Light emitting diode epitaxial wafer and preparation method thereof, and light emitting diode

By introducing a periodic multi-quantum-well layer structure into the epitaxial wafer of a GaN-based light-emitting diode and utilizing the co-doping of Be, Mg, and O to optimize the doping concentration and growth conditions, the problems of poor carrier expansion capability and insufficient antistatic capability were solved, thereby improving luminous efficiency and reducing operating voltage.

CN116705931BActive Publication Date: 2026-11-24JIANGXI ZHAO CHI SEMICON CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310572852.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-19
Publication Date
2026-11-24
Estimated Expiration
2043-05-19

AI Technical Summary

Technical Problem

Traditional GaN-based light-emitting diode epitaxial wafers suffer from problems such as poor carrier expansion capability, low luminous efficiency, high operating voltage, and insufficient anti-static capability.

Method used

A periodic multi-quantum-well layer structure is adopted, with each period consisting of a first ternary doped GaN layer, a SiGaN layer, and a second ternary doped GaN layer stacked sequentially. The doping elements are Be, Mg, and O. The lattice quality and carrier expansion are optimized by controlling the doping concentration and growth temperature and pressure.

Benefits of technology

It improves the luminous efficiency of LEDs, reduces the operating voltage, and enhances anti-static capability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116705931B_ABST
    Figure CN116705931B_ABST
Patent Text Reader

Abstract

This invention discloses a light-emitting diode (LED) epitaxial wafer and its fabrication method, relating to the field of semiconductor optoelectronic devices. The LED epitaxial wafer includes a substrate and a nucleation layer, an intrinsic GaN layer, an N-type GaN layer, a multiple quantum well layer, an electron blocking layer, and a P-type GaN layer sequentially disposed on the substrate. The multiple quantum well layer includes a potential well layer and a potential barrier layer. Each potential barrier layer includes a first ternary doped GaN layer, a SiGaN layer, and a second ternary doped GaN layer sequentially stacked. The doping elements of the first ternary doped GaN layer are Be, Mg, and O, and the doping elements of the second ternary doped GaN layer are Be, Mg, and O. The doping concentration of the first ternary doped GaN layer may be the same as or different from that of the second ternary doped GaN layer. Implementing this invention can improve the luminous efficiency and antistatic capability of the LED, and reduce its operating voltage.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of semiconductor optoelectronic devices, and more particularly to a light-emitting diode epitaxial wafer and its fabrication method, and a light-emitting diode. Background Technology

[0002] A typical GaN-based light-emitting diode (LED) epitaxial wafer includes a substrate, and on the substrate, sequentially grown a nucleation layer, an intrinsic GaN layer, an N-type semiconductor layer, a multiple quantum well layer, an electron blocking layer, and a P-type semiconductor layer. The multiple quantum wells are generally a periodic structure formed by InGaN and GaN barrier layers. Due to the high electron mobility, electrons often escape before recombination can occur in the quantum well layers, thus affecting luminous efficiency. Traditional structures also suffer from poor carrier expansion capabilities in the multiple quantum well layers, impacting LED luminous efficiency, causing high operating voltage, and resulting in poor electrostatic discharge (ESD) immunity. Summary of the Invention

[0003] The technical problem to be solved by the present invention is to provide an epitaxial wafer for a light-emitting diode and a method for preparing the same, which can improve the luminous efficiency and anti-static capability of the light-emitting diode and reduce its operating voltage.

[0004] The technical problem that this invention also aims to solve is to provide a light-emitting diode with high luminous efficiency, strong anti-static capability, and low operating voltage.

[0005] To address the aforementioned problems, this invention discloses a light-emitting diode epitaxial wafer, comprising a substrate and a nucleation layer, an intrinsic GaN layer, an N-type GaN layer, a multiple quantum well layer, an electron blocking layer, and a P-type GaN layer sequentially disposed on the substrate; the multiple quantum well layer has a periodic structure with a period number of 2 to 15, and each period includes a potential well layer and a potential barrier layer stacked sequentially; each potential barrier layer includes a first ternary doped GaN layer, a SiGaN layer, and a second ternary doped GaN layer stacked sequentially.

[0006] The first ternary doped GaN layer is doped with Be, Mg and O, and the second ternary doped GaN layer is doped with Be, Mg and O; the doping concentration of the first ternary doped GaN layer may be the same as or different from that of the second ternary doped GaN layer.

[0007] As an improvement to the above technical solution, the Be doping concentration in the first ternary doped GaN layer is 1×10⁻⁶. 15 cm -3 ~1×10 17 cm -3 The doping concentration of O is 1×10⁻⁶. 17 cm -3 ~1×10 19 cm-3 The Mg doping concentration is 1×10⁻⁶. 14 cm -3 ~1×10 16 cm -3 .

[0008] As an improvement to the above technical solution, the Be doping concentration in the second ternary doped GaN layer is 1×10⁻⁶. 15 cm -3 ~1×10 17 cm -3 The doping concentration of O is 1×10⁻⁶. 17 cm -3 ~1×10 19 cm -3 The Mg doping concentration is 1×10⁻⁶. 14 cm -3 ~1×10 16 cm -3 .

[0009] As an improvement to the above technical solution, the Si doping concentration in the SiGaN layer is 1×10⁻⁶. 16 cm -3 ~1×10 17 cm -3 .

[0010] As an improvement to the above technical solution, the thickness of the first ternary doped GaN layer is 1nm to 10nm, the thickness of the SiGaN layer is 1nm to 3nm, and the thickness of the second ternary doped GaN layer is 1nm to 10nm.

[0011] Accordingly, the present invention also discloses a method for preparing a light-emitting diode epitaxial wafer, for preparing the light-emitting diode epitaxial wafer as described above, comprising:

[0012] A substrate is provided on which a nucleation layer, an intrinsic GaN layer, an N-type GaN layer, a multiple quantum well layer, an electron blocking layer, and a P-type GaN layer are sequentially grown. The multiple quantum well layer has a periodic structure with 2 to 15 periods, and each period includes a potential well layer and a potential barrier layer stacked sequentially. Each potential barrier layer includes a first ternary doped GaN layer, a SiGaN layer, and a second ternary doped GaN layer stacked sequentially.

[0013] The first ternary doped GaN layer is doped with Be, Mg and O, and the second ternary doped GaN layer is doped with Be, Mg and O; the doping concentration of the first ternary doped GaN layer may be the same as or different from that of the second ternary doped GaN layer.

[0014] As an improvement to the above technical solution, the growth temperature of the first ternary doped GaN layer is less than the growth temperature of the second ternary doped GaN layer.

[0015] As an improvement to the above technical solution, the growth temperature of the first ternary doped GaN layer is 800℃~850℃, and the growth pressure is 100 torr~500 torr;

[0016] The growth temperature of the second ternary doped GaN layer is 850℃~950℃, and the growth pressure is 100 torr~500 torr.

[0017] As an improvement to the above technical solution, the growth temperature of the SiGaN layer is 850℃~950℃, and the growth pressure is 100 torr~500 torr.

[0018] Accordingly, the present invention also discloses a light-emitting diode, which includes the above-mentioned light-emitting diode epitaxial wafer.

[0019] Implementing this invention has the following beneficial effects:

[0020] In the epitaxial wafer of the light-emitting diode of the present invention, the barrier layer of the multi-quantum-well layer includes a first ternary doped GaN layer, a SiGaN layer, and a second ternary doped GaN layer stacked in one step. The doping elements of the first ternary doped GaN layer and the second ternary doped GaN layer are Be, O, and Mg. Among them, Be, being a small element, can block defects in the potential well layer and improve lattice quality. Furthermore, Be doping can reduce the bulk resistance of GaN material, increase carrier expansion, improve luminous efficiency, reduce operating voltage, and improve antistatic capability. Mg, as a p-type dopant, provides some holes, compensating for the lack of holes in traditional barrier layers, increasing the recombination probability of electrons and holes, and improving luminous efficiency. The introduction of O improves the doping efficiency of Be, which helps reduce the generation of vacant atoms. Moreover, the incorporation of O atoms helps open Mg-H bonds, avoids the formation of complexes, and increases the effective doping concentration of Mg, thereby improving the incorporation efficiency of Mg. In addition, the SiGaN layer can further improve electron expansion, improve the luminous efficiency of the light-emitting diode, reduce the operating voltage, and improve its antistatic capability. Attached Figure Description

[0021] Figure 1 This is a schematic diagram of the structure of a light-emitting diode epitaxial wafer in one embodiment of the present invention;

[0022] Figure 2 This is a schematic diagram of the structure of a multi-quantum well layer in one embodiment of the present invention;

[0023] Figure 3 This is a schematic diagram of the barrier layer structure in one embodiment of the present invention;

[0024] Figure 4 This is a flowchart of a method for preparing an epitaxial wafer for a light-emitting diode according to an embodiment of the present invention. Detailed Implementation

[0025] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be described in further detail below.

[0026] refer to Figures 1-3 This invention discloses a light-emitting diode epitaxial wafer, comprising a substrate 1 and a nucleation layer 2, an intrinsic GaN layer 3, an N-type GaN layer 4, a multiple quantum well layer 5, an electron blocking layer 6, and a P-type GaN layer 7 sequentially disposed on the substrate 1. The multiple quantum well layer 5 has a periodic structure with 2 to 15 periods, and each period includes a potential well layer 51 and a potential barrier layer 51 stacked sequentially.

[0027] Each barrier layer 52 comprises a first ternary doped GaN layer 521, a SiGaN layer 522, and a second ternary doped GaN layer 523, stacked sequentially. The doping elements of both the first ternary doped GaN layer 521 and the second ternary doped GaN layer 523 are Be, Mg, and O. The doping concentrations of the two layers may be the same or different. By introducing a GaN layer co-doped with Be, Mg, and O, firstly, the relatively small amount of Be can block defects in the potential well layer, improving lattice quality; and the doping of Be can reduce the bulk resistance of the GaN material, increase carrier expansion, improve luminous efficiency, reduce operating voltage, and improve antistatic capability. Secondly, Mg, as a p-type dopant, provides some holes, compensating for the lack of holes in traditional barrier layers, increasing the recombination probability of electrons and holes, and improving luminous efficiency. Thirdly, the introduction of O element improves the doping efficiency of Be, which helps to reduce the generation of vacant atoms. Furthermore, the incorporation of O atoms helps to open Mg-H bonds, avoid the formation of complexes, increase the effective doping concentration of Mg, thereby improving the incorporation efficiency of Mg and further improving the luminescence efficiency.

[0028] In the first ternary doped GaN layer 521, the Be doping concentration is 8 × 10⁻⁶. 14 cm -3 ~4×10 17 cm -3 When the Be doping concentration is < 8 × 10 14 cm -3 At this point, it is difficult to effectively reduce the bulk resistance and increase electron expansion. When the Be doping concentration is > 4 × 10⁻⁶, it becomes difficult to effectively reduce the bulk resistance and increase electron expansion. 17 cm -3 At this time, the crystal quality of the first ternary doped GaN layer 521 is poor. For example, the Be doping concentration in the first ternary doped GaN layer 521 is 9 × 10⁻⁶. 14 cm -3 2×1015 cm -3 5×10 15 cm -3 9×10 15 cm -3 4×10 16 cm -3 8×10 16 cm -3 Or 3×10 17 cm -3 However, it is not limited to this. A preferred value is 1×10. 15 cm -3 ~1×10 17 cm -3 .

[0029] The Mg doping concentration in the first ternary doped GaN layer 521 is 9 × 10⁻⁶. 13 cm -3 ~5×10 16 cm -3 When the Mg doping concentration is <9×10 13 cm -3 At this stage, the number of holes provided is relatively small, making it difficult to effectively increase the recombination probability of electrons and holes. However, the doping concentration of Mg is >5×10⁻⁶. 16 cm -3 At that time, the crystal quality of the first ternary doped GaN layer 521 was poor. For example, the Mg doping concentration in the first ternary doped GaN layer 521 was 9.5 × 10⁻⁶. 13 cm -3 3×10 14 cm -3 7×10 14 cm -3 1×10 15 cm -3 5×10 15 cm -3 2×10 16 cm -3 Or 4×10 16 cm -3 However, it is not limited to this. A preferred value is 1×10. 14 cm -3 ~1×10 16 cm -3 .

[0030] The O doping concentration in the first ternary doped GaN layer 521 is 8 × 10⁻⁶. 16 cm -3 ~3×10 19 cm -3 When the O doping concentration is < 8 × 10⁻⁶ 16 cm -3When the oxygen doping concentration is high, there are few vacant oxygen atoms, making it difficult to improve the luminous efficiency of the light-emitting diode; when the O doping concentration is >3×10 19 cm -3 In this process, O not only forms oxygen vacancies replacing nitrogen vacancies, but also replaces the original N in GaN, forming a partially electronic semiconductor and reducing hole generation, which in turn reduces the luminous efficiency of the light-emitting diode. For example, the O doping concentration in the first ternary doped GaN layer 521 is 9 × 10⁻⁶. 16 cm -3 2×10 17 cm -3 8×10 17 cm -3 3×10 18 cm -3 5×10 18 cm -3 9×10 18 cm -3 Or 2×10 19 cm -3 However, it is not limited to this. A preferred value is 1×10. 17 cm -3 ~1×10 19 cm -3 .

[0031] The thickness of the first ternary doped GaN layer 521 is 0.5 nm to 15 nm, exemplarily 1 nm, 3 nm, 7 nm, 10 nm or 14 nm, but not limited thereto. Preferably, it is 1 nm to 10 nm.

[0032] The Si doping concentration in the SiGaN layer 522 is 7 × 10⁻⁶. 15 cm -3 ~4×10 17 cm -3 An example is 8×10. 15 cm -3 2×10 16 cm -3 4×10 16 cm -3 6×10 16 cm -3 8×10 16 cm -3 Or 2×10 17 cm -3 However, it is not limited to this. A preferred value is 1×10. 16 cm -3 ~1×10 17 cm -3The thickness of the SiGaN layer 522 is 1nm to 5nm, with exemplary thicknesses of 1.5nm, 2nm, 2.5nm, 3.5nm, or 4.5nm, but not limited thereto. Preferably, it is 1nm to 3nm.

[0033] In particular, the Be doping concentration in the second ternary doped GaN layer 523 is 5 × 10⁻⁶. 14 cm -3 ~5×10 17 cm -3 When the Be doping concentration is < 5 × 10 14 cm -3 At this point, it is difficult to effectively reduce the bulk resistance and increase electron expansion. When the Be doping concentration is >5×10⁻⁶, it becomes difficult to effectively reduce the bulk resistance and increase electron expansion. 17 cm -3 At this time, the crystal quality of the second ternary doped GaN layer 523 is relatively poor. For example, the Be doping concentration in the second ternary doped GaN layer 523 is 7 × 10⁻⁶. 14 cm -3 9×10 14 cm -3 1×10 15 cm -3 6×10 15 cm -3 9×10 15 cm -3 4×10 16 cm -3 8×10 16 cm -3 Or 4×10 17 cm -3 However, it is not limited to this. A preferred value is 1×10. 15 cm -3 ~1×10 17 cm -3 .

[0034] The Mg doping concentration in the second ternary doped GaN layer 523 is 8 × 10⁻⁶. 13 cm -3 ~8×10 16 cm -3 When the Mg doping concentration is < 8 × 10⁻⁶ 13 cm -3 At this stage, the number of holes provided is relatively small, making it difficult to effectively increase the recombination probability of electrons and holes. However, the doping concentration of Mg is >8×10⁻⁶. 16 cm -3 At this time, the crystal quality of the second ternary doped GaN layer 523 is relatively poor. For example, the Mg doping concentration in the first ternary doped GaN layer 523 is 9.5 × 10⁻⁶. 13 cm -3 3×1014 cm -3 7×10 14 cm -3 1×10 15 cm -3 5×10 15 cm -3 2×10 16 cm -3 4×10 16 cm -3 Or 6×10 16 cm -3 However, it is not limited to this. A preferred value is 1×10. 14 cm -3 ~1×10 16 cm -3 .

[0035] The O doping concentration in the second ternary doped GaN layer 523 is 8 × 10⁻⁶. 16 cm -3 ~3×10 19 cm -3 When the O doping concentration is < 8 × 10⁻⁶ 16 cm -3 When the oxygen doping concentration is high, there are few vacant oxygen atoms, making it difficult to improve the luminous efficiency of the light-emitting diode; when the O doping concentration is >3×10 19 cm -3 In this process, O not only forms oxygen vacancies replacing nitrogen vacancies, but also replaces the original N in GaN, forming a partially electronic semiconductor and reducing hole generation, which in turn reduces the luminous efficiency of the light-emitting diode. For example, the O doping concentration in the second ternary doped GaN layer 523 is 9 × 10⁻⁶. 16 cm -3 2×10 17 cm -3 8×10 17 cm -3 3×10 18 cm -3 5×10 18 cm -3 9×10 18 cm -3 Or 2×10 19 cm -3 However, it is not limited to this. A preferred value is 1×10. 17 cm -3 ~1×10 19 cm -3 .

[0036] The thickness of the second ternary doped GaN layer 523 is 0.5 nm to 15 nm, with exemplary thicknesses of 1 nm, 3 nm, 7 nm, 10 nm, or 14 nm, but not limited thereto. Preferably, it is 1 nm to 10 nm.

[0037] Preferably, in one embodiment of the present invention, the doping concentrations of Be, Mg, and O in the second ternary doped GaN layer 523 are controlled to be greater than the doping concentrations of Be, Mg, and O in the first ternary doped GaN layer 521.

[0038] The potential well layer 51 is an InGaN layer, but is not limited thereto. The thickness of the potential well layer 51 is 3nm to 7nm, and exemplary examples are 3.5nm, 4nm, 5nm, 6nm or 6.5nm, but is not limited thereto.

[0039] The substrate 1 can be a sapphire substrate, a silicon substrate, a SiC substrate, a ZnO substrate, or a GaN substrate, but is not limited to these.

[0040] The nucleation layer 2 can be an AlN layer and / or an AlGaN layer, but is not limited thereto. Preferably, it is an AlN layer with a thickness of 20nm to 100nm, such as 25nm, 30nm, 35nm, 40nm, 50nm, 70nm or 85nm, but is not limited thereto.

[0041] The thickness of the intrinsic GaN layer 3 is 300nm to 800nm, with examples of 350nm, 400nm, 450nm, 500nm, 550nm, 600nm, 700nm or 750nm, but not limited to these.

[0042] The N-type GaN layer 4 is doped with Si, but is not limited to Si. The doping concentration of the N-type GaN layer 4 is 5 × 10⁻⁶. 18 ~1×10 19 cm -3 An example is 6×10 18 cm -3 7×10 18 cm -3 8×10 18 cm -3 Or 9×10 18 cm -3 However, it is not limited to this. The thickness of the N-type GaN layer 4 is 1 μm to 3 μm, with exemplary thicknesses of 1.2 μm, 1.6 μm, 2 μm, 2.4 μm, 2.8 μm or 2.9 μm, but it is not limited to this.

[0043] Among them, electron blocking layer 6 is Al α Ga 1-α N layer (α = 0.3–0.6) or Al β Inγ Ga 1-β-γ N (β = 0.1–0.2, γ = 0.2–0.5), but not limited thereto. Preferably, in one embodiment of the present invention, the electron blocking layer 6 is Al. a Ga 1- a N layer (a = 0.05–0.2) and In b Ga 1-b The structure consists of N layers (b = 0.1–0.5) growing alternately, with a periodicity of 3–20. The electron blocking layer 7 has a thickness of 30 nm–100 nm, exemplarily 35 nm, 40 nm, 60 nm, 80 nm, or 93 nm, but is not limited thereto.

[0044] The doping element in the p-type GaN layer 7 is Mg, but it is not limited to this. The doping concentration of Mg in the p-type GaN layer 7 is 5 × 10⁻⁶. 17 ~1×10 20 cm -3 An example is 6×10 17 cm -3 8×10 17 cm -3 1×10 19 cm -3 4×10 19 cm -3 7×10 19 cm -3 Or 9×10 19 cm -3 However, it is not limited to this. The thickness of the p-type GaN layer 7 is 5nm to 60nm, with examples being 10nm, 24nm, 30nm, 44nm or 58nm, but not limited to this.

[0045] Accordingly, refer to Figure 3 The present invention also discloses a method for preparing a light-emitting diode epitaxial wafer, which includes the following steps:

[0046] S1: Provides a substrate;

[0047] Preferably, in one embodiment of the present invention, the substrate is loaded into the MOCVD reaction chamber and pretreated in an H2 atmosphere for 5 min to 8 min, the treatment temperature is 1000℃ to 1200℃, and the treatment pressure is 200 torr to 600 torr.

[0048] S2: A nucleation layer, an intrinsic GaN layer, an N-type GaN layer, a multiple quantum well layer, an electron blocking layer, and a P-type GaN layer are sequentially grown on the substrate;

[0049] Specifically, step S2 includes:

[0050] S21: Growing a nucleation layer on the substrate;

[0051] Among them, AlGaN layers grown by MOCVD or AlN layers grown by PVD can be used as nucleation layers, but are not limited to these.

[0052] Preferably, in one embodiment of the present invention, an AlGaN layer is grown by MOCVD as a nucleation layer at a growth temperature of 500°C to 700°C and a growth pressure of 200 torr to 400 torr. During growth, NH3 is introduced into the MOCVD reaction chamber as an N source, N2 and H2 are introduced as carrier gases, TMGa is introduced as a Ga source, and TMAl is introduced as an Al source.

[0053] S22: Grow an intrinsic GaN layer on the nucleation layer;

[0054] In one embodiment of the present invention, an intrinsic GaN layer is grown in MOCVD at a growth temperature of 1100°C to 1150°C and a growth pressure of 100 torr to 500 torr. During growth, NH3 is introduced into the MOCVD reaction chamber as an N source, N2 and H2 are introduced as carrier gases, and TMGa is introduced as a Ga source.

[0055] S23: Growing an N-type GaN layer on an intrinsic GaN layer;

[0056] In one embodiment of the present invention, an N-type GaN layer is grown in MOCVD at a growth temperature of 1100℃ to 1150℃ and a growth pressure of 100 torr to 500 torr. During growth, NH3 is introduced into the MOCVD reaction chamber as an N source, N2 and H2 are introduced as carrier gases, TMGa is introduced as a Ga source, and SiH4 is introduced as an N-type doping source.

[0057] S24: Growth of multiple quantum well layers on N-type GaN layers;

[0058] In one embodiment of the present invention, a potential well layer and a potential barrier layer are periodically grown in MOCVD to form a multi-quantum well layer. The growth temperature of the potential well layer is 700°C to 800°C, and the growth pressure is 100 torr to 300 torr. During growth, NH3 is introduced into the MOCVD reaction chamber as an N source, N2 as a carrier gas, TMGa as a Ga source, and TMIn as an In source.

[0059] The preparation method for each barrier layer includes:

[0060] (I) Growth of the first ternary doped GaN layer;

[0061] In one embodiment of the present invention, a first ternary doped GaN layer is grown in MOCVD at a growth temperature of 800°C to 850°C and a growth pressure of 100 torr to 500 torr. During growth, NH3 is introduced as an N source, O2 as an O source, N2 and / or H2 as a carrier gas, TMGa as a Ga source, di-tert-butylberyllium as a Be source, and Cp2Mg as a Mg source in the MOCVD reaction chamber.

[0062] (II) Growing a SiGaN layer on a first ternary doped GaN layer;

[0063] In one embodiment of the present invention, a SiGaN layer is grown in MOCVD at a growth temperature of 850°C to 950°C and a growth pressure of 100 torr to 500 torr. During growth, NH3 is introduced into the MOCVD reaction chamber as an N source, N2 and / or H2 are introduced as carrier gases, TMGa is introduced as a Ga source, and SiH4 is introduced as an N-type doping source.

[0064] (III) A second ternary doped GaN layer is grown on the SiGaN layer;

[0065] In one embodiment of the present invention, a second ternary doped GaN layer is grown in MOCVD at a growth temperature of 850°C to 950°C and a growth pressure of 100 torr to 500 torr. During growth, NH3 is introduced as an N source, O2 as an O source, N2 and / or H2 as a carrier gas, TMGa as a Ga source, di-tert-butylberyllium as a Be source, and Cp2Mg as a Mg source in the MOCVD reaction chamber.

[0066] Preferably, in one embodiment of the present invention, the growth temperature of the second ternary doped GaN layer is controlled to be higher than that of the first ternary doped GaN layer. The lower growth temperature of the first ternary doped GaN layer prevents In desorption from the InGaN well layer. The higher growth temperature of the second ternary doped GaN layer improves its crystal quality, thereby increasing the doping concentrations of Be and Mg.

[0067] S25: Growth of an electron blocking layer on a multi-quantum-well layer;

[0068] Among them, Al can be grown through MOCVD and MBE. α Ga 1-α N layer (α = 0.3–0.6) or Al β In γ Ga 1-β-γ N (β = 0.1–0.2, γ = 0.2–0.5) serves as an electron blocking layer, but is not limited to this.

[0069] Preferably, in one embodiment of the present invention, Al is periodically grown by MOCVD. a Ga 1-a N layer (a = 0.05–0.2) and In b Ga 1-b N layers (b = 0.1–0.5) are formed until an electron blocking layer is obtained.

[0070] Among them, Al a Ga 1-a The growth temperature of the N layer is 900℃~1000℃, and the growth pressure is 100torr~500torr. During growth, NH3 is introduced into the MOCVD reaction chamber as the N source, N2 as the carrier gas, TMGa as the Ga source, and TMAl as the Al source. b Ga 1-b The growth temperature of the N layer is 900℃~1000℃, and the growth pressure is 100 torr~500 torr. During growth, NH3 is introduced into the MOCVD reaction chamber as the N source, N2 as the carrier gas, TMGa as the Ga source, and TMIn as the In source.

[0071] S26: Grow a P-type GaN layer on the electron blocking layer;

[0072] In one embodiment of the present invention, a p-type GaN layer is grown in MOCVD at a growth temperature of 800°C to 1000°C and a growth pressure of 100 torr to 300 torr. During growth, NH3 is introduced into the MOCVD reaction chamber as an N source, N2 and H2 are introduced as carrier gases, TMGa is introduced as a Ga source, and CP2Mg is introduced as a p-type doping source.

[0073] The present invention will be further described below with reference to specific embodiments:

[0074] Example 1

[0075] refer to Figures 1-3 This embodiment provides a light-emitting diode epitaxial wafer, including a substrate 1 and a nucleation layer 2, an intrinsic GaN layer 3, an N-type GaN layer 4, a multiple quantum well layer 5, an electron blocking layer 6, and a P-type GaN layer 7 sequentially disposed on the substrate 1.

[0076] In this design, substrate 1 is a sapphire substrate, nucleation layer 2 is an AlGaN layer with a thickness of 30 nm, intrinsic GaN layer 3 has a thickness of 520 nm, and N-type GaN layer 4 has a thickness of 2 μm and is doped with Si at a doping concentration of 8 × 10⁻⁶. 18 cm -3 .

[0077] The multi-quantum-well layer 5 has a periodic structure with 10 periods, each period consisting of a potential well layer 51 and a barrier layer 52 stacked sequentially. The potential well layer 51 is an InGaN layer with a thickness of 3 nm. Each barrier layer 52 includes a first ternary doped GaN layer 521, a SiGaN layer 522, and a second ternary doped GaN layer 523. The Be doping concentration in the first ternary doped GaN layer 521 is 3 × 10⁻⁶. 17 cm -3 The O doping concentration is 8 × 10⁻⁶. 16 cm -3 The Mg doping concentration is 9.5 × 10⁻⁶. 13 cm -3 Its thickness is 12 nm. The Si doping concentration in the SiGaN layer 522 is 5 × 10⁻⁶. 16 cm -3 Its thickness is 4 nm. The Be doping concentration in the second ternary doped GaN layer 523 is 3 × 10⁻⁶. 17 cm -3 The O doping concentration is 8 × 10⁻⁶. 16 cm -3 The Mg doping concentration is 9.5 × 10⁻⁶. 13 cm -3 Its thickness is 12nm.

[0078] Among them, electron blocking layer 6 has a periodic structure with 10 periods, each period consisting of sequentially stacked Al layers. a Ga 1-a N layers (a = 0.15) and In b Ga 1-b N layers (b = 0.4). A single Al a Ga 1-a The thickness of the N layer is 3nm, and a single In... b Ga 1-b The thickness of the N layer is 3 nm.

[0079] In this layer, the doping element of the p-type GaN layer 8 is Mg, and the doping concentration is 8 × 10⁸. 19 cm -3 The thickness is 50nm.

[0080] The method for fabricating the epitaxial wafer of the light-emitting diode in this embodiment includes the following steps:

[0081] (1) Provide a substrate;

[0082] Preferably, in one embodiment of the present invention, the substrate is loaded into the MOCVD reaction chamber, pretreated in an H2 atmosphere for 8 min, the treatment temperature is 1100°C, and the treatment pressure is 400 torr.

[0083] (2) Growing a nucleation layer on a substrate;

[0084] In this process, an AlGaN layer was grown in MOCVD as a nucleation layer at a growth temperature of 620℃ and a growth pressure of 300 torr. During growth, NH3 was introduced into the MOCVD reaction chamber as the N source, N2 and H2 as the carrier gases, TMGa was introduced as the Ga source, and TMAl was introduced as the Al source.

[0085] (3) Grow an intrinsic GaN layer on the nucleation layer;

[0086] Intrinsic GaN layers were grown in MOCVD at a temperature of 1120℃ and a pressure of 300 torr. During growth, NH3 was introduced into the MOCVD reaction chamber as the N source, N2 and H2 were introduced as the carrier gas, and TMGa was introduced as the Ga source.

[0087] (4) Growing an N-type GaN layer on the intrinsic GaN layer;

[0088] In this process, an N-type GaN layer was grown in MOCVD at a temperature of 1130℃ and a pressure of 300 torr. During growth, NH3 was introduced into the MOCVD reaction chamber as the N source, N2 and H2 as the carrier gas, TMGa was introduced as the Ga source, and SiH4 was introduced as the N-type doping source.

[0089] (5) Growth of multiple quantum well layers on N-type GaN layers;

[0090] In this process, potential well layers and barrier layers are periodically grown in MOCVD to form a multi-quantum well layer. The growth temperature of the potential well layer is 770℃, and the growth pressure is 300 torr. During growth, NH3 is introduced into the MOCVD reaction chamber as the N source, N2 as the carrier gas, TMGa as the Ga source, and TMIn as the In source.

[0091] The preparation method for each barrier layer includes:

[0092] (I) Growth of the first ternary doped GaN layer;

[0093] The first ternary doped GaN layer was grown in MOCVD at a temperature of 850℃ and a pressure of 300 torr. During growth, NH3 was introduced as the N source, O2 as the O source, N2 and / or H2 as the carrier gas, TMGa as the Ga source, di-tert-butylberyllium as the Be source, and Cp2Mg as the Mg source into the MOCVD reaction chamber.

[0094] (II) Growing a SiGaN layer on a first ternary doped GaN layer;

[0095] The SiGaN layer was grown in MOCVD at a temperature of 920℃ and a pressure of 300 torr. During growth, NH3 was introduced into the MOCVD reaction chamber as the N source, N2 and / or H2 as the carrier gas, TMGa as the Ga source, and SiH4 as the N-type doping source.

[0096] (III) A second ternary doped GaN layer is grown on the SiGaN layer;

[0097] The second ternary doped GaN layer was grown in MOCVD at a temperature of 850℃ and a pressure of 300 torr. During growth, NH3 was introduced as the N source, O2 as the O source, N2 and / or H2 as the carrier gas, TMGa as the Ga source, di-tert-butylberyllium as the Be source, and Cp2Mg as the Mg source into the MOCVD reaction chamber.

[0098] (6) Grow an electron blocking layer on a multi-quantum-well layer;

[0099] Among them, Al is grown periodically via MOCVD. a Ga 1-a N layers and In b Ga 1-b N layers, until an electron blocking layer is obtained. Al a Ga 1-a The N-layer was grown at a temperature of 950℃ and a growth pressure of 300 torr. During growth, NH3 was introduced into the MOCVD reaction chamber as the N source, N2 as the carrier gas, TMGa as the Ga source, and TMAl as the Al source. b Ga 1-b The growth temperature of the N layer is 920℃, and the growth pressure is 400 torr. During growth, NH3 is introduced into the MOCVD reaction chamber as the N source, N2 as the carrier gas, TMGa as the Ga source, and TMIn as the In source.

[0100] (7) Grow a P-type GaN layer on the electron blocking layer;

[0101] In this process, a P-type GaN layer was grown in MOCVD at a temperature of 980℃ and a pressure of 200 torr. During growth, NH3 was introduced into the MOCVD reaction chamber as the N source, N2 and H2 as the carrier gas, TMGa was introduced as the Ga source, and Cp2Mg was introduced as the P-type doping source.

[0102] Example 2

[0103] refer to Figures 1-3This embodiment provides a light-emitting diode epitaxial wafer, including a substrate 1 and a nucleation layer 2, an intrinsic GaN layer 3, an N-type GaN layer 4, a multiple quantum well layer 5, an electron blocking layer 6, and a P-type GaN layer 7 sequentially disposed on the substrate 1.

[0104] In this design, substrate 1 is a sapphire substrate, nucleation layer 2 is an AlGaN layer with a thickness of 30 nm, intrinsic GaN layer 3 has a thickness of 520 nm, and N-type GaN layer 4 has a thickness of 2 μm and is doped with Si at a doping concentration of 8 × 10⁻⁶. 18 cm -3 .

[0105] The multi-quantum-well layer 5 has a periodic structure with 10 periods, each period consisting of a potential well layer 51 and a barrier layer 52 stacked sequentially. The potential well layer 51 is an InGaN layer with a thickness of 3 nm. Each barrier layer 52 includes a first ternary doped GaN layer 521, a SiGaN layer 522, and a second ternary doped GaN layer 523. The Be doping concentration in the first ternary doped GaN layer 521 is 8 × 10⁻⁶. 16 cm -3 The doping concentration of O is 3 × 10⁻⁶. 17 cm -3 The Mg doping concentration is 9 × 10⁻⁶. 15 cm -3 Its thickness is 3 nm. The Si doping concentration in the SiGaN layer 522 is 5 × 10⁻⁶. 16 cm -3 Its thickness is 2 nm. The Be doping concentration in the second ternary doped GaN layer 523 is 8 × 10⁻⁶. 16 cm -3 The O doping concentration is 3 × 10⁻⁶. 17 cm -3 The Mg doping concentration is 9 × 10⁻⁶. 15 cm -3 Its thickness is 3nm.

[0106] Among them, electron blocking layer 6 has a periodic structure with 10 periods, each period consisting of sequentially stacked Al layers. a Ga 1-a N layers (a = 0.15) and In b Ga 1-b N layers (b = 0.4). A single Al a Ga 1-a The thickness of the N layer is 3nm, and a single In... b Ga 1-b The thickness of the N layer is 3 nm.

[0107] In this layer, the doping element of the p-type GaN layer 8 is Mg, and the doping concentration is 8 × 10⁸. 19cm -3 The thickness is 50nm.

[0108] The method for fabricating the epitaxial wafer of the light-emitting diode in this embodiment includes the following steps:

[0109] (1) Provide a substrate;

[0110] Preferably, in one embodiment of the present invention, the substrate is loaded into the MOCVD reaction chamber, pretreated in an H2 atmosphere for 8 min, the treatment temperature is 1100°C, and the treatment pressure is 400 torr.

[0111] (2) Growing a nucleation layer on a substrate;

[0112] In this process, an AlGaN layer was grown in MOCVD as a nucleation layer at a growth temperature of 620℃ and a growth pressure of 300 torr. During growth, NH3 was introduced into the MOCVD reaction chamber as the N source, N2 and H2 as the carrier gases, TMGa was introduced as the Ga source, and TMAl was introduced as the Al source.

[0113] (3) Grow an intrinsic GaN layer on the nucleation layer;

[0114] Intrinsic GaN layers were grown in MOCVD at a temperature of 1120℃ and a pressure of 300 torr. During growth, NH3 was introduced into the MOCVD reaction chamber as the N source, N2 and H2 were introduced as the carrier gas, and TMGa was introduced as the Ga source.

[0115] (4) Growing an N-type GaN layer on the intrinsic GaN layer;

[0116] In this process, an N-type GaN layer was grown in MOCVD at a temperature of 1130℃ and a pressure of 300 torr. During growth, NH3 was introduced into the MOCVD reaction chamber as the N source, N2 and H2 as the carrier gas, TMGa was introduced as the Ga source, and SiH4 was introduced as the N-type doping source.

[0117] (5) Growth of multiple quantum well layers on N-type GaN layers;

[0118] In this process, potential well layers and barrier layers are periodically grown in MOCVD to form a multi-quantum well layer. The growth temperature of the potential well layer is 770℃, and the growth pressure is 300 torr. During growth, NH3 is introduced into the MOCVD reaction chamber as the N source, N2 as the carrier gas, TMGa as the Ga source, and TMIn as the In source.

[0119] The preparation method for each barrier layer includes:

[0120] (I) Growth of the first ternary doped GaN layer;

[0121] The first ternary doped GaN layer was grown in MOCVD at a temperature of 850℃ and a pressure of 300 torr. During growth, NH3 was introduced as the N source, O2 as the O source, N2 and / or H2 as the carrier gas, TMGa as the Ga source, di-tert-butylberyllium as the Be source, and Cp2Mg as the Mg source into the MOCVD reaction chamber.

[0122] (II) Growing a SiGaN layer on a first ternary doped GaN layer;

[0123] The SiGaN layer was grown in MOCVD at a temperature of 920℃ and a pressure of 300 torr. During growth, NH3 was introduced into the MOCVD reaction chamber as the N source, N2 and / or H2 as the carrier gas, TMGa as the Ga source, and SiH4 as the N-type doping source.

[0124] (III) A second ternary doped GaN layer is grown on the SiGaN layer;

[0125] The second ternary doped GaN layer was grown in MOCVD at a temperature of 850℃ and a pressure of 300 torr. During growth, NH3 was introduced as the N source, O2 as the O source, N2 and / or H2 as the carrier gas, TMGa as the Ga source, di-tert-butylberyllium as the Be source, and Cp2Mg as the Mg source into the MOCVD reaction chamber.

[0126] (6) Grow an electron blocking layer on a multi-quantum-well layer;

[0127] Among them, Al is grown periodically via MOCVD. a Ga 1-a N layers and In b Ga 1-b N layers, until an electron blocking layer is obtained. Al a Ga 1-a The N-layer was grown at a temperature of 950℃ and a growth pressure of 300 torr. During growth, NH3 was introduced into the MOCVD reaction chamber as the N source, N2 as the carrier gas, TMGa as the Ga source, and TMAl as the Al source. b Ga 1-b The growth temperature of the N layer is 920℃, and the growth pressure is 400 torr. During growth, NH3 is introduced into the MOCVD reaction chamber as the N source, N2 as the carrier gas, TMGa as the Ga source, and TMIn as the In source.

[0128] (7) Grow a P-type GaN layer on the electron blocking layer;

[0129] In this process, a P-type GaN layer was grown in MOCVD at a temperature of 980℃ and a pressure of 200 torr. During growth, NH3 was introduced into the MOCVD reaction chamber as the N source, N2 and H2 as the carrier gas, TMGa was introduced as the Ga source, and Cp2Mg was introduced as the P-type doping source.

[0130] Example 3

[0131] refer to Figures 1-3 This embodiment provides a light-emitting diode epitaxial wafer, including a substrate 1 and a nucleation layer 2, an intrinsic GaN layer 3, an N-type GaN layer 4, a multiple quantum well layer 5, an electron blocking layer 6, and a P-type GaN layer 7 sequentially disposed on the substrate 1.

[0132] In this design, substrate 1 is a sapphire substrate, nucleation layer 2 is an AlGaN layer with a thickness of 30 nm, intrinsic GaN layer 3 has a thickness of 520 nm, and N-type GaN layer 4 has a thickness of 2 μm and is doped with Si at a doping concentration of 8 × 10⁻⁶. 18 cm -3 .

[0133] The multi-quantum-well layer 5 has a periodic structure with 10 periods, each period consisting of a potential well layer 51 and a barrier layer 52 stacked sequentially. The potential well layer 51 is an InGaN layer with a thickness of 3 nm. Each barrier layer 52 includes a first ternary doped GaN layer 521, a SiGaN layer 522, and a second ternary doped GaN layer 523. The Be doping concentration in the first ternary doped GaN layer 521 is 8 × 10⁻⁶. 16 cm -3 The O doping concentration is 3 × 10⁻⁶. 17 cm -3 The Mg doping concentration is 9 × 10⁻⁶. 15 cm -3 Its thickness is 3 nm. The Si doping concentration in the SiGaN layer 522 is 5 × 10⁻⁶. 16 cm -3 Its thickness is 2 nm. The Be doping concentration in the second ternary doped GaN layer 523 is 9 × 10⁻⁶. 16 cm -3 The O doping concentration is 4 × 10⁻⁶. 17 cm -3 The Mg doping concentration is 9.5 × 10⁻⁶. 15 cm -3 Its thickness is 3nm.

[0134] Among them, electron blocking layer 6 has a periodic structure with 10 periods, each period consisting of sequentially stacked Al layers. a Ga 1-a N layers (a = 0.15) and In bGa 1-b N layers (b = 0.4). A single Al a Ga 1-a The thickness of the N layer is 3nm, and a single In... b Ga 1-b The thickness of the N layer is 3 nm.

[0135] In this layer, the doping element of the p-type GaN layer 8 is Mg, and the doping concentration is 8 × 10⁸. 19 cm -3 The thickness is 50nm.

[0136] The method for fabricating the epitaxial wafer of the light-emitting diode in this embodiment includes the following steps:

[0137] (1) Provide a substrate;

[0138] Preferably, in one embodiment of the present invention, the substrate is loaded into the MOCVD reaction chamber, pretreated in an H2 atmosphere for 8 min, the treatment temperature is 1100°C, and the treatment pressure is 400 torr.

[0139] (2) Growing a nucleation layer on a substrate;

[0140] In this process, an AlGaN layer was grown in MOCVD as a nucleation layer at a growth temperature of 620℃ and a growth pressure of 300 torr. During growth, NH3 was introduced into the MOCVD reaction chamber as the N source, N2 and H2 as the carrier gases, TMGa was introduced as the Ga source, and TMAl was introduced as the Al source.

[0141] (3) Grow an intrinsic GaN layer on the nucleation layer;

[0142] Intrinsic GaN layers were grown in MOCVD at a temperature of 1120℃ and a pressure of 300 torr. During growth, NH3 was introduced into the MOCVD reaction chamber as the N source, N2 and H2 were introduced as the carrier gas, and TMGa was introduced as the Ga source.

[0143] (4) Growing an N-type GaN layer on the intrinsic GaN layer;

[0144] In this process, an N-type GaN layer was grown in MOCVD at a temperature of 1130℃ and a pressure of 300 torr. During growth, NH3 was introduced into the MOCVD reaction chamber as the N source, N2 and H2 as the carrier gas, TMGa was introduced as the Ga source, and SiH4 was introduced as the N-type doping source.

[0145] (5) Growth of multiple quantum well layers on N-type GaN layers;

[0146] In this process, potential well layers and barrier layers are periodically grown in MOCVD to form a multi-quantum well layer. The growth temperature of the potential well layer is 770℃, and the growth pressure is 300 torr. During growth, NH3 is introduced into the MOCVD reaction chamber as the N source, N2 as the carrier gas, TMGa as the Ga source, and TMIn as the In source.

[0147] The preparation method for each barrier layer includes:

[0148] (I) Growth of the first ternary doped GaN layer;

[0149] The first ternary doped GaN layer was grown in MOCVD at a temperature of 850℃ and a pressure of 300 torr. During growth, NH3 was introduced as the N source, O2 as the O source, N2 and / or H2 as the carrier gas, TMGa as the Ga source, di-tert-butylberyllium as the Be source, and Cp2Mg as the Mg source into the MOCVD reaction chamber.

[0150] (II) Growing a SiGaN layer on a first ternary doped GaN layer;

[0151] The SiGaN layer was grown in MOCVD at a temperature of 920℃ and a pressure of 300 torr. During growth, NH3 was introduced into the MOCVD reaction chamber as the N source, N2 and / or H2 as the carrier gas, TMGa as the Ga source, and SiH4 as the N-type doping source.

[0152] (III) A second ternary doped GaN layer is grown on the SiGaN layer;

[0153] The second ternary doped GaN layer was grown in MOCVD at a temperature of 850℃ and a pressure of 300 torr. During growth, NH3 was introduced as the N source, O2 as the O source, N2 and / or H2 as the carrier gas, TMGa as the Ga source, di-tert-butylberyllium as the Be source, and Cp2Mg as the Mg source into the MOCVD reaction chamber.

[0154] (6) Grow an electron blocking layer on a multi-quantum-well layer;

[0155] Among them, Al is grown periodically via MOCVD. a Ga 1-a N layers and In b Ga 1-b N layers, until an electron blocking layer is obtained. Al a Ga 1-aThe N-layer was grown at a temperature of 950℃ and a growth pressure of 300 torr. During growth, NH3 was introduced into the MOCVD reaction chamber as the N source, N2 as the carrier gas, TMGa as the Ga source, and TMAl as the Al source. b Ga 1-b The growth temperature of the N layer is 920℃, and the growth pressure is 400 torr. During growth, NH3 is introduced into the MOCVD reaction chamber as the N source, N2 as the carrier gas, TMGa as the Ga source, and TMIn as the In source.

[0156] (7) Grow a P-type GaN layer on the electron blocking layer;

[0157] In this process, a P-type GaN layer was grown in MOCVD at a temperature of 980℃ and a pressure of 200 torr. During growth, NH3 was introduced into the MOCVD reaction chamber as the N source, N2 and H2 as the carrier gas, TMGa was introduced as the Ga source, and Cp2Mg was introduced as the P-type doping source.

[0158] Example 4

[0159] refer to Figures 1-3 This embodiment provides a light-emitting diode epitaxial wafer, including a substrate 1 and a nucleation layer 2, an intrinsic GaN layer 3, an N-type GaN layer 4, a multiple quantum well layer 5, an electron blocking layer 6, and a P-type GaN layer 7 sequentially disposed on the substrate 1.

[0160] In this design, substrate 1 is a sapphire substrate, nucleation layer 2 is an AlGaN layer with a thickness of 30 nm, intrinsic GaN layer 3 has a thickness of 520 nm, and N-type GaN layer 4 has a thickness of 2 μm and is doped with Si at a doping concentration of 8 × 10⁻⁶. 18 cm -3 .

[0161] The multi-quantum-well layer 5 has a periodic structure with 10 periods, each period consisting of a potential well layer 51 and a barrier layer 52 stacked sequentially. The potential well layer 51 is an InGaN layer with a thickness of 3 nm. Each barrier layer 52 includes a first ternary doped GaN layer 521, a SiGaN layer 522, and a second ternary doped GaN layer 523. The Be doping concentration in the first ternary doped GaN layer 521 is 8 × 10⁻⁶. 16 cm -3 The O doping concentration is 3 × 10⁻⁶. 17 cm -3 The Mg doping concentration is 9 × 10⁻⁶. 15 cm -3 Its thickness is 3 nm. The Si doping concentration in the SiGaN layer 522 is 5 × 10⁻⁶. 16 cm -3Its thickness is 2 nm. The Be doping concentration in the second ternary doped GaN layer 523 is 9 × 10⁻⁶. 16 cm -3 The O doping concentration is 4 × 10⁻⁶. 17 cm -3 The Mg doping concentration is 9.5 × 10⁻⁶. 15 cm -3 Its thickness is 3nm.

[0162] Among them, electron blocking layer 6 has a periodic structure with 10 periods, each period consisting of sequentially stacked Al layers. a Ga 1-a N layers (a = 0.15) and In b Ga 1-b N layers (b = 0.4). A single Al a Ga 1-a The thickness of the N layer is 3nm, and a single In... b Ga 1-b The thickness of the N layer is 3 nm.

[0163] In this layer, the doping element of the p-type GaN layer 8 is Mg, and the doping concentration is 8 × 10⁸. 19 cm -3 The thickness is 50nm.

[0164] The method for fabricating the epitaxial wafer of the light-emitting diode in this embodiment includes the following steps:

[0165] (1) Provide a substrate;

[0166] Preferably, in one embodiment of the present invention, the substrate is loaded into the MOCVD reaction chamber, pretreated in an H2 atmosphere for 8 min, the treatment temperature is 1100°C, and the treatment pressure is 400 torr.

[0167] (2) Growing a nucleation layer on a substrate;

[0168] In this process, an AlGaN layer was grown in MOCVD as a nucleation layer at a growth temperature of 620℃ and a growth pressure of 300 torr. During growth, NH3 was introduced into the MOCVD reaction chamber as the N source, N2 and H2 as the carrier gases, TMGa was introduced as the Ga source, and TMAl was introduced as the Al source.

[0169] (3) Grow an intrinsic GaN layer on the nucleation layer;

[0170] Intrinsic GaN layers were grown in MOCVD at a temperature of 1120℃ and a pressure of 300 torr. During growth, NH3 was introduced into the MOCVD reaction chamber as the N source, N2 and H2 were introduced as the carrier gas, and TMGa was introduced as the Ga source.

[0171] (4) Growing an N-type GaN layer on the intrinsic GaN layer;

[0172] In this process, an N-type GaN layer was grown in MOCVD at a temperature of 1130℃ and a pressure of 300 torr. During growth, NH3 was introduced into the MOCVD reaction chamber as the N source, N2 and H2 as the carrier gas, TMGa was introduced as the Ga source, and SiH4 was introduced as the N-type doping source.

[0173] (5) Growth of multiple quantum well layers on N-type GaN layers;

[0174] In this process, potential well layers and barrier layers are periodically grown in MOCVD to form a multi-quantum well layer. The growth temperature of the potential well layer is 770℃, and the growth pressure is 300 torr. During growth, NH3 is introduced into the MOCVD reaction chamber as the N source, N2 as the carrier gas, TMGa as the Ga source, and TMIn as the In source.

[0175] The preparation method for each barrier layer includes:

[0176] (I) Growth of the first ternary doped GaN layer;

[0177] The first ternary doped GaN layer was grown in MOCVD at a temperature of 820℃ and a pressure of 300 torr. During growth, NH3 was introduced as the N source, O2 as the O source, N2 and / or H2 as the carrier gas, TMGa as the Ga source, di-tert-butylberyllium as the Be source, and Cp2Mg as the Mg source into the MOCVD reaction chamber.

[0178] (II) Growing a SiGaN layer on a first ternary doped GaN layer;

[0179] The SiGaN layer was grown in MOCVD at a temperature of 920℃ and a pressure of 300 torr. During growth, NH3 was introduced into the MOCVD reaction chamber as the N source, N2 and / or H2 as the carrier gas, TMGa as the Ga source, and SiH4 as the N-type doping source.

[0180] (III) A second ternary doped GaN layer is grown on the SiGaN layer;

[0181] In this process, a second ternary doped GaN layer was grown in MOCVD at a growth temperature of 910℃ and a growth pressure of 300 torr. During growth, NH3 was introduced as the N source, O2 as the O source, N2 and / or H2 as the carrier gas, TMGa as the Ga source, di-tert-butylberyllium as the Be source, and Cp2Mg as the Mg source in the MOCVD reaction chamber.

[0182] (6) Grow an electron blocking layer on a multi-quantum-well layer;

[0183] Among them, Al is grown periodically via MOCVD. a Ga 1-a N layers and In b Ga 1-b N layers, until an electron blocking layer is obtained. Al a Ga 1-a The N-layer was grown at a temperature of 950℃ and a growth pressure of 300 torr. During growth, NH3 was introduced into the MOCVD reaction chamber as the N source, N2 as the carrier gas, TMGa as the Ga source, and TMAl as the Al source. b Ga 1-b The growth temperature of the N layer is 920℃, and the growth pressure is 400 torr. During growth, NH3 is introduced into the MOCVD reaction chamber as the N source, N2 as the carrier gas, TMGa as the Ga source, and TMIn as the In source.

[0184] (7) Grow a P-type GaN layer on the electron blocking layer;

[0185] In this process, a P-type GaN layer was grown in MOCVD at a temperature of 980℃ and a pressure of 200 torr. During growth, NH3 was introduced into the MOCVD reaction chamber as the N source, N2 and H2 as the carrier gas, TMGa was introduced as the Ga source, and Cp2Mg was introduced as the P-type doping source.

[0186] Comparative Example 1

[0187] This comparative example provides a light-emitting diode epitaxial wafer, which differs from Example 1 in that the barrier layer is a GaN layer with a thickness of 10 nm, a growth temperature of 870 °C, and a growth pressure of 300 torr.

[0188] Comparative Example 2

[0189] This comparative example provides a light-emitting diode epitaxial wafer, which differs from Example 1 in that the barrier layer does not include a first ternary doped GaN layer, and correspondingly, the preparation method does not include the step of preparing this layer. All other aspects are the same as in Example 1.

[0190] Comparative Example 3

[0191] This comparative example provides a light-emitting diode epitaxial wafer, which differs from Example 1 in that the barrier layer does not include a second ternary doped GaN layer, and correspondingly, the preparation method does not include the step of preparing this layer. All other aspects are the same as in Example 1.

[0192] Comparative Example 4

[0193] This comparative example provides a light-emitting diode epitaxial wafer, which differs from Example 1 in that the barrier layer does not include a SiGaN layer, and correspondingly, the preparation method does not include the step of preparing this layer; otherwise, it is the same as Example 1.

[0194] Comparative Example 5

[0195] This comparative example provides a light-emitting diode epitaxial wafer, which differs from Example 1 in that the barrier layer does not include a first ternary doped GaN layer and a second ternary doped GaN layer. Correspondingly, the preparation method does not include the step of preparing these two layers. All other aspects are the same as in Example 1.

[0196] The epitaxial wafers of the light-emitting diodes obtained in Examples 1 to 4 and Comparative Examples 1 to 5 were tested. The specific test methods are as follows:

[0197] (1) The epitaxial wafer was fabricated into a chip with a vertical structure of 5mil×7mil, and its luminous brightness was tested at a current of 120mA.

[0198] (2) The epitaxial wafer was fabricated into a chip with a vertical structure of 5mil×7mil, and its working voltage was measured using a multimeter.

[0199] (3) Antistatic Performance Test: The antistatic performance of the chip was tested using an electrostatic meter under the HBM (Human Body Discharge Model) model. The percentage of the chip that could withstand 8000V reverse static electricity was tested. The specific results are as follows:

[0200] Luminous intensity / mW Operating voltage / V Antistatic properties / % Example 1 198.1 3.16 97.8 Example 2 200.5 3.12 98.5 Example 3 201.3 3.09 98.7 Example 4 202.1 3.05 99.3 Comparative Example 1 192.1 3.22 95.6 Comparative Example 2 193.5 3.21 96.1 Comparative Example 3 193.1 3.18 96.3 Comparative Example 4 193.4 3.25 94.3 Comparative Example 5 190.3 3.15 95.8

[0201] As can be seen from the table, when the barrier layer in the traditional light-emitting diode structure (Comparative Example 1) is replaced with the barrier layer structure of the present invention, the luminous brightness, antistatic capability, and operating voltage of the light-emitting diode epitaxial wafer are significantly improved.

[0202] Furthermore, a comparison between Example 1 and Comparative Examples 2 to 5 shows that when the structure of the barrier layer in this invention is changed, it is difficult to effectively improve brightness, antistatic capability, and reduce operating voltage.

[0203] The above description is a preferred embodiment of the invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made without departing from the principle of the invention, and these improvements and modifications are also considered to be within the scope of protection of the invention.

Claims

1. A light-emitting diode epitaxial wafer, comprising a substrate and a nucleation layer, an intrinsic GaN layer, an N-type GaN layer, a multiple quantum well layer, an electron blocking layer, and a P-type GaN layer sequentially disposed on the substrate; wherein the multiple quantum well layer has a periodic structure with a period number of 2 to 15, and each period includes a potential well layer and a potential barrier layer stacked sequentially; characterized in that, Each barrier layer comprises a first ternary doped GaN layer, a SiGaN layer, and a second ternary doped GaN layer stacked sequentially. The first ternary doped GaN layer is doped with Be, Mg and O, and the second ternary doped GaN layer is doped with Be, Mg and O; the doping concentration of the first ternary doped GaN layer may be the same as or different from that of the second ternary doped GaN layer.

2. The light-emitting diode epitaxial wafer as described in claim 1, characterized in that, The Be doping concentration in the first ternary doped GaN layer is 1×10⁻⁶. 15 cm -3 ~1×10 17 cm -3 The doping concentration of O is 1×10⁻⁶. 17 cm -3 ~1×10 19 cm -3 The Mg doping concentration is 1×10⁻⁶. 14 cm -3 ~1×10 16 cm -3 .

3. The light-emitting diode epitaxial wafer as described in claim 1, characterized in that, The Be doping concentration in the second ternary doped GaN layer is 1×10⁻⁶. 15 cm -3 ~1×10 17 cm -3 The doping concentration of O is 1×10⁻⁶. 17 cm -3 ~1×10 19 cm -3 The Mg doping concentration is 1×10⁻⁶. 14 cm -3 ~1×10 16 cm -3 .

4. The light-emitting diode epitaxial wafer as described in claim 1, characterized in that, The Si doping concentration in the SiGaN layer is 1×10⁻⁶. 16 cm -3 ~1×10 17 cm -3 .

5. The light-emitting diode epitaxial wafer as described in any one of claims 1 to 4, characterized in that, The thickness of the first ternary doped GaN layer is 1 nm to 10 nm, the thickness of the SiGaN layer is 1 nm to 3 nm, and the thickness of the second ternary doped GaN layer is 1 nm to 10 nm.

6. A method for preparing a light-emitting diode epitaxial wafer, used to prepare a light-emitting diode epitaxial wafer as described in any one of claims 1 to 5, characterized in that, include: A substrate is provided on which a nucleation layer, an intrinsic GaN layer, an N-type GaN layer, a multiple quantum well layer, an electron blocking layer, and a P-type GaN layer are sequentially grown. The multiple quantum well layer has a periodic structure with 2 to 15 periods, and each period includes a potential well layer and a potential barrier layer stacked sequentially. Each potential barrier layer includes a first ternary doped GaN layer, a SiGaN layer, and a second ternary doped GaN layer stacked sequentially. The first ternary doped GaN layer is doped with Be, Mg and O, and the second ternary doped GaN layer is doped with Be, Mg and O; the doping concentration of the first ternary doped GaN layer may be the same as or different from that of the second ternary doped GaN layer.

7. The method for fabricating a light-emitting diode epitaxial wafer as described in claim 6, characterized in that, The growth temperature of the first ternary doped GaN layer is less than the growth temperature of the second ternary doped GaN layer.

8. The method for fabricating a light-emitting diode epitaxial wafer as described in claim 6, characterized in that, The growth temperature of the first ternary doped GaN layer is 800℃~850℃, and the growth pressure is 100 torr~500 torr; The growth temperature of the second ternary doped GaN layer is 850℃~950℃, and the growth pressure is 100 torr~500 torr.

9. The method for fabricating a light-emitting diode epitaxial wafer as described in claim 6, characterized in that, The SiGaN layer is grown at a temperature of 850℃ to 950℃ and a growth pressure of 100 torr to 500 torr.

10. A light-emitting diode, characterized in that, Includes the light-emitting diode epitaxial wafer as described in any one of claims 1 to 5.

Citation Information

Patent Citations

  • LED (Light Emitting Diode) surface patch type encapsulating structure based on silicon base plate and encapsulating method thereof

    CN101997074A

  • Nitride semiconductor element and its fabrication process

    JP2006313845A