Vanadium-iron alloy smelting method for improving vanadium yield and vanadium-iron alloy
By using a batching method involving calcium-containing vanadium trioxide with metallic aluminum, iron, and lime, and adding it to the smelting furnace in batches, and strengthening slag reduction at the end of refining, the problems of splashing and vanadium loss in slag in ferrovanadium smelting were solved, achieving high yield and high purity of ferrovanadium alloy production.
Patent Information
- Application Number
- CN202310669099.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-06
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-06-06
AI Technical Summary
The existing ferrovanadium smelting process suffers from severe splashing, high vanadium loss in slag, and high oxygen content in the alloy due to alumina inclusions, which affect production pace and product cleanliness.
Calcium-containing vanadium trioxide is used as the vanadium source, and it is mixed with metallic aluminum, iron and lime. The mixture is added to the smelting furnace in batches, and the remaining lime is evenly distributed at the end of the refining process to enhance slag reduction, control the MgO and Al₂O₃ content in the slag, and improve the vanadium yield.
It suppressed splashing during the smelting process, extended the service life of the equipment, increased the vanadium yield to over 98%, reduced alumina inclusions in the alloy, and improved the cleanliness of the product.
Smart Images

Figure CN116694935B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of ferrovanadium alloy production technology, and more specifically to a ferrovanadium alloy smelting method and ferrovanadium alloy for improving vanadium yield. Background Technology
[0002] Ferrovanadium is the most produced vanadium product, accounting for over 70% of the final vanadium usage. It is an important alloying additive in the steel industry. Vanadium improves the strength, toughness, heat resistance, and ductility of steel. Ferrovanadium is commonly used in the production of carbon steel, low-alloy steel, high-strength steel, high-alloy steel, tool steel, and cast iron.
[0003] Currently, there are four main methods for producing ferrovanadium: carbothermic reduction, ladle reduction, electrosilicon thermal reduction, and electroaluminothermic reduction. Carbothermic reduction uses carbon as a reducing agent and can only produce high-carbon ferrovanadium. Electrosilicon thermal reduction involves using flaky vanadium pentoxide with 75% ferrosilicon and a small amount of aluminum as reducing agents in an alkaline electric arc furnace, undergoing two stages of reduction and refining to obtain a qualified product. Ladle reduction, also known as aluminothermic reduction, is one of the main methods for producing ferrovanadium in China. Because aluminothermic reduction is a multiphase reaction process with high temperature, fast speed, and short time, it is difficult to control once it begins; therefore, the requirements for the batching process are extremely high.
[0004] Currently, the electrothermal process is mainly used in China to smelt ferrovanadium alloys. When smelting ferrovanadium, the furnace body is placed on a smelting flatcar. The smelting flatcar is a flatbed car. The reducer is driven by electrical equipment installed at the bottom of the flatcar and moves along the track to the smelting station. After smelting, it moves out of the smelting station along the original route.
[0005] The high-temperature slag and iron splashed out can easily damage the main structure and electrical equipment of the flatcar, making it impossible to drive the flatcar, resulting in long accident handling time, serious equipment damage, and affecting the production rhythm.
[0006] Current methods for ferrovanadium smelting mainly involve combining vanadium oxide with reducing agent aluminum, calcium oxide, and iron materials to improve vanadium recovery. These methods include changing the batch size of the feed, setting different aluminum ratios for different phases, and optimizing the composition, proportion, and dosage of the depleted feedstock. However, these methods still have problems such as high vanadium loss in the slag, high oxygen content in the alloy due to alumina inclusions, and severe splashing. Summary of the Invention
[0007] The purpose of this invention is to provide a method for smelting ferrovanadium alloys to improve vanadium yield and a ferrovanadium alloy smelted using this method, thereby solving at least one of the aforementioned problems existing in the prior art.
[0008] To achieve the above-mentioned technical objectives, the technical solution adopted by the present invention is as follows:
[0009] According to one aspect of the present invention, a method for smelting ferrovanadium alloys to improve vanadium yield is provided, comprising the following steps:
[0010] Step S1: Add the calcium source to ammonium vanadate to prepare calcium-containing vanadium trioxide;
[0011] Step S2: The calcium-containing vanadium trioxide, metallic aluminum, metallic iron and lime are prepared by mixing the calcium-containing vanadium trioxide, metallic aluminum, metallic iron and a portion of lime to obtain a mixture;
[0012] Step S3: Add the mixture to a smelting furnace and smelt it by electricity;
[0013] Step S4: After smelting, refinement is carried out. After the slag reduction is enhanced by powering on, the remaining lime is evenly distributed into the furnace at the end of the refining process.
[0014] Step S5: After refining, air cool. When the surface temperature of the corundum slag meets the requirements, dismantle the furnace, remove the alloy cake, and water quench it.
[0015] Step S6: Crush and refine the alloy cake to obtain the vanadium-iron alloy.
[0016] According to one embodiment of the present invention, in step S1, the calcium source is selected from one or more of calcium oxide, calcium hydroxide, calcium ferrite, and calcium vanadate, and the ammonium vanadate salt is ammonium metavanadate or ammonium polyvanadate.
[0017] According to one embodiment of the present invention, in step S1, the calcium content in the prepared calcium-containing vanadium trioxide is 1% to 13%.
[0018] According to one embodiment of the present invention, in step S1, the preparation of calcium-containing vanadium trioxide includes adding a calcium source to ammonium vanadate, followed by drying and reduction to obtain calcium-containing vanadium trioxide.
[0019] According to one embodiment of the present invention, in step S2, the iron-vanadium ratio in the mixture is set according to the national standard FeV50 or FeV80 composition requirements, and the CaO / Al ratio in the mixture is set to a range of 0.2 to 0.4.
[0020] According to one embodiment of the present invention, in step S3, the mixture is added to the smelting furnace in one go or in batches.
[0021] According to one embodiment of the present invention, in step S4, the refined material is ball-milled iron particles and aluminum pellets.
[0022] According to one embodiment of the present invention, in step S4, the energizing time for enhancing slag reduction is 15 to 35 minutes.
[0023] According to one embodiment of the present invention, in step S4, 20% to 50% of the lime is evenly distributed into the furnace during the final stage of refining under the condition that the furnace body rotates or the feeding pipe rotates.
[0024] According to another aspect of the present invention, a vanadium-iron alloy with low inclusion content is provided, which is prepared by the above-described method.
[0025] Due to the adoption of the above technical solutions, the vanadium-iron alloy smelting method and vanadium-iron alloy provided by the present invention, which improves vanadium yield, have at least one of the following beneficial effects compared with the prior art:
[0026] (1) The splashing phenomenon during the smelting process is suppressed. The method of the present invention uses calcium-containing vanadium trioxide as the vanadium source. Compared with ordinary vanadium trioxide, the metallurgical performance of the calcium-containing vanadium trioxide is improved, the reactivity and bulk density are increased, the vanadium loss is reduced, and the vanadium iron smelting is strengthened from the source. The splashing phenomenon is improved and the service life of the vanadium iron smelting mobile flatcar is extended.
[0027] (2) Strengthen the refining process in the vanadium-iron smelting process, implement the classification and batch addition of lean materials, and on the basis of conventional batching, move 20% to 50% of the total amount of slag-forming agent calcium oxide to the furnace at the end of refining, which slows down the erosion of the magnesia furnace lining, effectively controls the MgO content in the slag (MgO < 8%), the Al2O3 content in the slag is higher than 80%, the TV content in the slag is lower than 0.8%, and the vanadium smelting yield is higher than 98%, thus improving the vanadium smelting yield.
[0028] (3) The amount of unsettled metal particles in the obtained vanadium-iron corundum slag was significantly reduced, and the area of CaO-Al2O3-based phase in the slag under the microscope increased from the original 30% to more than 60%.
[0029] (4) The alumina inclusions in the alloy are significantly reduced, which lowers the total oxygen content in the ferrovanadium alloy and improves the cleanliness of the ferrovanadium alloy product. Attached Figure Description
[0030] The accompanying drawings are provided to further illustrate the invention and form part of the specification. They are used together with the following detailed description to explain the invention, but do not constitute a limitation thereof. In the drawings:
[0031] Figure 1 A flowchart of a vanadium-iron alloy smelting method for improving vanadium yield according to an embodiment of the present invention;
[0032] Figure 2 The microstructure of corundum slag obtained according to the vanadium-iron alloy smelting method of Comparative Example 1.
[0033] Figure 3The microstructure of corundum slag obtained by the vanadium-iron alloy smelting method for improving vanadium yield according to Example 1. Detailed Implementation
[0034] The specific embodiments of this disclosure will be described in detail below with reference to the accompanying drawings. It should be understood that the specific embodiments described herein are for illustration and explanation only and are not intended to limit this disclosure.
[0035] Furthermore, the reference to "embodiment" herein means that a particular feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of the invention. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a separate or alternative embodiment mutually exclusive with other embodiments. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments.
[0036] Figure 1 A flowchart of a method for smelting ferrovanadium alloys to improve vanadium yield according to the present invention is shown. The method of the present invention will now be described in detail with reference to this flowchart.
[0037] The vanadium-iron alloy smelting method for improving vanadium yield according to the present invention generally includes the following steps:
[0038] Step S1: Add the calcium source to ammonium vanadate to prepare calcium-containing vanadium trioxide;
[0039] Step S2: Prepare the following ingredients: calcium-containing vanadium trioxide, metallic aluminum, metallic iron, and lime. Mix the calcium-containing vanadium trioxide, metallic aluminum, metallic iron, and a portion of lime to obtain a mixture.
[0040] Step S3: Add the mixture to the smelting furnace and smelt it by electricity;
[0041] Step S4: After smelting, refinement is carried out. After the slag reduction is enhanced by powering on, the remaining lime is evenly distributed into the furnace at the end of the refining process.
[0042] Step S5: After refining, air cool. When the surface temperature of the corundum slag meets the requirements, dismantle the furnace, remove the alloy cake, and water quench it.
[0043] Step S6: Crush and refine the alloy cake to obtain the vanadium-iron alloy.
[0044] The following is a detailed explanation of the specific steps involved.
[0045] In step S1, a calcium source is added to ammonium vanadate to prepare calcium-containing vanadium trioxide. The calcium source is selected from one or more of calcium oxide, calcium hydroxide, calcium ferrite, and calcium vanadate. The ammonium vanadate is ammonium metavanadate or ammonium polyvanadate. The calcium content in the prepared calcium-containing vanadium trioxide is 1% to 13%. The calcium source is added to the ammonium vanadate, and after drying and reduction, calcium-containing vanadium trioxide is obtained. The reducing agent can be a conventional reducing agent used to reduce vanadium trioxide with ammonium vanadate, such as, but not limited to, hydrogen, ammonia, and industrial coal gas. The reduction operation can be a conventional operation in the art and is not specifically limited here. The method of the present invention uses calcium-containing vanadium trioxide as a vanadium source. Compared with ordinary vanadium trioxide, the metallurgical properties of this calcium-containing vanadium trioxide are improved, its reactivity and bulk density are increased, the splashing phenomenon during the smelting process is suppressed, vanadium loss is reduced, and ferrovanadium smelting is strengthened from the source.
[0046] In step S2, vanadium trioxide containing calcium, metallic aluminum, metallic iron, and lime are batched. The vanadium trioxide, metallic aluminum, metallic iron, and a portion of the lime are mixed to obtain a mixture. The iron-vanadium ratio in the mixture is set according to the national standard FeV50 or FeV80 composition requirements, and the CaO / Al ratio in the mixture is set to a range of 0.2–0.4. If subsequent steps use a batch feeding method, the batching is divided into several stages according to the process requirements, each required proportion, and then mixed separately according to the required proportion, and placed into separate batch containers for each batch, awaiting use. If subsequent steps use a one-time feeding method, the batching is performed according to the standard proportions for the target product. In this operation, only a portion of the lime is added; the remaining lime is added at the end of the refining process.
[0047] In step S3, the mixture is added to a smelting furnace and smelted under electric current. The mixture can be added to the furnace all at once or in batches. An electric furnace, such as a straight-tube furnace, is used, with the refractory lining made of magnesia, magnesia clay, and brine. The furnace charge is ensured to be evenly distributed within the furnace, preventing accumulation in one area and excessively rapid reaction. Under optimal furnace conditions and with sufficient reaction time, smelting is carried out for 20–25 minutes. During this period, aluminothermic reduction occurs, reducing vanadium trioxide to metallic vanadium.
[0048] In step S4, after smelting, refining is carried out. After slag reduction is enhanced by electric current, residual lime is added as a covering agent, and the lime is evenly distributed into the furnace at the end of refining. The straight-tube furnace is then sent to the refining station for further removal of residual vanadium from the slag using a refining injection process, achieving the purpose of vanadium removal. The refining feed consists of ball-milled iron particles and aluminum pellets. During refining, after slag reduction is enhanced by electric current for 15-35 minutes, lime is added as a covering agent, with 20%-50% of the lime concentrated and evenly distributed at the end of refining under conditions of furnace rotation or feed pipe rotation. Due to the severe erosion of the refractory layer by the molten slag at high temperatures, the MgO content in the slag system increases sharply, the slag melting point rises, the slag viscosity increases, the injection refining efficiency decreases, and the total vanadium content in the slag is too high, reducing the vanadium yield. This invention strengthens the refining process in ferrovanadium smelting by adding depleting agents in batches and categories. Based on conventional batching, 20%-50% of the total amount of calcium oxide slag-forming agent is moved to the furnace at the end of refining, which slows down the erosion of the magnesia furnace lining, effectively controls the MgO content in the slag (MgO < 8%), and improves the vanadium yield.
[0049] In step S5, the refined alloy liquid is air-cooled. When the surface temperature of the corundum slag meets the requirements, the furnace is dismantled, the alloy cake is removed, and water quenching is performed. This step can be performed using conventional procedures in the art. For example, the corundum slag and the alloy are air-cooled together in the furnace. Due to the significant difference in specific gravity, the alloy and slag automatically separate into strata in the molten state. When the surface temperature of the corundum slag is detected by a temperature gun to be 300-500°C, the furnace is dismantled, the alloy cake is removed, and water quenching is performed.
[0050] In step S6, the alloy cake is crushed and refined to obtain a vanadium-iron alloy with low alumina inclusions.
[0051] When vanadium-iron alloys are prepared using this method, the amount of unsettled metal particles in the obtained vanadium-iron corundum slag is significantly reduced, and the area of CaO-Al2O3-based phase in the slag under a microscope increases from the original 30% to over 60%.
[0052] The present invention also provides a vanadium-iron alloy with low alumina inclusions, which is prepared according to the above method.
[0053] The following are specific embodiments of the method for preparing ferrovanadium alloy according to the present invention. Unless otherwise stated, the raw materials, equipment, consumables, etc. used in the following embodiments can be obtained through conventional commercial means.
[0054] For the parts involving numerical ranges, those skilled in the art can choose any value within the numerical range defined by this invention according to actual needs, and are not limited to the values listed in the specific embodiments. In the method of this invention, unless otherwise specified, ratios, contents, etc., all refer to mass percentages.
[0055] Example 1
[0056] First, a calcium source is added to ammonium polyvanadate, followed by drying and reduction to obtain calcium-containing vanadium trioxide with a calcium content of 1%. The calcium source is calcium oxide. The calcium-containing vanadium trioxide is then mixed with metallic aluminum, metallic iron, and lime to obtain a mixture. The iron-vanadium ratio in the mixture is approximately 1:1, meeting the national standard FeV50 composition requirements. The CaO / Al ratio in the mixture is set to a range of 0.2. 80% of the total lime is evenly distributed in each feed hopper. Based on this, batching, mixing, feeding, and electro-smelting are carried out according to conventional batching coefficients. The lean feed consists of ball-milled iron particles and aluminum pellets, which are then subjected to 35 minutes of electro-smelting to enhance slag reduction. Lime is added as a covering agent, and 20% of the total lime is evenly distributed during the final refining stage while the furnace is rotating, serving as both a covering agent and an endothermic agent. After smelting, the corundum slag and alloy are air-cooled together in the furnace. When the surface temperature of the corundum slag reaches 500℃ using a thermometer, the furnace is dismantled. The alloy cake is removed and water-quenched. The alloy cake is crushed and refined to obtain ferrovanadium alloy.
[0057] Example 2
[0058] First, a calcium source is added to ammonium metavanadate, followed by drying and reduction to obtain calcium-containing vanadium trioxide with a calcium content of 5%. The calcium source is calcium hydroxide. The calcium-containing vanadium trioxide is then mixed with metallic aluminum, metallic iron, and lime to obtain a mixture. The iron-vanadium ratio in the mixture is approximately 2:8, set according to the national standard FeV80 composition requirements. The CaO / Al ratio in the mixture is set to a range of 0.3. 50% of the total lime is evenly distributed in each feed hopper. Based on this, the batching, mixing, feeding, and electro-smelting are carried out according to conventional batching coefficients. The lean feed consists of ball-milled iron particles and aluminum pellets. After 35 minutes of enhanced slag reduction via electro-smelting, lime is added as a covering agent. During the final refining stage, with the furnace rotating, 50% of the total lime is evenly distributed as a covering agent and endothermic agent. After smelting, the corundum slag and alloy are air-cooled together in the furnace. When the surface temperature of the corundum slag reaches 300℃ using a thermometer, the furnace is dismantled. The alloy cake is removed and water-quenched. The alloy cake is crushed and refined to obtain ferrovanadium alloy.
[0059] Example 3
[0060] First, a calcium source is added to ammonium polyvanadate, followed by drying and reduction to obtain calcium-containing vanadium trioxide with a calcium content of 8%. The calcium source is calcium vanadate. The calcium-containing vanadium trioxide is then mixed with metallic aluminum, metallic iron, and lime to obtain a mixture. The iron-vanadium ratio in the mixture is approximately 2:8, set according to the national standard FeV80 composition requirements. The CaO / Al ratio in the mixture is set to a range of 0.4, and 50% of the total lime is evenly distributed in each feed hopper. Based on this, batching, mixing, feeding, and electro-smelting are carried out according to conventional batching coefficients. The lean feed consists of ball-milled iron particles and aluminum pellets. After 35 minutes of enhanced slag reduction via electro-smelting, 50% of the total lime is evenly distributed as a covering agent and endothermic agent under the condition of furnace rotation at the end of refining. After smelting, the corundum slag and alloy are air-cooled together in the furnace. When the surface temperature of the corundum slag reaches 400℃ using a temperature measuring gun, the furnace is dismantled. The alloy cake is removed and water-quenched. The alloy cake is crushed and refined to obtain ferrovanadium alloy.
[0061] Example 4
[0062] First, a calcium source is added to ammonium metavanadate, followed by drying and reduction to obtain calcium-containing vanadium trioxide with a calcium content of 13%. The calcium source is calcium vanadate. The calcium-containing vanadium trioxide is then mixed with metallic aluminum, metallic iron, and lime to obtain a mixture. The iron-vanadium ratio in the mixture is approximately 2:8, set according to the national standard FeV80 composition requirements. The CaO / Al ratio in the mixture is set to a range of 0.3, and 65% of the total lime is evenly distributed in each feed hopper. Based on this, batching, mixing, feeding, and electro-smelting are carried out according to conventional batching coefficients. The lean feed consists of ball-milled iron particles and aluminum pellets. After 35 minutes of enhanced slag reduction via electro-smelting, lime is added as a covering agent. During the final refining stage, with the furnace rotating, 35% of the total lime is evenly distributed as a covering agent and endothermic agent. After smelting, the corundum slag and alloy are air-cooled together in the furnace. When the surface temperature of the corundum slag reaches 400℃ using a temperature measuring gun, the furnace is dismantled. The alloy cake is removed and water-quenched. The alloy cake is crushed and refined to obtain ferrovanadium alloy.
[0063] Comparative Example 1
[0064] Ammonium metavanadate is dried and reduced to obtain conventional vanadium trioxide. Vanadium trioxide is then mixed with metallic aluminum, metallic iron, and lime to obtain a mixture. The iron-vanadium ratio in the mixture is approximately 1:1, set according to the national standard FeV50 composition requirements. The CaO / Al ratio in the mixture is set to a range of 0.2, and 90% of the total lime is evenly distributed in each feed hopper. Based on this, the mixture is batched, mixed, fed, and smelted using conventional batching coefficients. The lean feed consists of ball-milled iron particles and aluminum pellets. After 35 minutes of enhanced slag reduction using electricity, the remaining 10% of lime is added during the final refining stage when the furnace is stationary. After smelting, the corundum slag and alloy are air-cooled together in the furnace. When the surface temperature of the corundum slag reaches 500℃ using a thermometer, the furnace is dismantled. The alloy cake is removed and water-quenched. The alloy cake is then crushed and refined to obtain ferrovanadium alloy.
[0065] Comparative Example 2
[0066] Ammonium metavanadate is dried and reduced to obtain conventional vanadium trioxide. Vanadium trioxide is then mixed with metallic aluminum, metallic iron, and lime to obtain a mixture. The iron-vanadium ratio in the mixture is approximately 2:8, set according to the national standard FeV80 composition requirements. The CaO / Al ratio in the mixture is set to a range of 0.3, and 90% of the total lime is evenly distributed in each feed hopper. Based on this, the mixture is batched, mixed, fed, and smelted using conventional batching coefficients. The lean feed consists of ball-milled iron particles and aluminum pellets. After 35 minutes of enhanced slag reduction using electricity, the remaining 10% of lime is added during the final refining stage when the furnace is stationary. After smelting, the corundum slag and alloy are air-cooled together in the furnace. When the surface temperature of the corundum slag reaches 300℃ using a thermometer, the furnace is dismantled. The alloy cake is removed and water-quenched. The alloy cake is then crushed and refined to obtain ferrovanadium alloy.
[0067] Comparative Example 3
[0068] Ammonium metavanadate is dried and reduced to obtain conventional vanadium trioxide. Vanadium trioxide is then mixed with metallic aluminum, metallic iron, and lime to obtain a mixture. The iron-vanadium ratio in the mixture is approximately 2:8, set according to the national standard FeV80 composition requirements. The CaO / Al ratio in the mixture is set to a range of 0.4, and 90% of the total lime is evenly distributed in each feed hopper. Based on this, the mixture is batched, mixed, fed, and smelted using conventional batching coefficients. The lean feed consists of ball-milled iron particles and aluminum pellets. After 35 minutes of enhanced slag reduction using electricity, the remaining 10% of lime is added during the final refining stage when the furnace is stationary. After smelting, the corundum slag and alloy are air-cooled together in the furnace. When the surface temperature of the corundum slag reaches 400℃ using a thermometer, the furnace is dismantled. The alloy cake is removed and water-quenched. The alloy cake is then crushed and refined to obtain ferrovanadium alloy.
[0069] Comparative Example 4
[0070] Ammonium metavanadate is dried and reduced to obtain conventional vanadium trioxide. Vanadium trioxide is then mixed with metallic aluminum, metallic iron, and lime to obtain a mixture. The iron-vanadium ratio in the mixture is approximately 2:8, set according to the national standard FeV80 composition requirements. The CaO / Al ratio in the mixture is set to a range of 0.3, and 90% of the total lime is evenly distributed in each feed hopper. Based on this, the mixture is batched, mixed, fed, and smelted using conventional batching coefficients. The lean feed consists of ball-milled iron particles and aluminum pellets. After 35 minutes of enhanced slag reduction using electricity, the remaining 10% of lime is added during the final refining stage when the furnace is stationary. After smelting, the corundum slag and alloy are air-cooled together in the furnace. When the surface temperature of the corundum slag reaches 400℃ using a thermometer, the furnace is dismantled. The alloy cake is removed and water-quenched. The alloy cake is then crushed and refined to obtain ferrovanadium alloy.
[0071] The splashing behavior of Examples 1-4 and Comparative Examples 1-4 was observed, and the TV (total vanadium) content in the slag was detected. The results are shown in Table 1 below:
[0072] Table 1 Comparison of test results
[0073]
[0074] As shown in Table 1 above, the ferrovanadium smelting method of the present invention results in low TV content in the slag, no significant splashing during the smelting process, reduced flatcar damage, and a vanadium yield of over 98%. In contrast, conventional ferrovanadium smelting methods involve splashing during the smelting process, leading to increased vanadium loss and flatcar malfunctions.
[0075] Figure 2 The microstructure of corundum slag obtained according to the method of Comparative Example 1 is shown. Figure 3 The microstructure of corundum slag obtained by the vanadium-iron alloy smelting method for improving vanadium yield according to Example 1 is shown. As shown in the figure, the area of the CaO-Al2O3-based phase in the slag under the microscope increased from 30% in Comparative Example 1 to more than 60% in Example 1, and mechanically entrained metal particles were basically not observed. This indicates that the amount of non-settled metal particles in the vanadium-iron corundum slag obtained by the method of the present invention is significantly reduced.
[0076] The preferred embodiments of the present invention have been described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the scope of the technical concept of the present invention, various simple modifications can be made to the technical solution of the present invention, and these simple modifications all fall within the protection scope of the present invention.
[0077] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not describe the various possible combinations separately.
[0078] Furthermore, various different embodiments of the present invention can be combined in any way, as long as they do not violate the spirit of the present invention, they should also be regarded as the content disclosed by the present invention.
Claims
1. A method for smelting ferrovanadium alloys to improve vanadium yield, characterized in that, Includes the following steps: Step S1: Add the calcium source to ammonium vanadate, and prepare calcium-containing vanadium trioxide by drying and reduction. The calcium content in the calcium-containing vanadium trioxide is 1%~13%. Step S2: The calcium-containing vanadium trioxide, metallic aluminum, metallic iron and lime are prepared by mixing the calcium-containing vanadium trioxide, metallic aluminum, metallic iron and a portion of lime to obtain a mixture; Step S3: Add the mixture to a smelting furnace and smelt it by electricity; Step S4: After smelting, refinement is carried out. After the slag reduction is enhanced by powering on, the remaining lime is evenly distributed into the furnace at the end of the refining process. Step S5: After refining, air cool. When the surface temperature of the corundum slag meets the requirements, dismantle the furnace, remove the alloy cake, and water quench it. Step S6: Crush and refine the alloy cake to obtain the vanadium-iron alloy.
2. The method according to claim 1, characterized in that, In step S1, the calcium source is selected from one or more of calcium oxide, calcium hydroxide, calcium ferrite, and calcium vanadate, and the ammonium vanadate salt is ammonium metavanadate or ammonium polyvanadate.
3. The method according to claim 1, characterized in that, In step S2, the iron-vanadium ratio in the mixture is set according to the national standard FeV50 or FeV80 composition requirements, and the CaO / Al ratio in the mixture is set to a range of 0.2 to 0.
4.
4. The method according to claim 1, characterized in that, In step S3, the mixture is added to the smelting furnace either all at once or in batches.
5. The method according to claim 1, characterized in that, In step S4, the refining material consists of ball milled iron pellets and aluminum granules.
6. The method according to claim 1, characterized in that, In step S4, the energizing time for enhancing slag reduction is 15~35min.
7. The method according to claim 1, characterized in that, In step S4, 20% to 50% of the lime is evenly distributed into the furnace during the final stage of refining, under the condition that the furnace body or the feeding pipe is rotating.
8. A low-oxygen-content ferrovanadium alloy, characterized in that, The ferrovanadium alloy is prepared by the method according to any one of claims 1-7, and the total oxygen content in the ferrovanadium alloy is 0.01% to 0.5%.
Citation Information
Patent Citations
Method for preparing calciferous vanadium oxide from vanadate
CN102676817A
V2O3 electro-aluminothermic process for semelting FeV50
CN1343795A