LED chip and preparation method thereof
By growing a buffer layer and an isolation layer on the substrate, etching to form a groove, and growing an epitaxial layer in the groove, the sidewall damage caused by etching and dividing the epitaxial layer is solved, thereby improving the luminous brightness and crystal quality of the LED chip.
Patent Information
- Application Number
- CN202310760740.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-26
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-06-26
AI Technical Summary
In existing technologies, when fabricating micro LED chips by etching and dividing the epitaxial layer, the sidewalls of the epitaxial layer are easily damaged, resulting in a decrease in luminous brightness.
A buffer layer and an isolation layer are grown sequentially on a substrate, a groove is etched to form a trench, and a transition layer is deposited in the trench. Then, an epitaxial layer is grown, and finally the isolation layer is removed by an etching solution to form an independent LED chip.
This effectively avoids damage to the sidewalls of the epitaxial layer during etching, improves the luminous brightness of the LED chip, and ensures the crystal quality and isolation effect of the epitaxial layer.
Smart Images

Figure CN116705922B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of semiconductor technology, and more specifically to an LED chip and its fabrication method. Background Technology
[0002] A light-emitting diode (LED) is a semiconductor component. LEDs are known as the fourth generation of lighting sources or green light sources, characterized by energy saving, environmental friendliness, long lifespan, and small size. They are widely used in various indication, display, decoration, backlighting, general lighting, and urban nightscape applications. Based on their function, LEDs can be categorized into five main types: information display, signal lights, automotive lighting, LCD backlighting, and general lighting.
[0003] The most common method for manufacturing LED chips is to grow an epitaxial layer on the entire surface of a large wafer substrate, and then use photolithography to etch isolation trenches on the epitaxial layer to separate each LED chip. With the continuous development of technology, in order to achieve better light source display effects, LED chips are gradually becoming miniaturized. However, due to process limitations, sidewall damage is often encountered in the photolithography process. Sidewall damage itself can lead to non-radiative recombination in the LED chip, which greatly affects the radiative recombination efficiency of electrons and holes in the active layer, resulting in a decrease in luminous brightness. Summary of the Invention
[0004] In view of the shortcomings of the prior art, the purpose of this invention is to provide an LED chip and its preparation method, which aims to solve the technical problem that the existing technology of fabricating micro LED chips by etching and dividing the epitaxial layer is prone to causing damage to the sidewalls of the epitaxial layer, resulting in a reduction in luminous brightness.
[0005] The present invention provides a method for fabricating an LED chip, the method comprising:
[0006] A substrate is provided, and a buffer layer and an isolation layer are sequentially grown on the substrate;
[0007] The isolation layer is etched according to a preset etching pattern until the etched portion of the isolation layer exposes the buffer layer, so as to etch a number of spaced grooves on the isolation layer.
[0008] A transition layer is deposited in the groove, and an epitaxial layer is grown on the transition layer;
[0009] After the epitaxial layer has grown, the isolation layer is completely etched away using an etching solution.
[0010] Compared with the prior art, the beneficial effects of the present invention are as follows: the LED chip fabrication method provided by the present invention can effectively avoid the problem of sidewall damage during etching of the epitaxial layer and improve the luminous brightness of the LED chip. Specifically, the LED chip fabrication method includes: providing a substrate and sequentially growing a buffer layer and an isolation layer on the substrate; etching the isolation layer according to a preset etching pattern until the etched portion of the isolation layer exposes the buffer layer, thereby etching a plurality of spaced grooves on the isolation layer; the setting of the grooved isolation layer facilitates the isolation of the growth of each LED chip and avoids damage to the sidewalls of the epitaxial layer during etching. The epitaxial layers of the LED chip are bonded together and grown; a transition layer is deposited in the groove to improve the flatness of the bottom surface and sidewalls of the isolation layer of the groove structure, reduce the growth of crystal dislocations, and improve the crystal quality of the subsequently grown epitaxial layer; an epitaxial layer is grown on the transition layer; after the epitaxial layer has grown, the isolation layer is completely etched away with an etching solution to form isolation grooves, thereby forming individual well-divided LED chips. This solves the technical problem that etching and dividing the epitaxial layer during the fabrication of micro LED chips can easily cause damage to the sidewalls of the epitaxial layer, leading to a reduction in luminous brightness.
[0011] According to one aspect of the above technical solution, the isolation layer is a silicon dioxide layer, and the thickness of the isolation layer is greater than the thickness of the epitaxial layer, or the thickness of the isolation layer is less than the thickness of the epitaxial layer, with the thickness difference being less than [missing information].
[0012] According to one aspect of the above technical solution, the growth step of the isolation layer specifically includes:
[0013] The temperature is adjusted to 230℃-350℃, the pressure is adjusted to 60pa-180pa, and N2, SiH4, and N2O with flow rates of 200sccm-1000sccm, 50sccm-350sccm, and 400sccm-1500sccm are introduced to grow an isolation layer on the buffer layer.
[0014] According to one aspect of the above technical solution, the step of etching the isolation layer according to a preset etching pattern until the etched portion of the isolation layer exposes the buffer layer, thereby etching a plurality of spaced grooves on the isolation layer, specifically includes:
[0015] Adjust the pressure to 5mTorr-10mTorr, and introduce CF4 at a flow rate of 120sccm-280sccm, Ar at 10sccm-50sccm, and O2 at 10sccm-50sccm. Set the upper electrode RF power to 900W-1100W and the lower electrode RF power to 400W-600W. Etch the isolation layer using a hard mask with a preset etching pattern until the etched portion of the isolation layer exposes the buffer layer, thereby etching several spaced grooves on the isolation layer.
[0016] According to one aspect of the above technical solution, the etching solution includes a hydrofluoric acid solution and an ammonium fluoride solution, wherein the volume ratio of the hydrofluoric acid solution to the ammonium fluoride solution is (5.5-6.5):1.
[0017] According to one aspect of the above technical solution, the transition layer is an N-type AlGaN layer, and the thickness of the transition layer is 9nm-15nm.
[0018] According to one aspect of the above technical solution, the Al content of the transition layer is 0.11-0.18, and the dopant of the transition layer is silane.
[0019] Another aspect of the present invention is to provide an LED chip, the LED chip being prepared by the LED chip preparation method described above, the LED chip comprising a substrate, a buffer layer, a transition layer and an epitaxial layer stacked on the substrate.
[0020] According to one aspect of the above technical solution, the epitaxial layer includes an N-type semiconductor layer, a multiple quantum well layer, and a P-type semiconductor layer. The N-type semiconductor layer is an N-type GaN layer. The multiple quantum well layer includes several quantum well layers and quantum barrier layers stacked alternately in a periodic manner. The P-type semiconductor layer is a P-type GaN layer.
[0021] According to one aspect of the above technical solution, the thickness of the N-type semiconductor layer is 0.5μm-4μm, and the thickness of the P-type semiconductor is 130nm-500nm. Attached Figure Description
[0022] The above and / or additional aspects and advantages of the present invention will become apparent and readily understood from the description of the embodiments taken in conjunction with the following drawings, in which:
[0023] Figure 1 This is a flowchart of the LED chip fabrication method in this invention;
[0024] Figure 2 This is a schematic diagram of the LED chip fabrication method in this invention;
[0025] Component symbol explanation in the attached diagram:
[0026] Substrate 10, buffer layer 20, isolation layer 30, groove 31, transition layer 40, epitaxial layer 50. Detailed Implementation
[0027] To make the objectives, features, and advantages of the present invention more apparent and understandable, specific embodiments of the present invention will be described in detail below with reference to the accompanying drawings. Several embodiments of the present invention are shown in the drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. Rather, these embodiments are provided so that the disclosure of the present invention will be more thorough and complete.
[0028] It should be noted that when an element is referred to as being "fixed to" another element, it can be directly on the other element or there may be an intervening element. When an element is considered to be "connected" to another element, it can be directly connected to the other element or there may be an intervening element. The terms "vertical," "horizontal," "left," "right," "upper," "lower," and similar expressions used herein are for illustrative purposes only and are not intended to indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as limiting the invention.
[0029] In this invention, unless otherwise expressly specified and limited, the terms "installation," "connection," "linking," and "fixing," etc., should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral connection; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; and they can refer to the internal communication between two components. Those skilled in the art can understand the specific meaning of the above terms in this invention according to the specific circumstances. The term "and / or" as used herein includes any and all combinations of one or more of the related listed items.
[0030] Please see Figures 1-2 The image shows a method for fabricating an LED chip according to the present invention, the method comprising steps S10-S13:
[0031] Step S10: Provide a substrate, and grow a buffer layer and an isolation layer sequentially on the substrate;
[0032] The substrate 10 is made of one of sapphire, SiC, Si and ZnO, and can be a patterned substrate or a flat substrate.
[0033] A buffer layer 20 is grown on the substrate 10. The buffer layer 20 is used to alleviate the lattice mismatch and thermal mismatch between the substrate 10 and the epitaxial layer 50 and reduce the generation of dislocations. The buffer layer 20 is prepared by sputtering. The sputtering method for preparing the buffer layer 20 has the advantages of strong thickness controllability and high crystal orientation, and is conducive to the nucleation and growth of light-emitting epitaxial structures. The buffer layer 20 includes one of AlN layer, BN layer and AlGaN layer. For example, the crystal orientation or main crystal orientation of AlN layer is (0001).
[0034] Preferably, the thickness of the buffer layer 20 is 200-280 Å.
[0035] Among them, the isolation layer 30 is a SiO2 layer.
[0036] Specifically, the temperature is adjusted to 230℃-350℃, the pressure is adjusted to 60pa-180pa, and N2, SiH4, and N2O with flow rates of 200sccm-1000sccm, 50sccm-350sccm, and 400sccm-1500sccm are introduced to grow an isolation layer 30 on the buffer layer 20.
[0037] Among them, the gas flow rate ratio determines the proportion of silicon and oxygen content in the isolation layer 30.
[0038] It should be noted that, due to the inconsistency in the lattice structure between the isolation layer 30 and the epitaxial layer 50, the epitaxial layer 50 is not easily grown on the isolation layer 30. Therefore, it is possible to form spaced grooves 31 to facilitate the isolation of each LED chip. However, if the isolation layer 30 is grown first, and then the buffer layer 20 and the epitaxial layer 50 are grown, the epitaxial layer 50 will be deposited on the mesa of the groove 31 of the isolation layer 30 under the action of the buffer layer 20. This will cause the epitaxial layers 50 grown in each groove 31 to merge and grow, forming a complete epitaxial layer 50 that cannot be isolated and separated.
[0039] Therefore, growing the isolation layer 30 on the buffer layer 20 is beneficial for the isolation and segmentation of the LED chip without damaging the sidewalls. This improves the luminous brightness. It avoids the sidewall damage that can easily occur when fabricating micro-LED chips through etching, leading to non-radiative recombination within the LED chip and a decrease in luminous brightness.
[0040] Secondly, the thickness of the isolation layer 30 is greater than the thickness of the epitaxial layer 50, or the thickness of the isolation layer 30 is less than the thickness of the epitaxial layer 50, and the thickness difference is less than...
[0041] The isolation layer 30 is thicker than the epitaxial layer 50. This effectively prevents the epitaxial layer 50 from growing laterally and merging together after its thickness exceeds that of the isolation layer 30, thus preventing it from becoming a single, indivisible unit. To save materials and costs, the isolation layer 30 can also be thinner than the epitaxial layer 50, but the thickness difference should be less than [a certain value]. This is to achieve a better effect in improving brightness. When the thickness difference is too large, the epitaxial layer 50 will grow laterally and merge together after exceeding the isolation layer 30, causing the epitaxial layer 50 to merge into a whole and become impossible to isolate and cut.
[0042] Step S11: Etch the isolation layer according to the preset etching pattern until the etched part of the isolation layer exposes the buffer layer, so as to etch a number of spaced grooves on the isolation layer.
[0043] Specifically, the pressure is adjusted to 5mTorr-10mTorr, and a flow rate of 120sccm-280sccm of CF4, 10sccm-50sccm of Ar, and 10sccm-50sccm of O2 is introduced. The RF power of the upper electrode is set to 900W-1100W, and the RF power of the lower electrode is set to 400W-600W. The isolation layer 30 is etched through a hard mask with a preset etching pattern until the etched part of the isolation layer 30 exposes the buffer layer 20, so as to etch a number of spaced grooves on the isolation layer 30.
[0044] The etching time is 350s-1200s. The thickness of the isolation layer 30 will affect the etching effect. When the isolation layer 30 is too thick, the etching angle will be offset when etching from the surface to the bottom surface. The resulting sidewalls will have a certain angle, which will affect the growth of the epitaxial layer 50 and thus affect the performance of the LED chip.
[0045] In addition, the length and width of the groove 31 are adapted to the size of the LED chip and can be designed according to specific needs.
[0046] Step S12: Deposit a transition layer in the groove and grow an epitaxial layer on the transition layer;
[0047] The transition layer 40 is an N-type AlGaN layer with an Al content of 0.11-0.18%. The dopant in the transition layer 40 is silane to match the lattice constants of the buffer layer 20 and the epitaxial layer 50. On one hand, the transition layer 40 serves as a transition layer between the buffer layer 20 and the epitaxial layer 50, alleviating the lattice mismatch between them. On the other hand, etching can cause unevenness and non-uniformity on the bottom sidewalls of the isolation layer 30. The transition layer 40 is used to improve the flatness of the bottom surface and sidewalls of the isolation layer 30, reducing dislocation growth and thus improving the crystal quality of the epitaxial layer 50.
[0048] In addition, the thickness of the transition layer 40 is 9nm-15nm. When the thickness is too thin, the flatness improvement of the transition layer 40 is limited, and crystal dislocations will be generated, which will reduce the crystal quality of the epitaxial layer 50. When the thickness is too thick, it will affect the carrier migration rate.
[0049] The epitaxial layer 50 includes an N-type semiconductor layer, a multiple quantum well layer, and a P-type semiconductor layer.
[0050] The N-type semiconductor layer is an N-type GaN layer with a thickness of 0.5μm-4μm. It is used to provide electrons to recombine with the quantum well layer and holes to achieve the light-emitting effect of the LED chip.
[0051] The multiple quantum well layer consists of several periodically alternating quantum well layers and quantum barrier layers. The quantum well layers are InGaN layers, and the quantum barrier layers are GaN layers, with a period of 5.
[0052] The P-type semiconductor layer is a P-type GaN layer with a thickness of 130nm-500nm. It is used to provide a multi-quantum well layer for the recombination of holes and electrons to achieve the light-emitting effect of LED chips.
[0053] When the height of the isolation layer 30 is lower than the height of the epitaxial layer 50, due to the characteristics of the epitaxial layer 50, the portion of the epitaxial layer 50 that is higher than the isolation layer 30 will grow laterally. Therefore, the height difference is lower than... At this time, the lateral growth of each LED chip will not stick together, and will not affect the crystal quality of the epitaxial layer 50.
[0054] Step S13: After the epitaxial layer has grown, the isolation layer is completely etched away using an etching solution.
[0055] The etching solution includes hydrofluoric acid solution and ammonium fluoride solution, with a volume ratio of (5.5-6.5):1 between the hydrofluoric acid solution and the ammonium fluoride solution. The concentration of hydrofluoric acid in the hydrofluoric acid solution is 49%, and the concentration of ammonium fluoride in the ammonium fluoride solution is 40%. The solvent is water.
[0056] The LED chip is placed in the etching solution and etched for 5-10 minutes to remove the isolation layer 30 of the groove 31 structure, resulting in individual well-divided LED chips.
[0057] In addition, the present invention also provides an LED chip, which is prepared by the above-described LED chip preparation method.
[0058] The LED chip includes a substrate, and a buffer layer, a transition layer and an epitaxial layer stacked sequentially on the substrate. The epitaxial layer includes an N-type semiconductor layer, a multiple quantum well layer and a P-type semiconductor layer.
[0059] An isolation layer is placed on a buffer layer, and grooves are etched to form spaced grooves. In the grooves, a transition layer, an N-type semiconductor layer, a multi-quantum well layer, and a P-type semiconductor layer are sequentially stacked on the buffer layer to achieve the function of isolating and dividing the LED chip. After the stacking is completed, the isolation layer of the groove structure is etched away to form individual LED chips that are well divided. This avoids the risk of sidewall damage to the epitaxial layer caused by etching and dividing the epitaxial layer to make micro LED chips, which would lead to a decrease in luminous brightness.
[0060] The N-type semiconductor layer is an N-type GaN layer, the multiple quantum well layer consists of several periodically alternating quantum well layers and quantum barrier layers, and the P-type semiconductor layer is a P-type GaN layer. The thickness of the N-type semiconductor layer is 0.5μm-4μm, and the thickness of the P-type semiconductor layer is 130nm-500nm.
[0061] The present invention is further illustrated below with specific embodiments:
[0062] Example 1
[0063] The first embodiment of the present invention provides a method for fabricating an LED chip, the method comprising steps S10-S13:
[0064] Step S10: Provide a substrate, and grow a buffer layer and an isolation layer sequentially on the substrate;
[0065] The substrate material includes one of sapphire, SiC, Si and ZnO, and the substrate can be a patterned substrate or a flat substrate.
[0066] The buffer layer includes one of AlN layer, BN layer, and AlGaN layer. For example, the crystal orientation or main crystal orientation of the AlN layer is (0001).
[0067] Preferably, the thickness of the buffer layer is 200-280 Å.
[0068] The isolation layer is a SiO2 layer.
[0069] Specifically, the temperature is adjusted to 230℃-350℃, the pressure is adjusted to 60pa-180pa, and N2, SiH4, and N2O with flow rates of 200sccm-1000sccm, 50sccm-350sccm, and 400sccm-1500sccm are introduced to grow an isolation layer on the buffer layer.
[0070] Secondly, the thickness of the isolation layer is greater than the thickness of the epitaxial layer, or the thickness of the isolation layer is less than the thickness of the epitaxial layer, and the thickness difference is...
[0071] Step S11: Etch the isolation layer according to the preset etching pattern until the etched part of the isolation layer exposes the buffer layer, so as to etch a number of spaced grooves on the isolation layer.
[0072] Specifically, the pressure is adjusted to 5mTorr-10mTorr, and the flow rates of CF4 (120sccm-280sccm), Ar (10sccm-50sccm), and O2 (10sccm-50sccm) are introduced. The RF power of the upper electrode is set to 900W-1100W, and the RF power of the lower electrode is set to 400W-600W. The isolation layer is etched using a hard mask with a preset etching pattern until the etched part of the isolation layer exposes the buffer layer, so as to etch several spaced grooves on the isolation layer.
[0073] The etching time is 350s-1200s.
[0074] In addition, the length and width of the groove are adapted to the size of the LED chip, and can be designed according to specific needs.
[0075] Step S12: Deposit a transition layer in the groove and grow an epitaxial layer on the transition layer;
[0076] The transition layer is an N-type AlGaN layer with an Al content of 0.11-0.18% and silane as the dopant.
[0077] In addition, the thickness of the transition layer is 12nm.
[0078] The epitaxial layer includes an N-type semiconductor layer, a multiple quantum well layer, and a P-type semiconductor layer.
[0079] The N-type semiconductor layer is an N-type GaN layer with a thickness of 0.5μm-4μm. The multiple quantum well layer consists of several alternating layers of quantum well layers and quantum barrier layers. The quantum well layers are InGaN layers, and the quantum barrier layers are GaN layers with a period of 5. The P-type semiconductor layer is a P-type GaN layer with a thickness of 130nm-500nm.
[0080] Step S13: After the epitaxial layer has grown, the isolation layer is completely etched away using an etching solution.
[0081] The etching solution includes hydrofluoric acid solution and ammonium fluoride solution, with a volume ratio of (5.5-6.5):1 between the hydrofluoric acid solution and the ammonium fluoride solution. The concentration of hydrofluoric acid in the hydrofluoric acid solution is 49%, and the concentration of ammonium fluoride in the ammonium fluoride solution is 40%. The solvent is water.
[0082] The LED chip is placed in the etching solution and etched for 5-10 minutes to remove the isolation layer of the groove structure, resulting in individual LED chips that are perfectly segmented.
[0083] Example 2
[0084] The second embodiment of the present invention provides a method for fabricating an LED chip. The difference between the LED chip fabrication method in this embodiment and the LED chip fabrication method in the first embodiment is that:
[0085] The thickness of the isolation layer is less than the thickness of the epitaxial layer, and the thickness difference is...
[0086] Example 3
[0087] The third embodiment of the present invention provides a method for fabricating an LED chip. The difference between the LED chip fabrication method in this embodiment and the LED chip fabrication method in the first embodiment is that:
[0088] The thickness of the isolation layer is less than the thickness of the epitaxial layer, and the thickness difference is...
[0089] Example 4
[0090] The fourth embodiment of the present invention provides a method for fabricating an LED chip. The difference between the LED chip fabrication method in this embodiment and the LED chip fabrication method in the first embodiment is that:
[0091] The thickness of the transition layer is 9 nm.
[0092] Example 5
[0093] The fifth embodiment of the present invention provides a method for fabricating an LED chip. The difference between the LED chip fabrication method in this embodiment and the LED chip fabrication method in the first embodiment is that:
[0094] The thickness of the transition layer is 15 nm.
[0095] Comparative Example 1
[0096] The first comparative example of this invention provides a method for fabricating an LED chip. The difference between the LED chip fabrication method in this comparative example and the LED chip fabrication method in the first embodiment is that:
[0097] Traditionally, isolation trenches are etched into the epitaxial layer using photolithography to separate each LED chip.
[0098] Please refer to Table 1 below, which shows the parameters corresponding to Embodiments 1 to 5 and Comparative Example 1 of the present invention.
[0099] Table 1
[0100]
[0101]
[0102] It should be noted that the epitaxial wafers of Examples 1 to 5 and Comparative Example 1 were manufactured using the same process conditions and their performance was tested at a current of 100mA.
[0103] Based on the data from Examples 1 to 5 and Comparative Example 1, it can be seen that by growing an isolation layer on the buffer layer, etching to form a groove, and growing an epitaxial layer in the groove, the problem of damage to the sidewalls of the epitaxial layer during etching can be effectively avoided, thereby improving the luminous brightness of the LED chip.
[0104] Based on the data from Examples 1 to 3, it can be seen that when the thickness difference is too large, the epitaxial layer will grow laterally beyond the isolation layer and merge together, causing the epitaxial layer to merge into a whole and become impossible to isolate and cut. When the thickness difference is too small, it will not affect the performance of the LED chip, but it will reduce the process efficiency and increase the cost.
[0105] Based on the data from Examples 1, 4, and 5, it can be seen that when the thickness of the transition layer is too thin, the improvement in flatness is limited, crystal dislocations are generated, which will reduce the crystal quality of the epitaxial layer and cause the luminous brightness of the LED chip to decrease; when the thickness is too thick, it affects the migration rate of charge carriers, which also causes the luminous brightness of the LED chip to decrease.
[0106] In summary, by growing an isolation layer on the buffer layer, etching to form a groove, and growing an epitaxial layer within the groove, the problem of sidewall damage during epitaxial etching can be effectively avoided, thereby improving the luminous brightness of the LED chip.
[0107] In the description of this specification, references to terms such as "one embodiment," "some embodiments," "example," "specific example," or "some examples," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.
[0108] The embodiments described above are merely illustrative of several implementations of the present invention, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the present invention. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these all fall within the protection scope of the present invention. Therefore, the protection scope of this patent should be determined by the appended claims.
Claims
1. A method for fabricating an LED chip, characterized in that, The method for preparing the LED chip includes: A substrate is provided, and a buffer layer and an isolation layer are sequentially grown on the substrate. The growth steps of the isolation layer specifically include: The temperature is adjusted to 230℃-350℃, the pressure is adjusted to 60pa-180pa, and N2, SiH4, and N2O with a flow rate of 200sccm-1000sccm, 50sccm-350sccm, and 400sccm-1500sccm are introduced to grow an isolation layer on the buffer layer. The isolation layer is etched according to a preset etching pattern until the etched portion of the isolation layer exposes the buffer layer, so as to etch a number of spaced grooves on the isolation layer. A transition layer is deposited in the groove, and an epitaxial layer is grown on the transition layer; After the epitaxial layer has grown, the isolation layer is completely etched away using an etching solution.
2. The method for preparing an LED chip according to claim 1, characterized in that, The isolation layer is a SiO2 layer, and the thickness of the isolation layer is greater than the thickness of the epitaxial layer, or the thickness of the isolation layer is less than the thickness of the epitaxial layer, with the thickness difference being less than 3500Å-7000Å.
3. The method for preparing an LED chip according to claim 1, characterized in that, The step of etching the isolation layer according to a preset etching pattern until the etched portion of the isolation layer exposes the buffer layer, thereby etching a plurality of spaced grooves on the isolation layer, specifically includes: Adjust the pressure to 5mTorr-10mTorr, and introduce CF4 at a flow rate of 120sccm-280sccm, Ar at 10sccm-50sccm, and O2 at 10sccm-50sccm. Set the upper electrode RF power to 900W-1100W and the lower electrode RF power to 400W-600W. Etch the isolation layer using a hard mask with a preset etching pattern until the etched portion of the isolation layer exposes the buffer layer, thereby etching several spaced grooves on the isolation layer.
4. The method for preparing an LED chip according to claim 1, characterized in that, The etching solution includes hydrofluoric acid solution and ammonium fluoride solution, wherein the volume ratio of hydrofluoric acid solution to ammonium fluoride solution is (5.5-6.5):
1.
5. The method for preparing an LED chip according to claim 1, characterized in that, The transition layer is an N-type AlGaN layer with a thickness of 9nm-15nm.
6. The method for preparing an LED chip according to claim 5, characterized in that, The Al content of the transition layer is 0.11-0.18, and the dopant of the transition layer is silane.
7. An LED chip, characterized in that, The LED chip is prepared by the method for preparing an LED chip according to any one of claims 1-6, and the LED chip includes a substrate, a buffer layer, a transition layer and an epitaxial layer stacked on the substrate.
8. The LED chip according to claim 7, characterized in that, The epitaxial layer includes an N-type semiconductor layer, a multiple quantum well layer, and a P-type semiconductor layer. The N-type semiconductor layer is an N-type GaN layer. The multiple quantum well layer includes several periodically alternating quantum well layers and quantum barrier layers. The P-type semiconductor layer is a P-type GaN layer.
9. The LED chip according to claim 8, characterized in that, The thickness of the N-type semiconductor layer is 0.5μm-4μm, and the thickness of the P-type semiconductor layer is 130nm-500nm.
Citation Information
Patent Citations
Method for improving brightness of flip LED chip
CN115692559A
Semiconductor light emitting device
JP1998209499A