Adhesive sheet, display device using the same, and adhesive layer-forming composition for manufacturing the adhesive sheet

By using an adhesive sheet containing pigments with a specific wavelength range and an ultraviolet absorption layer in the display device, combined with low refractive index and high refractive index layers, the problems of high reflectivity, low brightness, and large thickness of the display device are solved, achieving high brightness, thinness, and improved color reproduction.

CN116710813BActive Publication Date: 2026-11-20TOPPAN HOLDINGS INC +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202180090713.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-01-19
Filing Date
2021-09-22
Publication Date
2026-11-20
Estimated Expiration
2041-09-22

AI Technical Summary

Technical Problem

The display quality of the display device is reduced due to reflection of external light, resulting in reduced brightness and insufficient color reproduction. Furthermore, the increased thickness caused by existing circular polarizers makes it difficult to achieve a thinner design.

Method used

By using adhesive sheets containing pigments and ultraviolet absorption layers with specific wavelength ranges, external light and ultraviolet rays are absorbed. Combined with low refractive index and high refractive index layers to reduce reflection, and using transparent substrates and anti-glare layers to control light scattering, thinness and high brightness are achieved.

Benefits of technology

It achieves low reflectivity, high brightness, and improved color reproduction in display devices, and can also be made thinner, solving the problems of reduced brightness and increased thickness in existing technologies.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116710813B_ABST
    Figure CN116710813B_ABST
Patent Text Reader

Abstract

Provided is an adhesive sheet capable of achieving low reflectance, high brightness, and thinness of a display device, a display device using the adhesive sheet, and an adhesive layer-forming composition for manufacturing the adhesive sheet. The adhesive sheet is characterized by comprising a first adhesive layer containing an adhesive and a pigment, and an ultraviolet absorbing layer laminated on one face side of the first adhesive layer, the pigment containing: a first color material having a maximum absorption wavelength in the range of 470 to 530 nm and a half-value width of an absorption spectrum of 15 to 45 nm, and a second color material having a maximum absorption wavelength in the range of 560 to 620 nm and a half-value width of an absorption spectrum of 15 to 55 nm, and the ultraviolet absorbing layer having an ultraviolet shielding rate of 85% or more according to JIS L 1925.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to adhesive sheets for display devices, display devices using the adhesive sheets, and compositions for forming adhesive layers for manufacturing adhesive sheets. Background Technology

[0002] Display devices, whether indoors or outdoors, are mostly used in environments with external light incident on them. External light incident on the display device is reflected off its surface, and the reflected image mixes with the displayed image, thus degrading display quality. Therefore, display devices need to be equipped with anti-reflective functions, and to improve display quality, high-performance anti-reflective functions are required.

[0003] Typically, anti-reflective properties can be achieved by forming a low-refractive-index layer on the surface of a display device. Furthermore, to further enhance the anti-reflective performance, methods are known to involve providing a high-refractive-index layer, or both a medium-refractive-index layer and a high-refractive-index layer, with a low-refractive-index layer formed on the outermost surface.

[0004] In addition, there is a problem that external light incident on the display device is reflected by components inside the display device (e.g., electrodes, phosphors, color filters), and the reflected light is then emitted again from the display surface, thereby reducing the display quality. To address this problem, methods are known to reduce the incidence of external light into the display device and its reflection inside by providing a circular polarizer on the display surface side (e.g., see Patent Document 1).

[0005] In addition, display devices typically require high color purity. Color purity indicates the breadth of colors a display device can display, also known as the color reproduction range. Therefore, high color purity means a wide color reproduction range and good color reproduction. Regarding improving color reproduction, methods are known to use color filters to separate the white light source of the display panel, or to use color filters to correct the monochromatic light source to narrow the half-width.

[0006] Existing technical documents

[0007] Patent documents

[0008] Patent Document 1: Japanese Patent Application Publication No. 2013-251376 Summary of the Invention

[0009] The problem that the invention aims to solve

[0010] In display devices that use circular polarizers to provide anti-reflective properties, the light emitted from the display panel is also absorbed by the polarizer. If absorption caused by films and other components outside the polarizer is considered, the transmittance of light emitted from the display panel is less than 50%, resulting in a significant reduction in brightness. To compensate for this brightness reduction, the luminous intensity of the display panel needs to be increased, but this may reduce the lifespan of the light-emitting elements. Furthermore, the use of circular polarizers also presents the challenge of achieving a thinner form factor due to the inherent thickness of the polarizer itself.

[0011] In addition, improving the color reproduction of display devices requires thicker color filters or higher concentrations of color materials, which can lead to a decrease in display quality, such as deterioration of pixel shape or viewing angle characteristics.

[0012] Therefore, the object of the present invention is to provide an adhesive sheet that can achieve low reflectivity, high brightness and thinness of a display device, as well as improved color reproduction, a display device using the adhesive sheet, and a composition for forming an adhesive layer for manufacturing the adhesive sheet.

[0013] Methods for solving problems

[0014] The adhesive sheet of the present invention comprises: a first adhesive layer containing an adhesive and a pigment, and an ultraviolet absorbing layer laminated on one side of the first adhesive layer. The pigment is characterized in that it comprises: a first color material with a maximum absorption wavelength in the range of 470–530 nm and a half-width of the absorption spectrum of 15–45 nm, and a second color material with a maximum absorption wavelength in the range of 560–620 nm and a half-width of the absorption spectrum of 15–55 nm; and the ultraviolet absorbing layer has an ultraviolet shielding rate of 85% or more according to JIS L 1925.

[0015] In addition, the display device of the present invention includes the aforementioned adhesive sheet.

[0016] Furthermore, the adhesive layer forming composition of the present invention is characterized in that it contains an adhesive, a pigment, and an additive, wherein the pigment contains: a first color material with a maximum absorption wavelength in the range of 470 to 530 nm and a half-width of the absorption spectrum of 15 to 45 nm, and a second color material with a maximum absorption wavelength in the range of 560 to 620 nm and a half-width of the absorption spectrum of 15 to 55 nm, and the additive contains one or more of a free radical scavenger, a peroxide decomposer, and a singlet oxygen quencher.

[0017] The effects of the invention

[0018] According to the present invention, an adhesive sheet capable of achieving low reflectivity, high brightness, thinness and improved color reproduction of a display device, a display device using the adhesive sheet, and a composition for forming an adhesive layer for manufacturing an adhesive film can be provided. Attached Figure Description

[0019] [ Figure 1 ] Figure 1 This is a cross-sectional view showing a schematic configuration of the adhesive sheet according to the first embodiment.

[0020] [ Figure 2 ] Figure 2 This is a cross-sectional view showing a schematic configuration of the adhesive sheet according to the second embodiment.

[0021] [ Figure 3 ] Figure 3 This is a cross-sectional view showing a schematic configuration of the adhesive sheet according to the third embodiment.

[0022] [ Figure 4 ] Figure 4 This is a cross-sectional view showing a schematic configuration of the adhesive sheet according to the fourth embodiment.

[0023] [ Figure 5 ] Figure 5 This is a cross-sectional view showing a schematic configuration of the display device according to the fifth embodiment.

[0024] [ Figure 6 ] Figure 6 This is a cross-sectional view showing a schematic configuration of the display device according to the sixth embodiment.

[0025] [ Figure 7 ] Figure 7 This is a cross-sectional view showing a schematic configuration of the display device according to the seventh embodiment.

[0026] [ Figure 8 ] Figure 8 It is the spectrum of a light source used to evaluate its transmission characteristics.

[0027] [ Figure 9 ] Figure 9 It is the spectrum of a light source used to evaluate color reproduction. Detailed Implementation

[0028] Figures 1-4 These are cross-sectional views illustrating the schematic configuration of the adhesive sheet according to embodiments 1 to 4. Figures 1-4 The upper side corresponds to the viewing side of the display device when used in a display device. In this specification, "adhesive sheet" refers to an adhesive sheet that contains an adhesive layer formed by making a sheet of adhesive material, either alone or in combination with other layers, including: an adhesive layer consisting only of sheet adhesive, an adhesive layer having a release film on one or both sides, and an adhesive layer having a film with a transparent substrate on at least one side.

[0029] Details will be discussed later. Figures 1-4The adhesive sheets 11-14 shown have a first adhesive layer 21 containing pigments that absorb light in a specific wavelength range. The display panel to which the adhesive sheets 11-14 are used is a display panel with a light source, particularly in the case of self-emissive display panels such as organic EL panels or micro-LED panels, where metal electrodes or reflective components are provided. The first adhesive layer 21 reduces reflected light by absorbing a portion of the external light incident on the adhesive sheets 11-14 and a portion of the external light reflected by the display panel (not shown) adhered to the first adhesive layer 21. However, the pigments contained in the first adhesive layer 21 have low lightfastness; if oxidized by ultraviolet light contained in external light, their light absorption decreases. Therefore, in this invention, by providing an ultraviolet absorption layer that absorbs ultraviolet light near the observation side of the first adhesive layer 21, the deterioration (fading) of the first adhesive layer 21 caused by incident ultraviolet light is suppressed.

[0030] Figure 1 The adhesive sheet 11 shown includes a first adhesive layer 21 and a second adhesive layer 22 laminated on one side of the first adhesive layer 21. The adhesive sheet 11 is used to adhere a separately manufactured optical film to a display panel. When using the adhesive sheet 11 to adhere the optical film, the adhesive sheet 11 is used with the first adhesive layer 21 facing the display panel side and the second adhesive layer 22 facing the optical film side. Figure 1 In this example, the second adhesive layer 22 functions as a UV-absorbing layer by containing a UV absorber. It should be noted that a release film (not shown) can also be peeled off from the surfaces of the first adhesive layer 21 and the second adhesive layer 22. The release film protects the first adhesive layer 21 and the second adhesive layer 22 until the adhesive sheet 11 is used.

[0031] Figure 2 The adhesive sheet 12 shown includes a first adhesive layer 21 and a transparent substrate 20 adhered to one side of the first adhesive layer 21. The adhesive sheet 12 with the transparent substrate 20 is used as an optical film adhered to the surface of a display panel. Typically, as described later, an optical functional layer for controlling incident light is provided on the transparent substrate 20. The adhesive sheet 12 is used with the first adhesive layer 21 adhered to the display panel and the transparent substrate 20 facing the viewing side of the display device. Figure 2 In this example, the transparent substrate 20 functions as a UV-absorbing layer by containing a UV absorber. It should be noted that a release film (not shown) can also be peeled off from the surface of the first adhesive layer 21. The release film protects the first adhesive layer 21 until the adhesive sheet 12 is used.

[0032] Figure 3 The adhesive sheet 13 shown is in Figure 1The adhesive sheet 13 shown is further formed by providing a transparent substrate 20 on the adhesive sheet 11. That is, the adhesive sheet 13 includes a first adhesive layer 21, a second adhesive layer 22 laminated on one side of the first adhesive layer 21, and a transparent substrate 20 adhered to the second adhesive layer 22. The adhesive sheet 13 with the transparent substrate 20 is used as an optical film adhered to the surface of a display panel. Typically, as described later, an optical functional layer for controlling incident light is provided on the transparent substrate 20. The adhesive sheet 13 is used with the first adhesive layer 21 adhered to the display panel and the transparent substrate 20 serving as the viewing side of the display device. Figure 3 In the example, the second adhesive layer 22 functions as an ultraviolet absorbing layer by containing an ultraviolet absorber. However, in addition to the second adhesive layer 22, the transparent substrate 20 can also be an ultraviolet absorbing layer containing an ultraviolet absorber. It should be noted that a release film (not shown) can also be adhered to the surface of the first adhesive layer 21 in a peelable manner. The release film can protect the first adhesive layer 21 until the adhesive sheet 12 is used.

[0033] Figure 4 The adhesive sheet 14 shown includes an adhesive layer 30 laminated on one side of the transparent substrate 20 and an oxygen barrier layer 23 laminated on the other side of the transparent substrate 20. The adhesive layer 30 is either the first adhesive layer 21 described above, or a laminate of a second adhesive layer 22 and a first adhesive layer 21 sequentially laminated from the transparent substrate 20 side. That is, Figure 4 The adhesive sheet 14 shown has in Figure 2 The adhesive sheet 11 shown or Figure 3 The adhesive sheet 13 shown is formed by further providing an oxygen barrier layer 23 on the transparent substrate 20. The oxygen barrier layer 23, as will be described later, is a functional layer used to inhibit the deterioration caused by the oxidation of pigments contained in the first adhesive layer 21 by blocking the intrusion of oxygen into the first adhesive layer 21. The adhesive sheet 14 with the transparent substrate 20 is used as an optical film adhered to the surface of the display panel. Typically, as described later, an optical functional layer for controlling incident light is provided on top of the transparent substrate 20. The adhesive sheet 14 is used with the first adhesive layer 21 adhered to the display panel and the oxygen barrier layer 23 facing the viewing side of the display device. Figure 4 In this example, the second adhesive layer 22 or the transparent substrate 20 contained in the adhesive layer 30 functions as a UV-absorbing layer by containing a UV absorber. It should be noted that a release film (not shown) can also be peeled off and adhered to the surface of the first adhesive layer 21. The release film protects the first adhesive layer 21 until the adhesive sheet 12 is used.

[0034] Figures 5-7 These are cross-sectional views showing schematic configurations of the display devices according to embodiments 5 through 7. Figures 5-7The upper side corresponds to the viewing side when observing the displayed image on the display device.

[0035] Figure 5 The display device 1 shown includes a display panel 10 and an adhesive sheet 15 disposed on the display surface side of the display panel 10. The display panel 10 is a display panel with a light source, typically a self-emissive display panel such as an organic EL panel or a micro-LED panel. The adhesive sheet 15 includes a transparent substrate 20, an adhesive layer 30 laminated on one side of the transparent substrate 20, a high refractive index layer 24 laminated on the other side of the transparent substrate, and a low refractive index layer 25. It should be noted that... Figures 5-7 The adhesive layer 30 shown is either the first adhesive layer 21 or a laminate of the first and second adhesive layers. The low-refractive-index layer 25 of the adhesive sheet 15 forms the outermost surface of the viewing side of the display device 1, and the adhesive layer 30 is adhered to the display surface of the display panel 10. The refractive index of the low-refractive-index layer 25 is lower than that of the high-refractive-index layer 24, and the high-refractive-index layer 24 and the low-refractive-index layer 25 constitute an anti-reflective layer. The high-refractive-index layer 24 and the low-refractive-index layer 25 cancel out external light incident on the adhesive sheet 15 and reflected light after interlayer reflection within the adhesive sheet 15 through interference, thereby reducing the reflection of external light. That is, Figure 5 The adhesive sheet 15 shown is in Figure 2 The adhesive sheet 12 shown or Figure 3 An adhesive sheet is formed by further providing an anti-reflective layer on the adhesive sheet 13 shown.

[0036] Figure 6 The display device 2 shown includes a display panel 10 and an adhesive sheet 16 disposed on the display surface side of the display panel 10. The adhesive sheet 16 includes a transparent substrate 20, an adhesive layer 30 laminated on one side of the transparent substrate 20, and an anti-glare layer 26 laminated on the other side of the transparent substrate 20. The anti-glare layer 26 of the adhesive sheet 16 forms the outermost surface of the viewing side of the display device 2, and the adhesive layer 30 is adhered to the display surface of the display panel 10. The anti-glare layer 26 is an optical functional layer for controlling the reflection of external light; it reduces the amount of external light entering by scattering external light through fine irregularities formed on its surface. That is, Figure 6 The adhesive sheet 16 shown is in Figure 2 The adhesive sheet 12 shown or Figure 3 An adhesive sheet is formed by further providing an anti-glare layer on the adhesive sheet 13 shown.

[0037] Figure 7The display device 3 shown includes a display panel 10 and an adhesive sheet 17 disposed on the display surface side of the display panel 10. The adhesive sheet 17 includes a transparent substrate 20, an adhesive layer 30 laminated on one side of the transparent substrate 20, an anti-glare layer 26 laminated on the other side of the transparent substrate 20, and a low-refractive-index layer 25. The low-refractive-index layer 25 of the adhesive sheet 17 forms the outermost surface of the viewing side of the display device 3, and the adhesive layer 30 is adhered to the display surface of the display panel 10. The anti-glare layer 26 is an optical functional layer for controlling the reflection of external light; it reduces the amount of external light entering by scattering external light through fine irregularities formed on its surface. Furthermore, the refractive index of the low-refractive-index layer 25 is lower than that of the anti-glare layer 26, and the anti-glare layer 26 and the low-refractive-index layer 25 constitute an anti-reflective layer. That is, Figure 7 The adhesive sheet 17 shown is in Figure 2 The adhesive sheet 12 shown or Figure 3 The adhesive sheet shown is formed by further providing an anti-glare layer and an anti-reflection layer on the adhesive sheet 13.

[0038] The following is a detailed description of each layer of the adhesive sheets 11 to 17.

[0039] <First adhesive layer>

[0040] The first adhesive layer 21 is a layer used to absorb a portion of the external light incident on the first adhesive layer 21 and a portion of the reflected light that is reflected by the metal electrodes or reflective components of the display panel and then re-incidentally incident on the first adhesive layer 21, thereby reducing the reflection of external light. The first adhesive layer 21 contains an adhesive and a pigment that absorbs visible light. The adhesive is not particularly limited and can be silicone-based, acrylic-based, urethane-based, etc. The first adhesive layer 21 contains a first color material and a second color material as pigments. The maximum absorption wavelength of the first color material is in the range of 470–530 nm and the half-width of the absorption spectrum is 15–45 nm, and the maximum absorption wavelength of the second color material is in the range of 560–620 nm and the half-width of the absorption spectrum is 15–55 nm. By using materials with the above-mentioned absorption properties as the first color material and the second color material contained in the first adhesive layer 21, the first adhesive layer 21 can absorb visible light in the wavelength region with relatively low luminous intensity emitted by the display panel.

[0041] In optical films used in display devices, optical functional layers such as anti-reflective layers or anti-glare layers are typically provided. However, a portion of the incident external light passes through these optical functional layers and reaches the display panel, where it is reflected by metal electrodes or reflective components present on the surface of the display panel. Since the light reflected inside the display device degrades the contrast and visibility of the displayed image, circular polarizers have traditionally been used to reduce reflected light from the surface of the display panel 10. In this invention, instead of reducing reflected light with a circular polarizer, a portion of the incident light is absorbed by a first adhesive layer 21 containing pigments. A portion of the remaining incident light not absorbed by the first adhesive layer 21 is reflected by the display panel, but the first adhesive layer 21 absorbs a portion of the reflected light. As a result, the internal reflectivity of external light is significantly reduced. The absorption wavelength regions of the two pigments contained in the first adhesive layer 21 do not overlap with the maximum wavelength of light emitted from the display panel, thus suppressing the reduction in the intensity of light emitted from the display panel.

[0042] The pigment contained in the first adhesive layer 21 can be a dye, pigment, or nano-metal, etc., preferably a colorant containing one or more compounds selected from the group consisting of: compounds having any one of the following structures within the molecule: porphyrin structure, phthalocyanine structure, azo structure, phthalocyanine structure, squartzite structure, coumarin structure, polyene structure, quinone structure, tetrazaporphyrin structure, pyrrole methylene structure, and indigo structure, and their metal complexes. In particular, metal complexes having a porphyrin structure, pyrrole methylene structure, or phthalocyanine structure within the molecule are more preferably used.

[0043] In addition to the two color materials mentioned above, the first adhesive layer 21 may also contain a third color material with a maximum absorption wavelength in the range of 650-800 nm. However, in the third color material, a pigment with a maximum absorption wavelength different from the maximum emission wavelength of the display panel 10 is used. By including the third color material in the first adhesive layer 21, the reflection of external light can be further reduced.

[0044] The thickness of the first adhesive layer 21 is not particularly limited, but is preferably about 5 to 100 μm, and more preferably about 10 to 60 μm.

[0045] <Second adhesive layer>

[0046] The second adhesive layer 22 is a UV-absorbing layer containing a UV absorber, used to prevent deterioration caused by oxidation of the pigments contained in the first adhesive layer 21. The adhesive is not particularly limited; silicone-based adhesives, acrylic-based adhesives, urethane-based adhesives, etc., can be used. Usable UV absorber compounds will be described later.

[0047] The thickness of the second adhesive layer 22 is not particularly limited, but is preferably about 5 to 100 μm, and more preferably about 10 to 60 μm.

[0048] <Resting Film>

[0049] When a release film is provided on the first adhesive layer 21 and / or the second adhesive layer 22, a known film that has been subjected to easy-peeling treatment by coating an organosilicon-based or non-organosilicon-based release agent on the surface of a substrate made of resins such as polyethylene terephthalate, polypropylene, and polyethylene can be used as the release film.

[0050] <Transparent substrate>

[0051] The transparent substrate 20 is formed of a material with excellent visible light transmittance. Materials forming the transparent substrate 20 can include: polyolefins such as polyethylene and polypropylene; polyesters such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate; polyacrylates such as polymethyl methacrylate; polyamides such as nylon 6 and nylon 66; transparent resins such as polyimide, polyarylate, polycarbonate, triacetyl cellulose, polyacrylate, polyvinyl alcohol, polyvinyl chloride, cyclic olefin copolymers, norbornene-containing resins, polyethersulfone, and polysulfone, or inorganic glass. A film made of polyethylene terephthalate is preferred. The thickness of the transparent substrate 20 is not particularly limited, but is preferably 10–100 μm.

[0052] like Figure 2 As shown in the configuration, without the second adhesive layer 22, the transparent substrate 20 can be used as the ultraviolet absorbing layer. In this case, the transparent substrate 20 is formed by containing a material with ultraviolet absorbing properties. Since the transparent substrate 20 has ultraviolet absorbing properties, the fading of the pigment contained in the first adhesive layer 21 can be suppressed.

[0053] <High Refractive Index Layer>

[0054] The high refractive index layer 24 can be formed by coating a high refractive index layer forming composition containing an active energy ray curable resin, a photopolymerization initiator, and a solvent, and then curing it. The high refractive index layer 24 is typically configured as a hard coating. The refractive index of the high refractive index layer 24 is preferably 1.50 to 2.40. The thickness of the high refractive index layer 24 is not particularly limited, but is preferably 2 to 10 μm. When the thickness of the high refractive index layer 24 is less than 2 μm, the hardness of the high refractive index layer 24 may be insufficient. When the thickness of the high refractive index layer 24 exceeds 10 μm, it is not conducive to the thinning of the display device, and is therefore not preferred. However, the film thickness of the high refractive index layer 24 can be appropriately set according to the required surface hardness and overall thickness. Furthermore, in order to adjust the refractive index and impart hardness, the high refractive index layer 24 may contain metal oxide particles. By incorporating metal oxide particles into the high refractive index layer 24 to achieve a high refractive index, it can be combined with the low refractive index layer described later to form an anti-reflective layer.

[0055] Resin that is cured by active energy radiation is a resin that is polymerized and cured by irradiation with active energy radiation such as ultraviolet light or electron beams. For example, monofunctional, difunctional, or trifunctional (meth)acrylate monomers can be used. It should be noted that in this specification, "(meth)acrylate" is a general term for both acrylate and methacrylate, and "(meth)acryloyl" is a general term for both acryloyl and methacryloyl.

[0056] Examples of monofunctional (meth)acrylate compounds include: 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, glycidyl (meth)acrylate, acryloylmorpholine, N-vinylpyrrolidone, tetrahydrofurfuryl acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isobornyl (meth)acrylate, and so on. Isodecyl acrylate, lauryl acrylate, tridecyl acrylate, hexadecyl acrylate, octadecyl acrylate, benzyl acrylate, 2-ethoxyethyl acrylate, 3-methoxybutyl acrylate, ethyl carbitol acrylate, methacrylate, ethylene oxide modified methacrylate, phenoxy acrylate, ethylene oxide modified phenoxy (meth)acrylate, propylene oxide modified phenoxy (meth)acrylate Methacrylate, nonylphenol (meth)acrylate, ethylene oxide modified nonylphenol (meth)acrylate, propylene oxide modified nonylphenol (meth)acrylate, methoxydiethylene glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, methoxypropylene glycol (meth)acrylate, 2-(meth)acryloyloxyethyl-2-hydroxypropyl phthalate, 2-hydroxy-3-phenoxypropyl acrylate, hydrogenated 2-(meth)acryloyloxyethyl phthalate, hydrogenated phthalic acid 2-(meth)acryloyloxypropyl ester, 2-(meth)acryloyloxypropyl hexahydrophthalic acid, 2-(meth)acryloyloxypropyl tetrahydrophthalic acid, dimethylaminoethyl methacrylate, trifluoroethyl methacrylate, tetrafluoropropyl methacrylate, hexafluoropropyl methacrylate, octafluoropropyl methacrylate, and mono(meth)acrylate derivatives of 2-adamantane and adamantanediol, such as adamantane acrylate and other mono(meth)acrylate derivatives.

[0057] Examples of difunctional (meth)acrylate compounds include: ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, butanediol di(meth)acrylate, hexanediol di(meth)acrylate, nonanediol di(meth)acrylate, ethoxylated hexanediol di(meth)acrylate, propoxylated hexanediol di(meth)acrylate, diethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, ethoxylated neopentyl glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, hydroxypentyl acid neopentyl glycol di(meth)acrylate, and other di(meth)acrylates.

[0058] Examples of trifunctional or higher (meth)acrylate compounds include: trimethylolpropane tri(meth)acrylate, ethoxylated trimethylolpropane tri(meth)acrylate, propoxylated trimethylolpropane tri(meth)acrylate, tris(2-hydroxyethyl)isocyanurate tri(meth)acrylate, glycerol tri(meth)acrylate, etc.; and trifunctional (meth)acrylates such as pentaerythritol tri(meth)acrylate, dipentaerythritol tri(meth)acrylate, and di(trimethylolpropane)acrylate. Acrylates; polyfunctional (meth)acrylates such as pentaerythritol tetra(meth)acrylate, di(trimethylolpropane)tetra(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, di(trimethylolpropane) penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and di(trimethylolpropane) hexa(meth)acrylate; and polyfunctional (meth)acrylates formed by substituting a portion of these (meth)acrylates with alkyl groups or ε-caprolactones.

[0059] Alternatively, urethane (meth)acrylates can also be used as active energy ray-curable resins. Examples of urethane (meth)acrylates include those obtained by reacting a product obtained by reacting an isocyanate monomer or prepolymer with a polyester polyol with a (meth)acrylate monomer having hydroxyl groups.

[0060] Examples of urethane (meth)acrylates include: pentaerythritol triacrylate hexamethylene diisocyanate urethane prepolymer, dipentaerythritol pentaacrylate hexamethylene diisocyanate urethane prepolymer, pentaerythritol triacrylate toluene diisocyanate urethane prepolymer, dipentaerythritol pentaacrylate toluene diisocyanate urethane prepolymer, pentaerythritol triacrylate isophorone diisocyanate urethane prepolymer, and dipentaerythritol pentaacrylate isophorone diisocyanate urethane prepolymer.

[0061] The aforementioned active energy ray-curable resin can be used in one or in combination of two or more. Furthermore, the aforementioned active energy ray-curable resin in the high refractive index layer forming composition can be a monomer or a partially polymerized oligomer.

[0062] Photopolymerization initiators used in compositions for forming high refractive index layers can include, for example, 2,2-ethoxyacetophenone, 1-hydroxycyclohexylphenyl ketone, bibenzoyl, benzoin, benzoin methyl ether, benzoin ethyl ether, p-chlorobenzophenone, p-methoxybenzophenone, michalcone, acetophenone, 2-chlorothiaxanone, etc. One of these can be used alone or in combination of two or more.

[0063] In addition, solvents used in compositions for forming high refractive index layers include: ethers such as dibutyl ether, dimethoxymethane, dimethoxyethane, diethoxyethane, propylene oxide, 1,4-dioxane, 1,3-dioxolane, 1,3,5-trioxane, tetrahydrofuran, anisole, and phenethyl ether; ketones such as acetone, methyl ethyl ketone, diethyl ketone, dipropyl ketone, diisobutyl ketone, methyl isobutyl ketone, cyclopentanone, cyclohexanone, methylcyclohexanone, and methylcyclohexanone; esters such as ethyl formate, propyl formate, n-pentyl formate, methyl acetate, ethyl acetate, methyl propionate, ethyl propionate, n-pentyl acetate, and γ-butyrolactone; and cellosolvents such as methyl cellosolvent, cellosolvent, butyl cellosolvent, and cellosolvent acetate. These can be used alone or in combination of two or more.

[0064] In addition, examples of metal oxide particles that can be incorporated into the composition for forming a high refractive index layer in order to adjust the refractive index and impart hardness include: zirconium oxide, titanium oxide, niobium oxide, antimony trioxide, antimony pentoxide, tin oxide, indium oxide, indium tin oxide, zinc oxide, etc.

[0065] As other additives, leveling agents, defoamers, antioxidants, ultraviolet absorbers, light stabilizers, photosensitizers, conductive materials, etc., can also be added to the compositions for forming high refractive index layers.

[0066] <Low Refractive Index Layer>

[0067] The low refractive index layer 25 can be formed by coating a low refractive index layer forming composition containing at least an active energy ray-curable resin onto a transparent substrate and then curing it. The active energy ray-curable resin used in the low refractive index layer forming composition can be the resin described in the high refractive index layer. To adjust the refractive index, microparticles such as LiF, MgF, 3NaF·AlF, AlF, and Na3AlF6, or silica microparticles can be incorporated into the low refractive index layer forming composition. Furthermore, using porous silica microparticles or hollow silica microparticles, which have pores within the particles, is effective for lowering the refractive index of the low refractive index layer. Additionally, photopolymerization initiators, solvents, and other additives described in the high refractive index layer can be appropriately incorporated into the low refractive index layer forming composition. The refractive index of the low refractive index layer 25 is preferably set to 1.20 to 1.55. Furthermore, the film thickness of the low refractive index layer 25 is not particularly limited, but is preferably set to 40 nm to 1 μm.

[0068] The low refractive index layer 25 may contain any one of silicon oxide, fluorinated silane compound, fluoroalkyl silazane, fluoroalkyl silane, fluorinated silicon compound, or silane coupling agent containing perfluoropolyether group. These materials can improve antifouling properties by imparting hydrophobicity and / or oleophobicity to the low refractive index layer 25.

[0069] Anti-glare layer

[0070] The anti-glare layer 26 is a layer with fine irregularities on its surface that scatter external light, thereby reducing the amount of external light entering the body. The anti-glare layer 26 can be formed by coating an anti-glare layer forming composition containing an active energy-curable resin, organic microparticles, and / or inorganic microparticles, and then curing it. The active energy-curable resin used in the anti-glare layer forming composition can be the resin described in the high refractive index layer section. The film thickness of the anti-glare layer 26 is not particularly limited, but is preferably 1 to 10 μm.

[0071] Organic microparticles are materials that form fine irregularities on the surface of the anti-glare layer 26, giving it the function of diffusing external light. As organic microparticles, resin particles composed of light-transmitting resin materials such as acrylic resin, polystyrene resin, styrene-(meth)acrylate copolymer, polyethylene resin, epoxy resin, silicone resin, polyvinylidene fluoride, and polyvinyl fluoride resin can be used. To adjust the refractive index and the dispersibility of the resin particles, two or more resin particles with different materials (refractive indices) can also be mixed and used.

[0072] Inorganic microparticles are primarily used to regulate the settling or agglomeration of organic microparticles in the anti-glare layer 26. These inorganic microparticles can include silica microparticles, metal oxide microparticles, and various mineral microparticles. For example, colloidal silica or silica microparticles with surface modifications using reactive functional groups such as (meth)acryloyl groups can be used. For example, alumina, zinc oxide, tin oxide, antimony oxide, indium oxide, titanium dioxide, and zirconium oxide can be used. For example, mica, synthetic mica, vermiculite, montmorillonite, iron montmorillonite, bentonite, bedesulfurite, soapstone, hydropyrite, talc soapstone, chloropyrite, magadiite, illite, hydrosilycite, layered titanate, montmorillonite, and synthetic montmorillonite can be used. The mineral microparticles can be either natural or synthetic (including substituted products and derivatives), or a mixture of both. Among the mineral microparticles, layered organic clay is more preferred. Layered organoclay refers to a substance obtained by introducing organonium ions into the interlayer of bentonite clay. There are no restrictions on the organonium ions as long as they can be organically converted using the cation exchange capacity of bentonite clay. When using layered organoclay minerals, the aforementioned synthetic montmorillonite is preferred as the mineral microparticle. Synthetic montmorillonite has the functions of increasing the viscosity of the coating liquid for forming the anti-glare layer, inhibiting the sedimentation of resin particles and inorganic microparticles, and adjusting the surface irregularity of the optical functional layer.

[0073] The anti-glare layer 26 may contain any one of silicon oxides, fluorinated silane compounds, fluoroalkyl silazanes, fluoroalkyl silanes, fluorinated silicon compounds, or silane coupling agents containing perfluoropolyether groups. These materials can improve the anti-fouling properties by imparting hydrophobicity and / or oleophobicity to the anti-glare layer 26.

[0074] By making the material unevenly distributed, the anti-glare layer 26 can also be formed by sequentially stacking a layer with a relatively high refractive index and a layer with a relatively low refractive index, starting from the side of the first adhesive layer 21. For example, the anti-glare layer 26 with uneven material distribution can be formed by coating a composition containing a low-refractive-index material and a high-refractive-index material with surface-modified silica particles or hollow silica particles, and then separating the two materials by utilizing the difference in their surface free energies. When the anti-glare layer 26 consists of two layers after layer separation, it is preferable to set the refractive index of the layer with a relatively high refractive index on the side of the first adhesive layer 21 to be 1.50 to 2.40, and the refractive index of the layer with a relatively low refractive index on the surface side to be 1.20 to 1.55.

[0075] <Ultraviolet Absorption Layer>

[0076] In the adhesive sheets 11-17 of the embodiments, an ultraviolet absorbing layer is provided on the upper layer (observation side) of the first adhesive layer to suppress the deterioration of the pigment contained in the first adhesive layer 21. The ultraviolet shading rate of the ultraviolet absorbing layer is preferably 85% or more. Here, the ultraviolet shading rate is a value measured according to JIS L 1925 and calculated by the following formula.

[0077] Ultraviolet (UV) blocking rate (%) = 100 - Average transmittance of UV rays with wavelengths of 290–400 nm (%)

[0078] The ultraviolet absorbing layer can be composed of a second adhesive layer 22 or a transparent substrate 20 disposed closer to the observation side than the first adhesive layer 21. However, it is also possible to replace the second adhesive layer 22 or the transparent substrate 20, or to provide an ultraviolet absorbing layer by including an ultraviolet absorber in any layer disposed closer to the observation side than the first adhesive layer 21, other than the second adhesive layer 22 or the transparent substrate 20. Furthermore, in Figures 4-7 In the example, one or more of the oxygen barrier layer 23, the high refractive index layer 24, the low refractive index layer 25 and the anti-glare layer 26 may contain ultraviolet absorbers, thus serving as ultraviolet absorbing layers.

[0079] The ultraviolet absorber is not particularly limited and can be a compound of benzophenone, benzotriazole, triazine, oxalate aniline, or cyanoacrylate. The ultraviolet absorber is formulated to inhibit the deterioration of the pigment contained in the first adhesive layer 21; therefore, a substance that absorbs light in a wavelength range that contributes to the deterioration of the pigment contained in the first adhesive layer 21 in the ultraviolet region is used.

[0080] When forming an ultraviolet-absorbing layer by coating and curing a photopolymerizable composition containing an ultraviolet absorber, if the ultraviolet absorption of the ultraviolet absorber is excessive, the curing of the composition becomes insufficient, resulting in an adhesive sheet with insufficient surface hardness. Therefore, when using a photopolymerizable composition containing an ultraviolet absorber to form an ultraviolet-absorbing layer, curing obstacles caused by the presence of the ultraviolet absorber can be suppressed by using an ultraviolet absorber whose absorption wavelength range in the ultraviolet region is different from that of the photopolymerization initiator in the ultraviolet region. The absorption wavelength range of the ultraviolet absorber in the ultraviolet region is preferably in the range of 290 to 370 nm. When the absorption wavelength range of the ultraviolet absorber contained in any layer constituting the ultraviolet-absorbing layer is set to this range, it is preferable to use an acylphosphine oxide-based photopolymerization initiator with an absorption wavelength range different from this wavelength range. Examples of acylphosphine oxide-based photopolymerization initiators include diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide or phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide. By making the absorption wavelength regions of the ultraviolet absorber and the photopolymerization initiator different, curing obstacles during the formation of an ultraviolet absorbing layer containing the ultraviolet absorber can be suppressed, and the deterioration of the pigment contained in the first adhesive layer 21 due to ultraviolet radiation can be suppressed after curing.

[0081] <Oxygen Barrier Layer>

[0082] The oxygen permeability of oxygen barrier layer 23 is 10 cc / (m 2 ·day·atm) or less, more preferably 5cc / (m 2 ·day·atm) or less, further preferably 1cc / (m 2 The oxygen barrier layer 23 can suppress the oxidative degradation (fading) of the colorant contained in the first adhesive layer 21 by means of its oxygen barrier properties. The oxygen barrier layer 23 is preferably formed of a material containing polyvinyl alcohol (PVA), ethylene-vinyl alcohol copolymer (EVOH), vinylidene chloride, siloxane resin, etc., and materials such as Maxive (registered trademark) manufactured by Mitsubishi Gas Chemical Co., Ltd., Eval manufactured by Kuraray Co., Ltd., Saran Latex and Saran Resin manufactured by Asahi Kasei Corporation can be used. Furthermore, the thickness of the oxygen barrier layer 23 is not particularly limited, as long as the desired oxygen barrier properties are achieved.

[0083] Furthermore, inorganic particles (particles composed of inorganic compounds) can be dispersed in the oxygen barrier layer 23. These inorganic particles further reduce oxygen permeability, thereby further suppressing the oxidative degradation (fading) of the first adhesive layer 21. There are no particular limitations on the size and content of the inorganic particles; they can be appropriately set according to the thickness of the oxygen barrier layer 23. The size (maximum length) of the inorganic particles dispersed in the oxygen barrier layer 23 is preferably smaller than the thickness of the oxygen barrier layer 23; the smaller the size, the more advantageous it is. It should be noted that the size of the inorganic particles dispersed in the oxygen barrier layer 23 can be uniform or non-uniform. Specifically, examples of inorganic particles dispersed in the oxygen barrier layer 23 include silica particles, alumina particles, silver particles, copper particles, titanium particles, zirconium dioxide particles, and tin particles.

[0084] The oxygen barrier layer 23 can be stacked on the observer side, above the first adhesive layer 21. Therefore, as... Figure 4 As shown, the oxygen barrier layer 23 can be laminated on the side of the transparent substrate 20 opposite to the side where the first adhesive layer 21 is provided, or it can be laminated between the transparent substrate 20 and the first adhesive layer 21. For example, in the adhesive sheet 15 according to the fifth embodiment, an oxygen barrier layer may be further provided between the transparent substrate 20 and the low refractive index layer 25. Furthermore, in the adhesive sheet 16 according to the sixth embodiment, an oxygen barrier layer may be further provided between the transparent substrate 20 and the anti-glare layer 26. Additionally, in the adhesive sheet 17 according to the seventh embodiment, an oxygen barrier layer may be further provided between the transparent substrate 20 and the low refractive index layer 25. Figures 5-7 In the layer configuration, an oxygen barrier layer may also be provided between the transparent substrate 20 and the first adhesive layer 21 (adhesive layer 30). By further providing an oxygen barrier layer, similar to the fourth embodiment, fading caused by pigment oxidation can be further suppressed.

[0085] <Composition for forming adhesive layer>

[0086] The first adhesive layer 21 described above can be formed by coating an adhesive layer forming composition containing an adhesive, a pigment, additives as needed, and a solvent onto a support such as a release film or a transparent substrate, and then drying it as needed. As the pigment, a first colorant and a second colorant having the above-described absorption properties can be used, and a third colorant having the above-described absorption properties can be further incorporated as needed. As the additive, at least one of a free radical scavenger, a singlet oxygen quencher, and a peroxide decomposer can be used.

[0087] Free radical scavengers capture free radicals generated during pigment oxidation and degradation, inhibiting auto-oxidation and thus suppressing pigment deterioration (fading). When hindered amine light stabilizers with a molecular weight of 2000 or higher are used as free radical scavengers, high fading inhibition effects can be achieved. With lower molecular weight free radical scavengers, they are more volatile, resulting in fewer molecules remaining in the first adhesive layer and making it difficult to achieve sufficient fading inhibition. Suitable materials for use as free radical scavengers include, for example, Chimasorb 2020FDL and Chimasorb 944FDL from BASF, Tinuvin 622, and LA-63P from ADEKA.

[0088] Singlet oxygen quenchers function by inertizing highly reactive singlet oxygen, which readily causes pigment oxidative degradation (fading), thereby inhibiting pigment oxidative degradation (fading). Examples of singlet oxygen quenchers include transition metal complexes, pigments, amines, phenols, and sulfides. Particularly preferred materials are transition metal complexes of dialkyl phosphates, dialkyl dithiocarbamates, or benzene dithiols or similar dithiols. Nickel, copper, or cobalt are preferred as the central metal.

[0089] As a peroxide decomposing agent, it decomposes the peroxides generated during pigment oxidation and deterioration, thereby stopping the auto-oxidation cycle and inhibiting pigment deterioration (fading). Phosphorus-based antioxidants and sulfur-based antioxidants can be used as peroxide decomposing agents.

[0090] Examples of phosphorus-based antioxidants include 2,2'-methylenebis(4,6-di-tert-butyl-1-phenoxy)(2-ethylhexyloxy)phosphine, 3,9-bis(2,6-di-tert-butyl-4-methylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane, and 6-[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propoxy]-2,4,8,10-tetra-tert-butyldibenzo[d,f][1,3,2]dioxaphosphepin, etc.

[0091] Examples of sulfur-based antioxidants include: 2,2-bis({[3-(dodecylthio)propionyl]oxy}methyl)-1,3-propanediyl-bis[3-(dodecylthio)propionate], 2-mercaptobenzimidazole, dilauryl-3,3'-thiodipropionate, dimyristyl-3,3'-thiodipropionate, distearate-3,3'-thiodipropionate, pentaerythritol-tetra(3-laurylthiopropionate), and 2-mercaptobenzimidazole.

[0092] As described above, the adhesive sheets 11-17 of the present invention include a first adhesive layer 21 containing a pigment with visible light absorption properties. A portion of the external light incident on the display device is absorbed by the first adhesive layer 21 during the process of passing through it and entering the display panel, and during the process of being reflected by the display panel and then passing through the first adhesive layer 21 again. Therefore, the intensity of the reflected external light is reduced. This improves the contrast and visibility of the displayed image on the display device. Furthermore, by providing an ultraviolet absorption layer on any layer closer to the viewing side than the first adhesive layer 21, pigment fading can be suppressed, maintaining the display performance of the display device.

[0093] Furthermore, when using the adhesive sheets 11-17 of the present invention, the transmittance of visible light emitted from the display panel can be made 50% or more depending on the selection and amount of pigment, thus without increasing the luminous intensity of the display panel. Compared with conventional configurations using circular polarizers, the brightness of the display device can be improved. Additionally, since it is not necessary to increase the luminous intensity of the display panel to improve brightness, the durability of the display panel can be improved. Furthermore, since the function of blocking visible light using a circular polarizer can be achieved through the thin film of the first adhesive layer 21, the display device can be made thinner compared to the case where a circular polarizer is used.

[0094] It should be noted that an antifouling layer may also be provided on the outermost surface of the adhesive sheet involved in the above embodiments. The antifouling layer improves the antifouling property by imparting hydrophobicity and / or oleophobicity to the optical laminate, and can be formed by dry coating or wet coating of silicon oxides, fluorinated silane compounds, fluoroalkylsilazanes, fluoroalkylsilanes, fluorinated silicon compounds, silane coupling agents containing perfluoropolyether groups, etc.

[0095] Alternatively, an antistatic layer can be provided on the adhesive sheet according to the above embodiments. The antistatic layer can be formed by coating an ionizing radiation-curable material comprising polyester acrylate monomers, epoxy acrylate monomers, urethane acrylate monomers, polyol acrylate monomers, etc., a polymerization initiator, and an antistatic agent, and then curing it by polymerization. As an antistatic agent, for example, antimony-doped tin oxide (ATO), tin-doped indium oxide (ITO), or other metal oxide particles, polymeric conductive compositions, quaternary ammonium salts, etc., can be used. The antistatic layer can be provided on the outermost surface of the optical laminate, or between the optical functional layer and the transparent substrate. Alternatively, the antistatic layer can be formed by incorporating an antistatic agent into any layer constituting the optical functional layer. When an antistatic layer is provided, the surface resistivity is preferably 1.0 × 10⁻⁶. 6 ~1.0×10 12 (Ω / cm).

[0096] Furthermore, in the adhesive sheet according to the fifth embodiment described above, in order to improve the performance of the anti-reflective layer, a medium refractive index layer may be further provided between the high refractive index layer and the transparent substrate. Similarly, in the adhesive sheet according to the seventh embodiment described above, a medium refractive index layer may be further provided between the anti-glare layer and the transparent substrate. In these cases, each layer can be stacked sequentially from the transparent substrate side in the order of medium refractive index layer, high refractive index layer (the layer that functions as the high refractive index layer), and low refractive index layer. The medium refractive index layer can be formed by coating a medium refractive index layer forming composition containing at least an active energy ray curable resin onto the transparent substrate and then curing it. As the active energy ray curable resin used for the low refractive index layer forming composition, the resin described in the high refractive index layer section can be used. In order to adjust the refractive index, metal particles such as zirconium oxide, titanium oxide, niobium oxide, antimony trioxide, antimony pentoxide, tin oxide, indium oxide, indium tin oxide, and zinc oxide can be incorporated into the medium refractive index layer forming composition. Alternatively, the photopolymerization initiator, solvent, and other additives described in the hard coating section may be appropriately incorporated into the composition for forming the intermediate refractive index layer.

[0097] Furthermore, in the adhesive sheets described in the above embodiments, in addition to the high refractive index layer and the anti-glare layer, a hard coating layer may be provided to impart surface hardness. The hard coating layer can be formed by coating a composition containing the active energy ray curable resin described in the high refractive index layer and then curing it.

[0098] Example

[0099] The following describes the embodiments. However, the present invention is not limited to the following embodiments.

[0100] In the following embodiments and comparative examples, adhesive sheets 1 to 16 with the layer structures shown in Tables 1A, 1B, 2A, and 2B were fabricated, and the characteristics of the fabricated adhesive sheets were evaluated. Furthermore, the display device characteristics of the organic EL display panel using the adhesive sheets were confirmed through simulation.

[0101] [Table 1A]

[0102]

[0103] [Table 1B]

[0104]

[0105] [Table 2A]

[0106]

[0107] [Table 2B]

[0108]

[0109] <Making of Adhesive Sheets>

[0110] The formation methods of each layer are explained below.

[0111] (Substrate)

[0112] The following materials are used as transparent substrates.

[0113] • TAC: Triacetyl cellulose membrane (manufactured by FUJIFILM, TG60UL, substrate thickness 60μm, UV blocking rate 92.9%)

[0114] •PMMA1: Polymethyl methacrylate film (manufactured by Sumitomo Chemical Co., Ltd., W001U80, substrate thickness 80μm, UV blocking rate 93.4%)

[0115] •PMMA2: Polymethyl methacrylate film (manufactured by Sumitomo Chemical Co., Ltd., W002N80, substrate thickness 80μm, UV blocking rate 13.9%)

[0116] •PET1: Polyethylene terephthalate film (manufactured by Toyobo Co., Ltd., SRF, substrate thickness 80μm, UV blocking rate 88.3%)

[0117] •PET2: Polyethylene terephthalate film (manufactured by SKC, TOR20, substrate thickness 40μm, UV blocking rate 88.6%)

[0118] (Fabrication of the optical functional layer)

[0119] [Formation of the oxygen barrier layer]

[0120] An 80% aqueous solution of PVA117 (manufactured by KURARAY) was coated onto the transparent substrate of Example 7 shown in Table 1B and allowed to dry, thereby forming an oxygen permeability of 1 cc / m. 2 ·Tian·atm oxygen barrier layer.

[0121] [Formation of hard coating]

[0122] (Composition for forming a hard coating)

[0123] The compositions shown in Table 3 were prepared using the following materials as the materials for the hard coating forming composition.

[0124] • Resins that cure under active energy rays:

[0125] UA-306H (manufactured by Kyoeisha Chemical Co., Ltd., pentaerythritol triacrylate hexamethylene diisocyanate urethane prepolymer)

[0126] DPHA (Dipentaerythritol Hexaacrylate)

[0127] PETA (Pentaerythritol triacrylate)

[0128] • Initiator:

[0129] Omnirad TPO (manufactured by IGM Resins BV)

[0130] Solvent:

[0131] MEK (Methyl Ethyl Ketone)

[0132] Methyl acetate

[0133] [Table 3]

[0134]

[0135] The hard coating composition shown in Table 3 is applied to the transparent substrate or oxygen barrier layer shown in Tables 1A, 1B, 2A, and 2B, dried in an oven at 80°C for 60 seconds, and then irradiated with an ultraviolet light at a linear intensity of 150 mJ / cm². 2 The coating was cured by ultraviolet irradiation (manufactured by Fusion UV System Japan, light source H Bulb), thereby forming the hard coatings 1 and 2 described in Tables 1A, 1B, 2A and 2B with a cured film thickness of 5.0 μm.

[0136] [Formation of a low-refractive-index layer]

[0137] (Composition for forming low refractive index layers)

[0138] The following materials are used as a composition for forming a low-refractive-index layer.

[0139] • Refractive index adjuster:

[0140] Porous silica microparticle dispersion (average particle size 75 nm, solid content 20%, solvent methyl isobutyl ketone) 8.5 parts by weight

[0141] • Antifouling agent:

[0142] OPTOOL AR-110 (manufactured by Daikin Industries, Ltd., 15% solids, solvent methyl isobutyl ketone) 5.6 parts by weight

[0143] • Resins that cure under active energy rays:

[0144] Pentaerythritol triacrylate 0.4 parts by weight

[0145] • Initiator:

[0146] Omnirad 184 (manufactured by IGM Resins BV) 0.07 parts by weight

[0147] Leveling agent:

[0148] RS-77 (manufactured by DIC) 1.7 parts by weight

[0149] Solvent:

[0150] 83.73 parts by weight of methyl isobutyl ketone

[0151] The low refractive index layer forming composition described above was applied to the hard coatings shown in Tables 1A, 1B, 2A, and 2B, dried in an oven at 80°C for 60 seconds, and then irradiated with an ultraviolet light source (Fusion UV Systems Japan, light source H Bulb) at a linear dose of 200 mJ / cm². 2 The coating was cured by ultraviolet irradiation, resulting in a low refractive index layer with a cured film thickness of 100 nm, as shown in Tables 1A, 1B, 2A, and 2B.

[0152] [Formation of the anti-glare layer]

[0153] (Composition for forming an anti-glare layer)

[0154] The compositions shown in Table 4 were prepared using the following materials as the materials for forming the anti-glare layer composition.

[0155] • Resins that cure under active energy rays:

[0156] LIGHT ACRYLATE PE-3A (manufactured by Kyoeisha Chemical Co., Ltd., refractive index 1.52)

[0157] Photopolymerization initiator:

[0158] Omnirad TPO (manufactured by IGM Resins BV)

[0159] • Resin particles:

[0160] Styrene-methyl methacrylate copolymer particles (refractive index 1.515, average particle size 2.0 μm)

[0161] Inorganic particles 1:

[0162] Synthetic montmorillonite

[0163] Inorganic particles 2:

[0164] Alumina nanoparticles, average particle size 40nm

[0165] Solvent

[0166] Toluene

[0167] Isopropanol

[0168] [Table 4]

[0169]

[0170] The anti-glare layer composition shown in Table 4 was coated onto the transparent substrate of Example 12 shown in Table 2A, dried in an oven at 80°C for 60 seconds, and then subjected to ultraviolet irradiation at a linear intensity of 150 mJ / cm. 2 The coating was cured by ultraviolet irradiation (using Fusion UV Systems Japan, with light source H Bulb), resulting in an anti-glare layer of Table 2A with a cured film thickness of 5.0 μm.

[0171] [Formation of the first and second adhesive layers]

[0172] (Preparation of the base adhesive)

[0173] The following composition was used as the base adhesive.

[0174] • Adhesive resin: 70 parts by weight of a butyl acrylate (BA) / hydroxyethyl methacrylate (HEMA) copolymer solution dissolved in ethyl acetate.

[0175] • Curing agent: 0.037 parts by weight of isocyanate-based crosslinking agent

[0176] • Additives: 0.048 parts by weight of silane coupling agent

[0177] Solvent: 30 parts by weight of MEK (methyl ethyl ketone)

[0178] (Composition for forming the first and second adhesive layers)

[0179] The compositions shown in Tables 5A and 5B were prepared using the following materials as the materials for forming the adhesive layers of the first and second adhesive layers. It should be noted that the characteristic values ​​in the adhesive layer were calculated based on the spectral transmittance for the maximum absorption wavelength and half-width of the colorant.

[0180] ·The first color material

[0181] Dye-1 is a pyrrole methylene cobalt complex dye represented by chemical formula 1 (described later) with a maximum absorption wavelength of 493 nm and a half-width at half-maximum of 26 nm.

[0182] ·Second color material:

[0183] Dye-2 is a tetrazaporphyrin copper complex dye (manufactured by Yamamoto Chemical Co., Ltd., PD-311S, maximum absorption wavelength 584nm, half width at half maximum 17nm).

[0184] ·Third color material:

[0185] Dye-3 copper phthalocyanine complex dye (Yamada Chemical Co., Ltd., FDN-002, maximum absorption wavelength 800nm)

[0186] ·additive:

[0187] Hindered amine light stabilizer Chimassorb 944FDL (manufactured by BASF Japan, molecular weight 2000-3100)

[0188] Hindered amine light stabilizer Tinuvin 249 (manufactured by BASF Japan, molecular weight 482)

[0189] Singlet oxygen quencher D1781 (manufactured by Tokyo Chemical Industry Co., Ltd.)

[0190] • Ultraviolet absorber:

[0191] Tinuvin479 (manufactured by BASF Japan, maximum absorption wavelength 322nm)

[0192] LA-36 (manufactured by ADEKA, with maximum absorption wavelengths of 310nm and 350nm)

[0193] • Adhesive: The basic adhesive prepared above

[0194] Solvent: Ethyl acetate

[0195] [Chemistry 1]

[0196] (Chemical Formula 1)

[0197]

[0198] [Table 5A]

[0199]

[0200] [Table 5B]

[0201]

[0202] (Preparation of adhesive layers and adhesive sheets)

[0203] The adhesive obtained as described above is applied to the release substrate film to a film thickness of 25 μm upon drying. After thorough drying, the release film is laminated to obtain the adhesive layer. One release film of the obtained adhesive layer is peeled off and adhered to an alkali-free glass support with a thickness of 0.7 mm. Then, the other release film of the adhesive layer is peeled off and a substrate with the functional layers shown in Tables 1A, 1B, 2A, and 2B is adhered to, thereby obtaining adhesive sheets 1 to 16.

[0204] [Evaluation of Adhesive Patch Properties]

[0205] (UV blocking rate of the layer above the first adhesive layer)

[0206] For the laminates above the first adhesive layer in Examples 1-13 and Comparative Examples 1-3, the transmittance was measured using an automatic spectrophotometer (Hitachi, Ltd., U-4100). The average transmittance in the ultraviolet region (290-400 nm) was calculated using these transmittance values, and the ultraviolet shielding rate shown in Equation (1) was calculated.

[0207] Equation (1)

[0208] Ultraviolet (UV) shielding rate (%) = 100 - Average transmittance (%) in the UV region (290–400 nm)

[0209] (Lightfastness test)

[0210] As a reliability test for the obtained adhesive sheet, a xenon lamp weathering tester (manufactured by Suga Test Instrument Co., Ltd., X75) was used at a xenon lamp illuminance of 60 W / cm². 2 The test was conducted for 120 hours under conditions of 300–400 nm, internal temperature 45 °C, and RH 50%. Transmittance was measured before and after the test using an automatic spectrophotometer (Hitachi, Ltd., U-4100). The transmittance difference ΔTλ1 (representing the minimum transmittance before the test at wavelength λ1 within the wavelength range of 470–530 nm), the transmittance difference ΔTλ2 (representing the minimum transmittance before the test at wavelength λ2 within the wavelength range of 560–620 nm), and the color difference ΔEab under light source C before and after the test were calculated. A transmittance difference and color difference close to zero are considered good, with ΔEab ≤ 5 being preferred.

[0211] The evaluation results of the above projects are shown in Tables 6A, 6B, 7A and 7B.

[0212] [Table 6A]

[0213]

[0214] [Table 6B]

[0215]

[0216] [Table 7A]

[0217]

[0218] [Table 7B]

[0219]

[0220] According to the results in Tables 6A, 6B, 7A, and 7B, the adhesive layer containing the first and second colorants significantly improves lightfastness by having an ultraviolet-absorbing layer with an ultraviolet blocking rate of over 85% on top. The effect is less pronounced when the adhesive layer itself has ultraviolet absorption capacity, requiring the formation of other layers above it. Furthermore, lightfastness is further improved by layering an oxygen barrier layer, including a high-molecular-weight hindered amine light stabilizer as a free radical scavenger within the adhesive layer, and a nickel dialkyl dithiocarbamate complex as a singlet oxygen quencher.

[0221] [Display Device Characteristic Evaluation]

[0222] The following evaluations were performed on the obtained adhesive sheets 6, 11, 13, and 16.

[0223] (White indicates transmission characteristics)

[0224] The transmittance of the obtained adhesive sheet was measured using an automatic spectrophotometer (Hitachi, Ltd., U-4100). This transmittance was used to calculate the efficiency of light passing through the optical film in white display, and this was used to evaluate the white display transmittance characteristics. As a benchmark, [the following will be used]... Figure 8 The efficiency of the white spectrum output from the white organic EL light source and color filter shown is set to 100.

[0225] (Reflective characteristics of display devices)

[0226] The transmittance of the adhesive sheet was measured using an automatic spectrophotometer (Hitachi, Ltd., U-4100). The reflectance of the display panel was set to 40%. The surface reflectance R was set to 1% when the anti-reflective layer, such as the low refractive index layer or anti-glare layer on the adhesive sheet was placed on the outermost layer on the observer side, and the surface reflectance R was set to 4% when no anti-reflective layer was placed. Ignoring the interface reflection and surface reflection in other layers, the relative reflectance value of the display device with a D65 light source set to 100 was calculated based on Equation (2), and this was used to evaluate the reflectance characteristics of the display device.

[0227] [Mathematical Expression 1]

[0228] Equation (2)

[0229]

[0230]

[0231] Here, R is the surface reflectance of the outermost layer on the observer side, T(λ) is the transmittance of the optical film, and P(λ) is the spectrum of the D65 light source. This is the CIE1931 color function.

[0232] (Color reproduction)

[0233] The transmittance of the obtained adhesive sheet was measured using an automatic spectrophotometer (Hitachi, Ltd., U-4100). Figure 8 The spectrum shown is output from a white EL light source and a color filter. Figure 9 The red, green, and blue displays show the spectrum. This is based on the measured transmittance and... Figure 9 The NTSC ratio is calculated based on the CIE1931 chromaticity values ​​obtained from the red, green, and blue display spectra, and is used as an indicator of color reproducibility for evaluation.

[0234] Table 8 shows the white display transmission characteristics, display device reflection characteristics, and color reproduction performance as evaluation criteria for display devices.

[0235] [Table 8]

[0236]

[0237] According to the results in Table 8, the reflectivity of the display device having a colored adhesive layer as the first adhesive layer is significantly reduced. Furthermore, while it is generally believed that the transmittance is halved in a circular polarizer, the brightness efficiency is excellent, as shown in the evaluation values ​​for the transmittance characteristics of white displays, and color reproduction is also improved.

[0238] Industrial applicability

[0239] This invention can be used as an adhesive sheet for optical films used in display devices.

[0240] Explanation of symbols

[0241] 1, 2, 3 Display devices

[0242] 10 Display Panel

[0243] 11, 12, 13, 14, 15, 16, 17 Adhesive sheets

[0244] 20 Transparent substrate

[0245] 21 First adhesive layer

[0246] 22 Second adhesive layer

[0247] 23 Oxygen Barrier Layer

[0248] 24 High Refractive Index Layer

[0249] 25 Low-refractive-index layer

[0250] 26 Anti-glare layer

[0251] 30 Adhesive Layer

Claims

1. An adhesive sheet, characterized in that, have: The first adhesive layer containing adhesive and pigment, and An ultraviolet-absorbing layer is stacked on one side of the first adhesive layer. The pigment contains: The first-color material has a maximum absorption wavelength in the range of 470–530 nm and a half-width of 15–45 nm in its absorption spectrum. The second color material has a maximum absorption wavelength in the range of 560–620 nm and a half-width of 15–55 nm in its absorption spectrum. The ultraviolet-absorbing layer has an ultraviolet shielding rate of over 85% according to JIS L 1925. The first colorant is a pyrrole methylene cobalt complex dye. The first adhesive layer contains a hindered amine light stabilizer with a molecular weight of 2000 or more and a singlet oxygen quencher.

2. The adhesive sheet according to claim 1, characterized in that, The half-width of the absorption spectrum of the first color material is 15–26 nm.

3. The adhesive sheet according to claim 1 or 2, characterized in that, The first adhesive layer contains a peroxide decomposing agent.

4. The adhesive sheet according to claim 1, characterized in that, The singlet oxygen quencher is a dialkyl phosphate, a dialkyl dithiocarbamate, or a benzenethiol or a similar dithiol transition metal complex.

5. The adhesive sheet according to any one of claims 1 to 4, characterized in that, The first adhesive layer further contains a third colorant with a maximum absorption wavelength in the range of 650-800 nm as the pigment.

6. The adhesive sheet according to any one of claims 1 to 5, characterized in that, The pigment contained in the first adhesive layer comprises one or more compounds selected from the group consisting of compounds having any one of the following structures: porphyrin, phthalocyanine, phthalocyanine, azo, phthalocyanine, squartzium, coumarin, polyene, quinone, tetrazaporphyrin, pyrrole methylene, and indigo, as well as their metal complexes.

7. The adhesive sheet according to any one of claims 1 to 6, characterized in that, The ultraviolet absorbing layer is a second adhesive layer containing an adhesive and an ultraviolet absorber.

8. The adhesive sheet according to any one of claims 1 to 6, characterized in that, The ultraviolet absorption layer is a transparent substrate.

9. The adhesive sheet according to any one of claims 1 to 8, characterized in that, On the side closer to the ultraviolet absorbing layer than the first adhesive layer, there is further an oxygen permeability of 10 cc / m 2 Oxygen barrier layer below · atm.

10. The adhesive sheet according to any one of claims 1 to 9, wherein, The ultraviolet absorption layer is further provided with an anti-glare layer or an anti-reflection layer containing a high refractive index layer and a low refractive index layer as an optical functional layer to reduce the reflection of incident external light.

11. The adhesive sheet according to any one of claims 1 to 10, characterized in that, It further includes an antistatic layer or an antifouling layer.

12. A display device comprising an adhesive sheet according to any one of claims 1 to 11.

13. A composition for forming an adhesive layer, characterized in that, It contains adhesives, pigments, and additives. The pigment contains: The first color material with a maximum absorption wavelength in the range of 470–530 nm and a half-width of 15–45 nm in its absorption spectrum, and A second color material with a maximum absorption wavelength in the range of 560–620 nm and a half-width of 15–55 nm in its absorption spectrum. The first colorant is a pyrrole methylene cobalt complex dye. The additive contains hindered amine light stabilizers with a molecular weight of 2000 or higher and singlet oxygen quenchers.

Citation Information

Patent Citations

  • Organic el display device and organic el display device polarization element

    JP2013251376A

  • Absorber for visible light in the short wavelength range and ultraviolet rays

    JP2018193538A

  • Display optical filter and display having the same