An organic field effect transistor, a preparation method and application thereof
By using polystyrene and poly[2,6′]-4,8-di(5-ethylhexylthiophene)benzo[1,2-b;3,3-b]dithiophene]{3-fluoro-2[(2-ethylhexyl)carbonyl]thiophene[3,4-b]thiophenediyl} blend film and pentaphenyl film layer in organic field-effect transistors, the problem of low photon absorption efficiency is solved, and a stable combination of memory and photosynaptic functions is achieved, supporting the application of neuromorphic computing systems.
Patent Information
- Application Number
- CN202310781543.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-29
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-06-29
AI Technical Summary
Existing organic field-effect transistors based on polymers and single semiconductor layers have low photon absorption efficiency, making it difficult to simultaneously realize the functions of memory and photosynaptic transistors, thus limiting the stable realization of neuromorphic computing systems.
Organic field-effect transistors were fabricated using a blend of polystyrene and poly[2,6′]-4,8-di(5-ethylhexylthiophene)benzo[1,2-b;3,3-b]dithiophene]{3-fluoro-2[(2-ethylhexyl)carbonyl]thiophene[3,4-b]thiophenediyl} as the functional layer, combined with a pentaphenyl film layer, via a one-step solution spin-coating method.
It achieves stable storage window and photosynaptic function under photoelectric operation, reduces operating voltage and power consumption, and supports the construction of neuromorphic computing systems.
Smart Images

Figure CN116709790B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of organic electronics and information technology, specifically relating to an organic field-effect transistor, its fabrication method, and its application. Background Technology
[0002] Optical memory uses photoresponsive semiconductors, such as pentacene, as the active layer, and performs erase and write operations through optical manipulation. Optical manipulation plays an auxiliary role in the write / erase process, primarily contributing by increasing the storage window, reducing operating voltage, and lowering power consumption. When the optical memory is exposed to light, a large number of photogenerated carriers are generated in the photosensitive charge trapping layer or organic semiconductor layer. During the write operation, these carriers are trapped in the underlying charge trapping layer under the influence of the gate electric field, creating a larger storage window. During the erase operation, the photogenerated carriers recombine with the stored carrier charges, completing the erase operation. This type of optical memory has many advantages, such as a larger storage window, longer sustaining time, and faster read / write / erase speeds. These transistors can also simulate artificial synapses through optical manipulation and are applied to functions such as photosynaptic devices, and are called photosynaptic transistors. Their operating principle is based on the lowest unoccupied molecular orbital and highest occupied molecular orbital energy levels between the matched semiconductor and the charge storage layer. Photogenerated electrons or holes in the organic semiconductor layer are transferred to the dielectric layer through band bending.
[0003] Furthermore, organic field-effect transistors (OFETs) that simultaneously function as memory and photosynaptic transistors hold immense potential for building neuromorphic computing systems. However, photoelectric writing operations and stable photosynaptic simulations require certain conditions, such as sufficient photon energy and high photon absorption efficiency. OFETs based on polymers and single semiconductor layers have low photon absorption efficiency, making it difficult to simultaneously achieve both functions. Ensuring the stable implementation of both functions is a key research focus in establishing neuromorphic computing systems. Summary of the Invention
[0004] To address the shortcomings of existing technologies, this invention provides an organic field-effect transistor and its fabrication method, which improves the storage operation voltage based on PS transistors and expands the functionality of photoelectric synaptic transistors on the basis of memory functions, showing great application potential in the field of neuromorphic optoelectronic computing.
[0005] When the organic field-effect transistor provided by this invention is applied in the optoelectronic field, it can simultaneously realize the functions of memory and photosynaptic transistor, and has great application potential in building neuromorphic computing systems.
[0006] To address the shortcomings of existing technologies, the technical solution provided by this invention is as follows:
[0007] An organic field-effect transistor, comprising,
[0008] Gate layer;
[0009] The gate insulating layer located on the surface of the gate layer;
[0010] A functional layer located on the surface of the gate insulating layer; the functional layer is a blend film of polystyrene and poly[2,6′]-4,8-di(5-ethylhexylthiophene)benzo[1,2-b;3,3-b]dithiophene]{3-fluoro-2[(2-ethylhexyl)carbonyl]thiophene[3,4-b]thiophenediyl};
[0011] An organic semiconductor layer located on the surface of the functional layer;
[0012] The source electrode and drain electrode are located on the surface of the organic semiconductor layer.
[0013] Preferably, the thickness of the functional layer is 30-40 nm.
[0014] Preferably, the functional layer is prepared by coating and drying a mixed solution of poly[2,6′]-4,8-di(5-ethylhexylthiophene)benzo[1,2-b;3,3-b]dithiophene]{3-fluoro-2[(2-ethylhexyl)carbonyl]thiophene[3,4-b]thiophenediyl} and polystyrene on the surface of the gate insulating layer in one step.
[0015] Preferably, in the mixed solution of poly[2,6′]-4,8-bis(5-ethylhexylthiophene)benzo[1,2-b;3,3-b]dithiophene]{3-fluoro-2[(2-ethylhexyl)carbonyl]thiophene[3,4-b]thiophenediyl} and polystyrene, the solvent is chlorobenzene.
[0016] Preferably, the mixed solution of poly[2,6′]-4,8-di(5-ethylhexylthiophene)benzo[1,2-b; 3,3-b]dithiophene]{3-fluoro-2[(2-ethylhexyl)carbonyl]thiophene[3,4-b]thiophenediyl} and polystyrene is prepared by mixing a chlorobenzene solution of poly[2,6′]-4,8-di(5-ethylhexylthiophene)benzo[1,2-b; 3,3-b]dithiophene]{3-fluoro-2[(2-ethylhexyl)carbonyl]thiophene[3,4-b]thiophenediyl} with a concentration of 10 mol / ml and a chlorobenzene solution of polystyrene with a concentration of 10 mg / ml in a volume ratio of (1-2):(1-2).
[0017] Preferably, the molecular weight of the poly[2,6′]-4,8-di(5-ethylhexylthiophene)benzo[1,2-b;3,3-b]dithiophene]{3-fluoro-2[(2-ethylhexyl)carbonyl]thiophene[3,4-b]thiophenediyl} is 70,000; and the molecular weight of the polystyrene is 280,000.
[0018] Preferably, the organic semiconductor layer is a pentacene film layer.
[0019] The aforementioned method for fabricating organic field-effect transistors includes,
[0020] A gate insulating layer is formed on the surface of the gate layer;
[0021] A mixed solution of poly[2,6′]-4,8-di(5-ethylhexylthiophene)benzo[1,2-b;3,3-b]dithiophene]{3-fluoro-2[(2-ethylhexyl)carbonyl]thiophene[3,4-b]thiophenediyl} and polystyrene is coated onto the surface of the gate insulating layer in one step and dried to form a functional layer on the surface of the gate insulating layer.
[0022] An organic semiconductor layer is formed on the surface of the functional layer;
[0023] Source and drain electrodes are fabricated in an organic semiconductor layer to form an organic field-effect transistor.
[0024] Preferably, a mixed solution of poly[2,6′]-4,8-di(5-ethylhexylthiophene)benzo[1,2-b;3,3-b]dithiophene]{3-fluoro-2[(2-ethylhexyl)carbonyl]thiophene[3,4-b]thiophenediyl} and polystyrene is spin-coated onto the surface of the gate insulating layer in one step and dried to form a functional layer on the surface of the gate insulating layer;
[0025] Spin coating was performed at a speed of 1500 rpm for 30 seconds; drying temperature was 110℃ and drying time was 30 minutes.
[0026] The aforementioned organic field-effect transistors have applications in the optoelectronic field.
[0027] The beneficial effects of this invention are:
[0028] The functional layer adopted in this invention is subjected to a gate bias of 20V and 5mW / cm². 2 With the synergistic effect of white light, the device can obtain a storage window of nearly 20V in 1 second. In the sustain test, it can achieve an effective information storage time of 10,000 seconds, and there is no significant degradation of source-drain current switching ratio after 90 write / erase cycles, which greatly reduces the power consumption problem of existing technologies.
[0029] The organic field-effect transistor functional layer provided by this invention is prepared by a one-step solution spin coating method, which is simple, fast, and can be mass-produced.
[0030] Based on the memory function of organic field-effect crystals based on single-layer PS, this invention further uses photoelectric pulse stimulation to simulate the functions of photoelectric artificial synapses, such as excitatory postsynaptic current, short-term plasticity, and long-term plasticity. It is dependent on light intensity and gate bias intensity, and has a strong light response to 420nm blue-violet light. Attached Figure Description
[0031] Figure 1 This is a device structure diagram of the organic field-effect transistor provided by the present invention;
[0032] Figure 2 These are scanning electron microscope images of the functional layer prepared in Example 1;
[0033] Figure 3 These are the storage window characteristic curves of the transistors prepared in Example 1 and Comparative Example 1;
[0034] Figure 4 The transfer characteristic curves of the organic field-effect transistor prepared in Comparative Example 2 are shown.
[0035] Figure 5 The transfer characteristic curves are those of the organic field-effect transistor prepared in Example 1;
[0036] Figure 6 The output characteristic curve of the organic field-effect transistor prepared in Example 1;
[0037] Figure 7 The storage window characteristic curve is shown for the organic field-effect transistor prepared in Example 1.
[0038] Figure 8 These are the read / write / erase cycle characteristic curves of the organic field-effect transistor prepared in Example 1;
[0039] Figure 9 This is the sustain time characteristic curve of the organic field-effect transistor prepared in Example 1;
[0040] Figure 10 These are simulated artificial synaptic excitatory postsynaptic current images of the organic field-effect transistor prepared in Example 1;
[0041] Figure 11 These are simulation curves of the dual-pulse facilitated synaptic function of the organic field-effect transistor prepared in Example 1;
[0042] Figure 12 The simulated curve of the dual-pulse suppression synaptic function of the organic field-effect transistor prepared in Example 1 is shown.
[0043] Figure 13 These are simulation curves of enhanced synaptic function of the organic field-effect transistor prepared in Example 1 based on different gate bias voltages;
[0044] Figure 14 These are simulation curves of the synaptic suppression function of the organic field-effect transistor prepared in Example 1 based on different gate bias voltages;
[0045] Figure 15 These are the UV-Vis absorption curves of the functional layer and organic semiconductor layer in the organic field-effect transistor prepared in Example 1;
[0046] Figure 16 These are simulation curves of enhanced synaptic function based on different lights for the organic field-effect transistor prepared in Example 1;
[0047] Figure 17 The mobility comparison diagram shows the organic field-effect transistors prepared in Examples 1-3;
[0048] Wherein, 1 is the gate layer; 2 is the gate insulating layer; 3 is the functional layer; 4 is the organic semiconductor layer; 5 is the source electrode; and 6 is the drain electrode. Detailed Implementation
[0049] The present invention will be further described below with reference to the embodiments. The following embodiments are only used to more clearly illustrate the technical solution of the present invention, and should not be used to limit the scope of protection of the present invention.
[0050] This invention provides an organic field-effect transistor, see [link to relevant documentation]. Figure 1 ,include,
[0051] Gate layer 1;
[0052] Gate insulating layer 2 located on the surface of gate layer 1;
[0053] Functional layer 3 is located on the surface of the gate insulating layer 2; the functional layer is a blend of polystyrene (PS) and poly[2,6′]-4,8-di(5-ethylhexylthiophene)benzo[1,2-b;3,3-b]dithiophene]{3-fluoro-2[(2-ethylhexyl)carbonyl]thiophene[3,4-b]thiophenediyl} (PTB7-Th);
[0054] Organic semiconductor layer 4 located on the surface of functional layer 3;
[0055] The source electrode 5 and drain electrode 6 are located on the surface of the organic semiconductor layer 4.
[0056] Specifically, the thickness of the functional layer is 30-40 nm. The molecular weight of PTB7-Th is 70,000. The molecular weight of polystyrene is 280,000. The functional layer is made by coating and drying a mixed solution of poly[2,6′]-4,8-di(5-ethylhexylthiophene)benzo[1,2-b;3,3-b]dithiophene]{3-fluoro-2[(2-ethylhexyl)carbonyl]thiophene[3,4-b]thiophenediyl} and polystyrene on the surface of the gate insulating layer in one step. Preferably, the solvent of the mixed solution is chlorobenzene.
[0057] When preparing a mixed solution of PS and PTB7-Th, PS and PTB7-Th can be dissolved separately in chlorobenzene solvent before mixing. When dissolving PS, the concentration is 10 mol / ml, and the solution is allowed to stand for 24 hours. When dissolving PTB7-Th, the concentration is 10 mg / ml, and the solution is stirred at 75°C for 5 hours. Afterwards, the PS and PTB7-Th solutions are mixed in a specific ratio and stirred at 75°C for 1.5 hours to obtain the mixed solution of PS and PTB7-Th. The volume ratio of the PS solution to the PTB7-Th solution is (1-2):(1-2), preferably 1:1.
[0058] The gate layer is made of highly doped silicon. The gate insulating layer is made of silicon dioxide and has a thickness of 50 nm. The source and drain electrodes are made of metallic copper and have a thickness of 50 nm.
[0059] A base layer can be added to the bottom of the gate layer as needed.
[0060] The organic semiconductor layer is a pentacene film with a thickness of 50 nm.
[0061] This invention also provides a method for fabricating an organic field-effect transistor, comprising,
[0062] 1) Forming a gate insulating layer on the gate layer surface: A highly doped silicon wafer can be used as the gate layer. Silicon dioxide is generated by thermal oxidation on the highly doped silicon wafer as the gate insulating layer. The wafer is then sequentially cleaned with acetone, ethanol, and deionized water for 15 min each, dried, and treated with ultraviolet ozone for 5 min. The thickness of the gate insulating layer is preferably 50 nm.
[0063] 2) Fabrication of functional layers:
[0064] Preparation of the blended layer material solution: PS and PTB7-Th can be dissolved separately in chlorobenzene solvent and then mixed. When dissolving PS (molecular weight 280,000), the concentration is 10 mol / ml, and it is allowed to stand for 24 hours. When dissolving PTB7-Th (molecular weight 70,000), the concentration is 10 mg / ml, and it is stirred at 75°C for 5 hours. Then, the PS solution and PTB7-Th solution are mixed at a volume ratio of 1:1 and stirred at 75°C for 1.5 hours to obtain a mixed solution of PS and PTB7-Th.
[0065] A mixed solution of PS and PTB7-Th was spin-coated onto the surface of the gate insulating layer in one step (1500 rpm, 30 s), and then dried (110 ℃, 30 min) to form a functional layer with a thickness of 30-40 nm.
[0066] 3) Forming an organic semiconductor layer on the surface of the functional layer: A pentabenzene layer was prepared by vacuum evaporation at a deposition rate of [missing information]. Vacuum degree controlled at 5*10 -4 Below pa. The thickness of the organic semiconductor layer is 50 nm.
[0067] 4) A source electrode and a drain electrode are formed on the surface of the organic semiconductor layer to obtain the aforementioned organic field-effect transistor.
[0068] The source and drain electrodes are made of copper with a thickness of 50 nm. They were fabricated using vacuum evaporation at a deposition rate of [missing information]. Vacuum degree controlled at 5*10 -4 Below pa.
[0069] The organic field-effect transistor provided by this invention can be used in optoelectronic fields, such as semiconductor storage, microelectronics, and integrated circuits.
[0070] In the following examples and comparative examples, the gate layer and gate insulating layer are finished products purchased from Suzhou Jingxi Electronics Technology Co., Ltd. The surface is 50nm silicon dioxide as the gate insulating layer, and the bottom layer is a silicon wafer as the gate layer with an area of 1.5*1.5cm.
[0071] PTB7-Th was prepared using the method described in the literature Random terpolymer with a cost-effective monomer and comparable efficiency to PTB7-Th for bulk-heterojunction polymer solar cells. (10.1039 / c5py01771h).
[0072] PS (molecular weight 280,000) was purchased from Sigma, CAS number: 9003-53-6. Pentylene was purchased from Sigma, CAS number: 135-48-8.
[0073] Example 1
[0074] (1) Preparation of functional layer material solution: When dissolving PS (molecular weight 280,000), the concentration was 10 mol / ml, and the solution was allowed to stand for 24 h. When dissolving PTB7-Th (molecular weight 70,000), the concentration was 10 mg / ml, and the solution was stirred at 75℃ for 5 h. Afterwards, the PS solution and PTB7-Th solution were mixed at a volume ratio of 1:1 and stirred at 75℃ for 1.5 h.
[0075] (2) The gate layer and the gate insulating layer were sequentially cleaned with acetone, ethanol and deionized water for 15 min each, and then dried.
[0076] (3) Place the cleaned gate layer and gate insulating layer after drying into an ultraviolet ozone treatment for 5 minutes;
[0077] (4) Use a pipette to take the solution prepared in step (1) and spin-coat the grid insulating layer prepared in step (3) to form a film (spin-coat 100 μL). Adjust the rotation speed to 1500 rpm and rotate at a constant speed for 30 seconds. Place the spin-coated sample in an oven at 110°C for 30 minutes to remove excess solvent.
[0078] (5) An organic semiconductor layer, source electrode, and drain electrode are deposited on the sample prepared in (4) to obtain an organic field-effect transistor. The deposition rate is [missing information]. Vacuum degree controlled at 5*10 -4 The source and drain electrodes are made of copper with a thickness of 50 nm. The organic semiconductor layer is a pentacene film with a thickness of 50 nm. The mask has a channel width of 1500 μm and a length of 100 μm.
[0079] Figure 2 The image shows the surface of the functional layer observed by scanning electron microscopy. The white stripes are precipitated PTB7-Th, indicating that PTB7-Th has been precipitated at the micrometer level on the surface.
[0080] Example 2
[0081] Except for mixing the PS solution and PTB7-Th solution at a volume ratio of 1:2 when preparing the functional layer material solution, the other steps are the same as in Example 1.
[0082] Example 3
[0083] Except for mixing the PS solution and PTB7-Th solution at a volume ratio of 2:1 when preparing the functional layer material solution, the other steps are the same as in Example 1.
[0084] Comparative Example 1
[0085] Except for replacing the functional layer material solution with a 10 mol / ml PS (molecular weight 280,000) chlorobenzene solution, the remaining steps are the same as in Example 1.
[0086] Comparative Example 2
[0087] Except for replacing the functional layer material solution with a 10 mg / ml PTB7-Th (molecular weight 70000) chlorobenzene solution, the remaining steps are the same as in Example 1.
[0088] The performance of transistors was examined in air using a Keithley 4200 semiconductor parameter analyzer.
[0089] Figure 3 The transistors fabricated for Example 1 (illustrated Example 1) and Comparative Example 1 (illustrated PS transistor) were subjected to the same optical operation writing conditions (source-drain voltage 20V, 5mW / cm). 2 By comparing the storage windows under white light (1s) conditions, it is clear that Example 1 can obtain a larger storage window under the same conditions.
[0090] Figure 4 The transfer characteristic curves of the transistor prepared in Comparative Example 2 are shown. Figure 5 The transfer characteristic curve of the transistor prepared in Example 1 is shown. Test conditions: dark conditions, source-drain voltage -15V. Compared to Comparative Example 2, the mobility of Example 1 increased from 0.016 cm⁻¹. 2 V -1 s -1 Increased to 0.036cm 2 V -1 s -1 The switching ratio is from 10 2 Upgraded to 10 3 The threshold voltage dropped from 0.85V to 0.82V.
[0091] Figure 17 The mobility of the transistors prepared in Examples 1-3 was measured under dark conditions with a source-drain voltage of -15V. It can be seen that the transistors have the highest mobility when the PS solution and PTB7-Th solution are mixed at a volume ratio of 1:1.
[0092] Figure 6 The output curves of the transistor prepared in Example 1 (under dark conditions) were tested with different gate bias voltages of 0, -2V, -4V, -6V, -8V, and -10V. It can be seen that the device has good field effect.
[0093] Figure 7 The storage window curve of the transistor prepared in Example 1 is shown, with the source-drain voltage fixed at -15V. After a gate bias of 20V and a voltage of 5mW / cm², the transistor was... 2The transistor, with its white light synergy, can achieve a storage window of nearly 20V in 1s (write condition) and can be erased by a -20V gate bias in 1s (erase condition). After 90 write / erase cycles, the transistor shows no significant degradation in source-drain current on / off ratio and achieves an effective information storage time of 10,000s in sustain time testing. See [link to relevant documentation] for details. Figure 8 The read / write erase cycle curves (source / drain current values when gate bias is 0V) and Figure 9 The sustain time curves (after passing the write condition, the source and drain current of the transistor is tested with a source and drain voltage of -15V under a gate bias of 0V to obtain the current curve of the write state; after passing the erase condition, the source and drain current of the transistor is tested with a source and drain voltage of -15V under a gate bias of 0V to obtain the current curve of the erase state).
[0094] The short-term time-dependent plasticity of the photosynaptic function of the organic field-effect transistor prepared in Example 1 was investigated. Figure 10 The gate bias voltage was 0V, the source-drain voltage was -15V, a 20V gate bias voltage pulse was applied for 3.2s at 100s, and a 5mW / cm pulse was applied for 3.2s at 200s. 2 A white light pulse was generated, with a 20V gate bias and 5mW / cm² applied for 3.2 seconds at 200s. 2 A white light pulse. It can be seen that using 5mW / cm... 2 Co-pulse stimulation with white light and a 20V gate bias voltage simulated the excitatory postsynaptic current characteristics of an artificial synapse after 300 s. At a source-drain voltage of -15V, two 0.4s-long gate bias voltages with a 3.2s interval and a voltage of 5mW / cm² were applied. 2 Co-pulses of white light, such as Figure 11 As shown, two consecutive excitatory current behaviors were observed, and the transistor simulated the double-pulse dissimilarity characteristic of an artificial synapse after stimulation. Following the double-pulse dissimilarity characteristic experiment, a -20V gate bias voltage, lasting 0.4s and spaced 3.2s apart, was applied at a source-drain voltage of -15V. (See [reference needed]). Figure 12 The transistor exhibited two consecutive inhibitory current behaviors after being stimulated, simulating the double-pulse inhibition characteristics of an artificial synapse.
[0095] The long-term ductility of the organic field-effect transistor prepared in Example 1 under different gate bias voltages was investigated. Figure 13 For 30 consecutive 0.4s cycles of 5mW / cm², the transistor... 2Long-range enhancement curves of artificial synapses under synergistic pulse stimulation with white light and different gate bias voltages were plotted. The source-drain voltage was -15V, and the gate bias voltage was 0V without pulses. Each pulse interval was 3.2s. The increase in source-drain current increased with increasing forward gate bias voltage. When the applied forward gate bias voltage was 20V, the current quickly reached its maximum value, and further stimulation could not increase the current further. Following the long-range enhancement stimulation experiment, a long-range inhibition experiment of artificial synapses was performed on the transistor. Figure 14 The figures show the long-range suppression curves of the artificial synapse under 30 consecutive pulses with different gate biases. The source-drain voltage was -15V, and the gate bias was 0V when there was no pulse. The pulse interval was 3.2s. The decrease in source-drain current after each pulse increased with the increase of negative gate bias. These two factors indicate that the organic field-effect transistor fabricated in this invention has adjustable synaptic characteristics to different gate biases, simulating the function of a photoelectric synaptic transistor.
[0096] The photosynaptic transistor function of the organic field-effect transistor prepared in Example 1 was examined based on the long-term plasticity of different light.
[0097] Figure 15 These are the UV-Vis absorption curves of the functional layer, organic semiconductor layer (pentaphenyl layer), and functional layer and organic semiconductor layer of an organic field-effect transistor (obtained by a LAMBDA 650S UV-Vis spectrophotometer).
[0098] See Figure 16 ,according to Figure 15 The UV-Vis curves were obtained using 420nm and 670nm light. Test conditions included a source-drain voltage of -15V, a gate bias of 0V without pulses, and a pulse interval of 3.2s. Under the combined pulses of light and a 20V gate bias, the transistor's source-drain current continuously increased, analogous to the long-term enhancement characteristics of an artificial synapse. Furthermore, this transistor simulates the synaptic characteristics of an artificial synapse with adjustable synaptic properties for different light sources.
[0099] In summary, the organic field-effect transistor provided by this invention can stably realize the functions of memory and photoelectric synaptic transistor, and has potential applications in optoelectronic human-computer interaction and cognitive systems.
[0100] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the technical principles of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. An organic field-effect transistor, characterized in that, include, Gate layer; The gate insulating layer located on the surface of the gate layer; A functional layer located on the surface of the gate insulating layer; the functional layer is a blend film of polystyrene and poly[2,6′]-4,8-bis(5-ethylhexylthiophene)benzo[1,2-b;3,3-b]dithiophene]{3-fluoro-2[(2-ethylhexyl)carbonyl]thiophene[3,4-b]thiophenediyl}; An organic semiconductor layer located on the surface of the functional layer; The source electrode and drain electrode are located on the surface of the organic semiconductor layer; The mixed solution of poly[2,6′]-4,8-di(5-ethylhexylthiophene)benzo[1,2-b;3,3-b]dithiophene]{3-fluoro-2[(2-ethylhexyl)carbonyl]thiophene[3,4-b]thiophenediyl} and polystyrene is prepared by mixing a chlorobenzene solution of poly[2,6′]-4,8-di(5-ethylhexylthiophene)benzo[1,2-b;3,3-b]dithiophene]{3-fluoro-2[(2-ethylhexyl)carbonyl]thiophene[3,4-b]thiophenediyl} with a concentration of 10 mg / ml and a chlorobenzene solution of polystyrene with a concentration of 10 mg / ml in a volume ratio of (1-2):(1-2); The molecular weight of the poly[2,6′]-4,8-bis(5-ethylhexylthiophene)benzo[1,2-b;3,3-b]dithiophene]{3-fluoro-2[(2-ethylhexyl)carbonyl]thiophene[3,4-b]thiophenediyl} is 70,000; the molecular weight of the polystyrene is 280,000.
2. The organic field-effect transistor according to claim 1, characterized in that, The thickness of the functional layer is 30-40 nm.
3. The organic field-effect transistor according to claim 1, characterized in that, The functional layer is prepared by coating and drying a mixed solution of poly[2,6′]-4,8-bis(5-ethylhexylthiophene)benzo[1,2-b;3,3-b]dithiophene]{3-fluoro-2[(2-ethylhexyl)carbonyl]thiophene[3,4-b]thiophenediyl} and polystyrene on the surface of the gate insulating layer in one step.
4. The organic field-effect transistor according to claim 1, characterized in that, The organic semiconductor layer is a pentacene film layer.
5. The method for fabricating an organic field-effect transistor according to any one of claims 1-4, characterized in that, include, A gate insulating layer is formed on the surface of the gate layer; A mixed solution of poly[2,6′]-4,8-bis(5-ethylhexylthiophene)benzo[1,2-b;3,3-b]dithiophene]{3-fluoro-2[(2-ethylhexyl)carbonyl]thiophene[3,4-b]thiophenediyl} and polystyrene is coated onto the surface of the gate insulating layer in one step and dried to form a functional layer on the surface of the gate insulating layer; An organic semiconductor layer is formed on the surface of the functional layer; Source and drain electrodes are fabricated in an organic semiconductor layer to form an organic field-effect transistor.
6. The preparation method according to claim 5, characterized in that, A mixed solution of poly[2,6′]-4,8-bis(5-ethylhexylthiophene)benzo[1,2-b;3,3-b]dithiophene]{3-fluoro-2[(2-ethylhexyl)carbonyl]thiophene[3,4-b]thiophenediyl} and polystyrene is spin-coated onto the surface of a gate insulating layer in one step and dried to form a functional layer on the surface of the gate insulating layer; Spin coating was performed at a speed of 1500 rpm for 30 seconds; drying temperature was 110 ℃ and drying time was 30 minutes.
7. The application of the organic field-effect transistor according to any one of claims 1-4 in the optoelectronic field.
Citation Information
Patent Citations
Organic field effect transistor, preparation and application thereof
CN101295765A
Semiconductor polymer containing benzobithiophene and thiophene, preparation and applications thereof
CN104448247A
Thin-film transistors
US20090256139A1