cool down to 400℃ at a rate of 16℃ / h, with a process time of 20.9h; controlling these process conditions enables the transformation from austenite to pearlite to be completed in the phase transformation zone of the support roller.
[0100] Step 10: Cool down to 150℃ at a rate of 8℃ / h, with a process time of 31.3h. The purpose of controlling these process conditions is to ensure that the core of the support roller completes the phase transformation, and that the austenite in the core is completely transformed into a microstructure dominated by granular pearlite. In addition, cooling down to 150℃ at a slow rate reduces the thermal stress caused by the temperature difference between the inside and outside, and prevents the support roller from cracking.
[0101] The test forging of the support roll with Cr5 coating and a roll body diameter of 1680mm takes approximately 23 days to complete using the traditional post-forging heat treatment process; however, the optimized process reduces the cycle to 11 days, significantly shortening the production time.
[0102] After the above-mentioned post-forging heat treatment, the support roll forging was subjected to overall flaw detection and dissection analysis. The test results of the internal and external microstructure of the roll body, the surface hardness of the roll, and flaw detection are as follows:
[0103] I. In terms of microstructure, Figure 5 The microstructure of the roller body surface. Figure 6 The microstructure of the roller body consists entirely of granular pearlite and a small amount of lamellar pearlite. Traditional heat treatment, spheroidizing annealing, corresponds to a microstructure of granular spheroidized pearlite. Therefore, it can be concluded that the heat treatment method of this invention can obtain the same microstructure as traditional heat treatment methods, thereby ensuring the performance and quality of the support roller.
[0104] II. Regarding mechanical properties, the mechanical properties of the support roll forgings are shown in Table 3.
[0105] Table 3 Mechanical properties of Cr5 support rollers
[0106]
[0107] The surface hardness of the roll workpiece fully meets the requirements of rough machining, and the core impact energy of the support roll forging is ≥70J, with high safety performance.
[0108] III. In terms of flaw detection
[0109] In this embodiment, the processed support rollers were subjected to flaw detection. The results showed that no recordable defects were found, and the bottom wave was clearly visible. The flaw detection was qualified, and the flaw detection report can be found here. Figure 7 .
[0110] The test results show that the heat treatment of the support roll after forging adopts a segmented cooling method, which can achieve the goal of "eliminating forging stress, refining the overall structure, and meeting the requirements of machining". All performance indicators fully meet the requirements and the flaw detection is qualified.
[0111] Example 3
[0112] This embodiment uses the above-mentioned heat treatment method after forging of support rolls to conduct production tests on support roll forgings made of Cr4 with a roll body diameter of 1600mm. The internal and external microstructure and hardness of the workpiece are dissected and tested to verify the feasibility of the process.
[0113] Support roll forging roll body diameter The process employs high-temperature annealing, and the specific steps are as follows:
[0114] Step 1: Prepare and heat the material at 650℃ for 38 hours;
[0115] Step 2: Seal the furnace and cool it to 395℃. The process takes 25 hours.
[0116] Step 3: Keep warm at 395℃ for 28 hours;
[0117] Step 4: Increase the temperature to 665℃ at a rate of 30℃ / h, with a process time of 9 hours;
[0118] Step 5: Keep warm at 660℃ for 28 hours;
[0119] Step 6: Increase the temperature to 920℃ at a rate of 50℃ / h, with a process time of 5.2h;
[0120] Step 7: Hold at 920℃ for 43 hours to refine the austenite grains inside and outside the workpiece and achieve recrystallization.
[0121] Step 8: Cool down to 700℃ at a rate of 8℃ / h. The process takes 27.5h. The process conditions at this stage should be controlled to achieve austenitization conditions that facilitate the formation of particulate pearlite, i.e., a slow cooling rate.
[0122] Step 9: Cool down to 400℃ at a rate of 17℃ / h, with a process time of 17.6h; controlling these process conditions enables the transformation from austenite to pearlite to be completed in the phase transformation zone of the support roller.
[0123] Step 10: Cool down to 150℃ at a rate of 8℃ / h, with a process time of 31.3h. The purpose of controlling these process conditions is to ensure that the core of the support roller completes the phase transformation, and that the austenite in the core is completely transformed into a microstructure dominated by granular pearlite. In addition, cooling down to 150℃ at a slow rate reduces the thermal stress caused by the temperature difference between the inside and outside, and prevents the support roller from cracking.
[0124] The test forging of the support roll with Cr4 and a roll body diameter of 1600mm takes about 23 days to complete using the traditional post-forging heat treatment process; however, the optimized process reduces the cycle to 10.52 days, significantly shortening the production cycle.
[0125] After the above-mentioned post-forging heat treatment, the support roll forging was dissected and analyzed. The test results of the internal and external microstructure of the roll body, the surface hardness of the roll, and the overall flaw detection are as follows:
[0126] I. Regarding the microstructure, the Cr4 support roller prepared in this embodiment exhibits granular pearlite and a small amount of lamellar pearlite on both the roller body surface and the roller body interior. Traditional heat treatment involves spheroidizing annealing, which corresponds to a granular spheroidized pearlite microstructure. Therefore, it can be concluded that the heat treatment method of this invention can obtain the same microstructure as traditional heat treatment methods, thereby ensuring the performance and quality of the support roller.
[0127] II. Regarding mechanical properties, the mechanical properties of the support roll forgings are shown in Table 4.
[0128] Table 4 Mechanical properties of Cr4 support rollers
[0129]
[0130] The surface hardness of the roll workpiece fully meets the requirements of rough machining, and the core impact energy of the support roll forging is ≥60J, ensuring high safety performance.
[0131] III. In terms of flaw detection
[0132] In this embodiment, the processed support roller is subjected to flaw detection. The flaw detection results are as follows: no recordable defects were found, and the bottom wave is clearly visible, indicating that the flaw detection is qualified.
[0133] The test results show that the heat treatment of the support roll after forging adopts a segmented cooling method, which can achieve the goal of "eliminating forging stress, refining the overall structure, and meeting the requirements of machining". All performance indicators fully meet the requirements and the flaw detection is qualified.
[0134] Compare with Example 1
[0135] The traditional post-forging heat treatment process curves for continuous rolling mill support rolls of different specifications and sizes (1000mm ≤ roll body diameter D < 1700mm) and different materials (including Cr5, Cr4, and Cr3 forged steel) are shown below. Figure 1 Traditional post-forging heat treatment processes specifically include:
[0136] Step 1: Wait for the material at 600-650℃ and keep it at that temperature for 10-30 hours to eliminate forging stress.
[0137] Step 2: Seal the furnace and cool it to 300-400℃. The process takes about 20-30 hours.
[0138] Step 3: Hold at 300-400℃ for 10-30 hours; this stage allows the core of the forging to fully transform from austenite to ferrite-carbide structure, which is beneficial for adjusting and refining the grain structure of the steel through subsequent phase transformation recrystallization.
[0139] Step 4: Heat to 650-670℃ at a rate of less than or equal to 30℃ / h, with a process time of 10h; this stage is a rate-limited heating to try to reduce the internal and external temperature difference and instantaneous internal stress in large support roll forgings.
[0140] Step 5: Hold at 650-670℃ for 10-30 hours; minimize the temperature difference between the inside and outside of the forging during the heating transformation and the non-simultaneity of the transformation, and further reduce the stress and deformation in the workpiece.
[0141] Step 6: Increase the temperature to 900-950℃ at a rate of less than or equal to 50℃ / h, with a process time of 10 hours.
[0142] Step 7: Hold at 900-950℃ for 15-40 hours, then heat to the austenitizing temperature for recrystallization to refine the austenite grains, improve the microstructure, and enhance the properties.
[0143] Step 8: Remove the roller from the trolley and air cool it. When the roller body is cooled to 400-500℃, put it into the furnace. The process takes 10-20 hours.
[0144] Step 9: Cool down to 300-400℃ at a rate of less than or equal to 10℃ / h, with a process time of 10 hours.
[0145] Step 10: Hold at 300-400℃ for 10-30 hours; this stage allows the austenite in the core of the forging to fully transform into a ferrite-carbide structure.
[0146] Step 11: Increase the temperature to 650-670℃ at a rate of less than or equal to 30℃ / h, with a process time of 12 hours.
[0147] Step 12: Hold at 650-670℃ for 10-20 hours; minimize the internal and external temperature difference and non-simultaneous transformation of the forging during heating transformation, and further reduce stress and deformation in the workpiece.
[0148] Step 13: Increase the temperature to 760-810℃ at a rate of less than or equal to 50℃ / h, with a process time of 3 hours.
[0149] Step 14: Hold at 760-810℃ for 30-60 hours; this stage is spheroidizing annealing. Hold at a temperature above Ac1 for a relatively long time to dissolve some of the (Fe,Cr)3C type carbides, and the remaining undissolved carbides aggregate and spheroidize. After cooling, the fine spheroids are evenly distributed to obtain a granular pearlite (spheroidized body) structure with good plasticity and toughness.
[0150] Step 15: Cool the furnace to 400℃, the process takes 20 hours.
[0151] Step 16: Cool down to 300-400℃ at a rate of less than or equal to 10℃ / h, with a process time of 10h.
[0152] Step 17: Hold at 300-400℃ for 10-30 hours; this stage allows the austenite in the core of the forging to fully transform into a ferrite-carbide structure.
[0153] Step 18: Increase the temperature to 640-660℃ at a rate of 30℃ / h or less, taking 10 hours.
[0154] Step 19: Hold at 640-660℃ for 100-150 hours; this also helps to expand hydrogen, effectively prevent white spots and hydrogen embrittlement, further reduce the stress on the forging, and facilitate machining.
[0155] Step 20: Cool the forging to 400℃ at a rate of less than or equal to 20℃ / h, with a process time of 15h; minimize residual stress in the forging during the cooling process.
[0156] Step 21: Cool down to 150℃ at a rate of less than or equal to 10℃ / h, with a process time of 25h; below 400℃, since the steel has entered a range of greater cold hardening and brittleness, a slower cooling rate is adopted to avoid cracking and reduce instantaneous stress.
[0157] The total time for the above process is 340-565 hours, or 15-25 days.
[0158] The disadvantages of the above process are: long cycle time and high cost.
[0159] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in the present invention should be included within the scope of protection of the present invention.
Claims
1. A short-cycle, low-energy-consumption heat treatment method for support rolls after forging, characterized in that, Includes the following steps: Step 1: Prepare and heat the support rollers; The support rollers are placed under a temperature of 600-650℃ for a total time of 20-40 hours for material preparation and heat preservation. The [H] content of the support roller is controlled to be below 1 PPM; Step 2: The support rollers processed in Step 1 are then subjected to furnace cooling. In step 2, the furnace is sealed and cooled to 300-400℃, and the process takes 20-30 hours. Step 3: Incubate at 300-400℃ for 10-30 hours. Step 4: After heat preservation, raise the temperature of the support roller to 650-670℃; After heat preservation, the support roller is heated to 650-670℃ at a rate of less than or equal to 30℃ / h, and the process takes 7-10 hours. Step 5: Incubate at 650-670℃ for 10-30 hours. Step 6: Increase the temperature to 880-950℃ at a rate of less than or equal to 50℃ / h, and the process takes 7-10 hours. Step 7: Keep warm at 880-950 ℃ for 20-45 h; Step 8: Cool down to 640-740℃ at a rate of less than or equal to 10℃ / h, with a process time of 20-35h; so that granular pearlite is obtained from the surface of the support roller to the core area; Step 9: Cool down to 400℃ at a rate of less than or equal to 20℃ / h, with a process time of 15-20h; Step 10: Cool down to 150℃ at a rate of less than or equal to 10℃ / h, with a process time of 25-30 h; The diameter of the roller body forging of the support roller is <1700mm, and the material is Cr3\Cr4\Cr5.
2. The short-cycle, low-energy-consumption heat treatment method for support rolls after forging according to claim 1, characterized in that, In step 9, the temperature is reduced to 400°C at a rate of less than or equal to 18°C / h, and the process takes 17-20 hours.
3. The short-cycle, low-energy-consumption heat treatment method for support rolls after forging according to claim 1, characterized in that, In step 1, the support roller is subjected to material preparation and heat preservation at 600-640℃ for a total duration of 20 hours.
4. The short-cycle, low-energy-consumption heat treatment method for support rolls after forging according to claim 1, characterized in that, In step 2, the support rollers processed in step 1 are cooled in a sealed furnace to 310-400℃, and the process takes 25-30 hours.
5. The short-cycle, low-energy-consumption heat treatment method for support rolls after forging according to claim 1, characterized in that, In step 3, the heat preservation time is 10 hours.
6. The short-cycle, low-energy-consumption heat treatment method for support rolls after forging according to claim 1, characterized in that, In step 4, after heat preservation, the support roller is heated to 660-670℃ at a rate of less than or equal to 30℃ / h.
7. The short-cycle, low-energy-consumption heat treatment method for support rolls after forging according to claim 1, characterized in that, In step 5, the heat preservation time is 10 hours.
Citation Information
Patent Citations
Technology for conducting heat treatment of whole-ring magnet yoke forge piece after forging is accomplished
CN113528797A