A method for preparing high-bet and high-structure white carbon black based on precipitation method

By combining a step-by-step precipitation method with surfactants and controlling the reaction conditions, high BET and high structured silica were prepared, solving the problems of low specific surface area and poor structured structure in traditional precipitation methods and improving the reinforcing properties of rubber.

CN116715247BActive Publication Date: 2026-11-20CHANGZHOU UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310533503.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-12
Publication Date
2026-11-20
Estimated Expiration
2043-05-12

AI Technical Summary

Technical Problem

Silica prepared by traditional precipitation methods has a low specific surface area and poor structure, resulting in poor dispersibility and reinforcing effect in rubber, which makes it difficult to meet the requirements of the tire industry.

Method used

A step-precipitation method was adopted, and by controlling the reaction temperature, time and the amount of surfactant added, combined with surfactants such as sodium dodecylbenzenesulfonate, the reaction pH value was adjusted to form silica with high BET and high structure.

Benefits of technology

It significantly improves the specific surface area and structure of silica, enhances the processing and mechanical properties of rubber, and improves the reinforcing effect of rubber.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116715247B_ABST
    Figure CN116715247B_ABST
Patent Text Reader

Abstract

The present application belongs to the field of inorganic material preparation, and particularly relates to a preparation method of high-BET and high-structure white carbon black based on a precipitation method. The high-BET and high-structure white carbon black used for reinforcing butadiene styrene rubber is prepared by using a ladder precipitation method, with water glass and dilute sulfuric acid as raw materials and sodium dodecyl benzene sulfonate as a dispersant. The white carbon black prepared by the process has typical characteristics of high specific surface area and high structure. When used for reinforcing butadiene styrene rubber, the white carbon black shows excellent processing performance and mechanical strength. Compared with the same kind of commercially available high-quality white carbon black prepared by a precipitation method, the tensile strength, 300% elongation and 500% elongation are all significantly improved. The method is simple in process and easy to realize industrialization.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of inorganic material preparation, specifically relating to a method for preparing high BET and high structure silica based on precipitation method. Background Technology

[0002] Silica is an amorphous powder with various properties such as porosity, high dispersibility, and high temperature resistance. Due to its excellent physical and chemical properties, silica is widely used as a rubber reinforcing agent. Rubber reinforced with silica exhibits significantly improved physical properties, tear resistance, fatigue resistance, and abrasion resistance. In addition, silica is widely used in industries such as cement, composite materials, papermaking, and pharmaceuticals. Silica prepared by traditional precipitation processes has a low specific surface area (BET), numerous surface hydroxyl groups, poor structure, and severe agglomeration. When used to reinforce styrene-butadiene rubber (SBR), its poor dispersibility in the rubber reduces its reinforcing effect. How to improve the specific surface area of ​​silica while simultaneously increasing its structure to meet the requirements of the tire industry has become a hot topic in recent years.

[0003] CN106044790A discloses a method for preparing silica by precipitation, comprising the following steps: (1) adding n-butanol aqueous solution and sodium chloride to a reactor, then adding water glass solution, then adding cationic surfactant, stirring, heating, and then continuing to add water glass solution, ammonium chloride aqueous solution and hydrochloric acid to the reactor in a continuous co-current manner; (2) controlling the pH value of the reaction to 8-9 until the water glass solution is completely added; (3) adding ammonium chloride aqueous solution and hydrochloric acid, adjusting the pH value to 4-5, aging for 2 hours to obtain a slurry; (4) filtering the slurry, washing with water and then washing with ethanol; (5) crushing the filter cake, drying it by microwave, and calcining it to obtain silica. The silica prepared by the above method has an oil absorption value of 2.85-2.95 mL / g and a BET specific surface area of ​​204-211 m². 2 The amount of waste liquid generated is between / g and the amount of waste liquid generated is too large and difficult to handle. Summary of the Invention

[0004] The present invention aims to provide a method for preparing high-BET and high-structure silica. This method employs a stepwise precipitation process, improving particle formation conditions by adding appropriate amounts of surfactants such as polyethylene glycol 4000, hexadecyltrimethylammonium bromide, sodium dodecylbenzenesulfonate, and cocamidopropyl betaine. Simultaneously, by adjusting the reaction temperature, reaction time, and surfactant dosage, high BET and high structure of the silica are effectively achieved. When applied to the reinforcement of styrene-butadiene rubber (SBR), this method significantly improves the processing and mechanical properties of the rubber.

[0005] Based on the above objectives, the present invention adopts the following technical solution.

[0006] A method for preparing high-BET and high-structure silica based on precipitation includes the following steps: silica is prepared using a stepwise precipitation method. Step A: A certain amount of water glass solution and surfactant are added to a reaction vessel as the base liquid. After heating to a certain temperature, sulfuric acid is added to the reaction vessel at a constant rate using a peristaltic pump until the pH of the reaction system reaches a certain value. Step B: Water glass solution and dilute sulfuric acid are added dropwise using two peristaltic pumps simultaneously, maintaining a constant pH value throughout the process. After the addition is complete, the pH value of the system is adjusted to 4. The mixture is then filtered, washed with water to remove salt, extracted with industrial ethanol, filtered, dried, ground, and sieved to obtain high-BET and high-structure high-performance silica.

[0007] The concentration of the water glass solution is 0.3–0.5 mol / L; the mass fraction of the dilute sulfuric acid is 10.0%; the reaction temperature is 70–85℃; the total reaction time is 100 min; the amount of surfactant added is 0.5–2.0% (based on the mass fraction of water glass solution added to the base solution); and the reaction pH is 9.5–10.5.

[0008] Preferred parameters: 10.0% dilute sulfuric acid, 80°C reaction temperature, 100 min total reaction time, sodium dodecylbenzenesulfonate as surfactant, 1.5% added (based on the mass fraction of water glass solution added to the base solution), and pH value of the reaction is 10.0–10.5.

[0009] Silica was prepared by a stepwise precipitation method, wherein the amount of A-stage water glass added was 17.5% of the total amount and the amount of B-stage water glass added was 82.5% of the total amount.

[0010] Compared with the prior art, the present invention has the following beneficial effects:

[0011] (1) This invention uses a step-by-step precipitation method, which makes it easier to maintain the pH value of the reaction system within a relatively stable range. Traditional processes result in unstable pH values ​​in the reaction system, with significant fluctuations. If the reaction pH is too high, the silicate particles in the reaction system gel at a faster rate, resulting in poorly structured silica; if the reaction pH is too low, the silicate particles gel at a slower rate, leading to Oswald curing. system Smaller sol particles dissolve and redeposit onto larger sol particles, resulting in a poorly developed pore structure in the generated silica. However, through stepwise precipitation, the pH of the reaction system is maintained within a relatively stable range, allowing the silica particles in the reaction system to gel at an appropriate rate, thereby obtaining silica with high BET and high structural density.

[0012] (2) In this invention, sodium dodecylbenzenesulfonate, a surfactant, is used as a dispersant. By affecting the Stern layer (electric double layer) on the surface of silica particles, the electrostatic repulsion between sol particles is increased, thereby affecting the gelation of silica particles and improving the dispersibility and structure of silica.

[0013] (3) The high BET silica prepared by this invention has a specific surface area of ​​up to 309 m². 2 With an oil absorption value of over 4.72 mL / g, when mixed with styrene-butadiene rubber, it can significantly improve the mechanical properties of the reinforcing rubber while maintaining excellent processing performance and vulcanization time. Attached image description:

[0014] Figure 1 The particle size distribution diagram shows the silica prepared in the embodiments and comparative examples of this invention. Detailed Implementation

[0015] This invention is not limited to the specific embodiments listed below. Those skilled in the art can implement this invention using various other specific embodiments based on the content disclosed herein. Any modifications or alterations made to the design structure and concept of this invention fall within the protection scope of this invention. It should be noted that, unless otherwise specified, the embodiments and features described in this invention can be combined with each other.

[0016] The following detailed description is provided in conjunction with specific examples:

[0017] In the following embodiments, the testing methods for each performance parameter are as follows:

[0018] (1) Measurement of specific surface area (BET):

[0019] The procedure was performed according to HG / T 3073-1999. The specific surface area of ​​the silica sample was calculated using the liquid nitrogen adsorption method, based on the theoretical calculation model proposed by Brunauer, Emmett, and Teller, and the unit is m². 2 / g.

[0020] (2) Determination of oil absorption value (DBP):

[0021] Perform according to HG / T 3072-2008. The amount of dibutyl phthalate (DBP) absorbed by 1g of silica is expressed as the volume of DBP, in mL / g.

[0022] (3) Determination of particle size distribution:

[0023] The procedure was performed according to GB / T 32698-2016. 50 mL of distilled water was measured using a graduated cylinder, and 0.5 g of high-temperature dried silica sample was added. After stirring thoroughly, the silica was ultrasonically dispersed for 7 min at 600 W using an ultrasonic disperser. The ultrasonically dispersed silica suspension was then immediately poured into the circulation pump of a laser particle size analyzer to determine the particle size distribution of the silica.

[0024] (4) Rubber mixing step:

[0025] The rubber compound was prepared according to HG / T2404-2008 "Identification of Precipitated Hydrated Silica in Styrene-Butadiene Rubber", with the following formula: 200g styrene-butadiene rubber, 100g silica, 10g ZnO, 2g stearic acid, 6g polyethylene glycol, 2.4g accelerator DM, 1.4g accelerator M, 1g accelerator DPG, and 4g sulfur. The silica-styrene-butadiene rubber compound was then vulcanized at 160℃ using a flat vulcanizing press.

[0026] (5) Performance testing of the compound:

[0027] The Mooney viscosity of rubber was tested according to GB / T1232-2016 "Determination of unvulcanized rubber using a disc shear viscometer - Part 1: Determination of Mooney viscosity".

[0028] The vulcanization characteristics of rubber were tested according to GB / T9869-1997 "Determination of vulcanization characteristics of rubber compounds (disc oscillating vulcanizer method)".

[0029] The stress-strain characteristics were tested according to GB / T528-2009 "Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber".

[0030] Example 1

[0031] 870 mL of a 0.45 mol / L water glass solution was added to a reactor as the base solution (17.5% of the total water glass added), along with 1.5% (approximately 13.5 g by mass fraction of the water glass solution added to the base solution) of sodium dodecylbenzenesulfonate. The mixture was stirred and heated to 80°C. A certain amount of 10.0% dilute sulfuric acid was added to the reactor at a constant rate using a peristaltic pump until the pH of the reaction system reached 10.0. Then, water glass solution (82.5% of the total water glass added) and dilute sulfuric acid were simultaneously added dropwise to the reactor using two peristaltic pumps, maintaining a constant pH. After the addition was complete, the pH of the system was adjusted to 4, and the total reaction time was controlled to 100 min. The mixture was filtered, washed with water to remove salt, extracted with industrial ethanol, filtered, dried, ground, and sieved to obtain high-BET and high-structure high-performance silica.

[0032] Example 2

[0033] This embodiment provides a method for preparing high-performance silica with ultra-high BET and high structure. Except that the amount of sodium dodecylbenzenesulfonate added in the step is 0.5% (based on the mass fraction of water glass solution added to the bottom solution), the rest is the same as in Example 1.

[0034] Example 3

[0035] This embodiment provides a method for preparing high-performance silica with high BET and high structure. Except that the amount of sodium dodecylbenzenesulfonate added in the step is 2.0% (based on the mass fraction of water glass solution added to the base liquid), the rest is the same as in Example 1.

[0036] Example 4

[0037] This embodiment provides a method for preparing high-performance silica with high BET and high structure. Except for adjusting the reaction pH value in the steps to 10.5, the rest is the same as in Example 1.

[0038] Example 5

[0039] This embodiment provides a method for preparing high-performance silica with high BET and high structure. Except for adjusting the reaction pH value to 9.5 in the steps, the rest is the same as in Example 1.

[0040] Example 6

[0041] This embodiment provides a method for preparing high-performance silica with high BET and high structure. Except for replacing the surfactant in the steps with polyethylene glycol 4000 and adding it at a rate of 1.0% (based on the mass fraction of water glass solution added to the base solution), the rest is the same as in Example 1.

[0042] Example 7

[0043] This embodiment provides a method for preparing high-performance silica with high BET and high structure. Except for replacing the surfactant mentioned in the steps with hexadecyltrimethylammonium bromide and adding it at 1.0% (based on the mass fraction of water glass solution added to the base solution), the rest is the same as in Example 1.

[0044] Example 8

[0045] This embodiment provides a method for preparing high-performance silica with high BET and high structure. Except for replacing the surfactant in the steps with cocamidopropyl betaine and adding it at 1.0% (based on the mass fraction of water glass solution added to the base solution), the rest is the same as in Example 1.

[0046] Comparative Example 1

[0047] This embodiment provides a method for preparing silica, except that the step precipitation is replaced with a single precipitation in the traditional process, and the rest is the same as in Example 1.

[0048] Water glass solution and 13.5g of sodium dodecylbenzenesulfonate were added to a reaction vessel. After stirring and heating to 80°C, a certain amount of 10.0% dilute sulfuric acid was added to the reaction vessel at a uniform rate using a peristaltic pump, controlling the total reaction time to 100min. After the addition was completed, the pH of the system was adjusted to 4. The mixture was then filtered, washed with water to remove salt, extracted with industrial ethanol, filtered, dried, ground, and sieved to obtain the silica product.

[0049] Comparative Example 2

[0050] This embodiment provides a method for preparing silica without the addition of surfactants; all other aspects are the same as in Example 1.

[0051] 870 mL of a 0.45 mol / L water glass solution (17.5% of the total water glass added, calculated as SiO2) was added to a reaction vessel and heated to 80 °C with stirring. A certain amount of 10.0% dilute sulfuric acid was added to the reaction vessel at a uniform rate using a peristaltic pump until the pH of the reaction system reached 10.0. Then, water glass solution (82.5% of the total water glass added) and dilute sulfuric acid were simultaneously added dropwise to the reaction vessel using two peristaltic pumps, maintaining a constant pH. After the addition was completed, the pH of the system was adjusted to 4, and the total reaction time was controlled to 100 min. The solution was filtered, washed with water to remove salt, extracted with industrial ethanol, filtered, dried, ground, and sieved to obtain the silica product.

[0052] Table 1 shows the comparison of the performance indicators of the silica in the above embodiments and comparative examples with those of similar commercially available high-BET silica products at home and abroad.

[0053] Table 1. Performance comparison of each example, comparative example, and commercially available silica.

[0054] product <![CDATA[BET(m 2 / g)]]> DBP (mL / g) <![CDATA[D 50 (one)]]> Example 1 309 4.72 0.43 Example 2 305 4.60 0.48 Example 3 286 4.46 0.55 Example 4 310 4.60 0.43 Example 5 192 4.46 2.4 Example 6 163 4.62 0.50 Example 7 176 4.60 0.58 Example 8 273 4.58 0.81 Comparative Example 1 286 4.20 3.8 Comparative Example 2 304 4.26 0.49 Domestic silica (930GR model) 236 2.40 1.6 Imported silica (WK62 grade) 243 2.00 1.7

[0055] As shown in Table 1, compared with commercially available high-BET silica based on precipitation method, the silica provided in Examples 1, 2, and 4 have significant advantages in specific surface area and structure. Meanwhile, the median diameter D... 50 It also decreased significantly, and the dispersion improved markedly.

[0056] As can be seen from the comparison between Example 1 and Comparative Example 1, when the preparation process is changed from single precipitation to step precipitation, the defect of unstable pH in the reaction system can be avoided, and the reaction pH can be kept in a stable range, so as to control the polymerization rate of silica sol. The prepared silica has a significant improvement in specific surface area and structure.

[0057] A comparison of Examples 1, 4, and 5 shows that when the reaction pH is too low, the specific surface area of ​​silica will be severely reduced, while when the reaction pH is too high, the structure of silica will be affected.

[0058] The comparison of Examples 6-8 shows that the different types of hydrophilic groups in surfactants have different effects on the specific surface area and structure of silica. Sodium dodecylbenzenesulfonate can effectively improve the structure of silica while increasing its specific surface area.

[0059] The rubber compounding performance of the above representative examples and comparative examples of silica was tested and compared with commercially available high-BET silica from domestic and foreign markets. The test results are shown in Table 2.

[0060] Table 2. Test results of precipitated silica prepared from each example, comparative example, and commercially available precipitated silica.

[0061]

[0062] As shown in Table 2, compared with commercially available high-BET silica, the silica prepared by this invention has significant advantages in the mechanical properties of reinforcing rubber, mainly reflected in the significant improvement in tensile strength, 300% elongation stress, and 500% elongation stress. Taking Example 1 as an example, compared with the traditional one-step precipitation method, the processing performance is significantly improved, the vulcanization time is shortened by 10.9%, and the mechanical properties are also significantly improved. Tensile strength increased by 11.6%, 300% elongation increased by 3.8%, and 500% elongation increased by 10.7%. Compared with commercially available high-quality silica in China, tensile strength increased by 12.3%, 300% elongation increased by 12.5%, and 500% elongation increased by 22.9%. Compared with commercially available high-quality silica abroad, tensile strength increased by 7.0%, 300% elongation increased by 22.7%, and 500% elongation increased by 28.8%.

[0063] Based on the above-described preferred embodiments of the present invention, and through the foregoing description, those skilled in the art can make various changes and modifications without departing from the inventive concept. The technical scope of this invention is not limited to the contents of the specification, but must be determined according to the scope of the claims.

Claims

1. A method for preparing high-BET and high-structure silica based on precipitation method, characterized in that: The step-by-step precipitation method includes the following steps: Step A: Water glass solution and dispersant are added to the reactor as the base liquid. After heating to the reaction temperature, 10.0% dilute sulfuric acid is added at a uniform rate to control the pH of the reaction system to 10.0-10.

5. The dispersant is sodium dodecylbenzenesulfonate. Step B: Water glass solution and 10.0% dilute sulfuric acid were added dropwise at a uniform rate while keeping the pH constant. After the addition was completed, the pH of the system was adjusted to 4, and the total reaction time was controlled to be 100 min. The mixture was washed, filtered, dried, ground, and sieved to obtain silica with high BET and high structure. The amount of water glass added is 17.5% of the total amount for Class A and 82.5% of the total amount for Class B.

2. The method for preparing high BET and high structure silica according to claim 1, characterized in that: The reaction temperature is 70–85℃, and the amount of dispersant added is 0.5–2.0% based on the mass fraction of the water glass solution added to the base liquid.

3. The method for preparing high BET and high structure silica according to claim 2, characterized in that: The reaction temperature is 80℃.

4. The method for preparing high BET and high structure silica according to claim 2, characterized in that: The amount of sodium dodecylbenzenesulfonate added is 1.5%.

5. The method for preparing high BET and high structure silica according to claim 1, characterized in that: The pH value of the reaction system is 10.0.

Citation Information

Patent Citations

  • Method for preparing white carbon black with precipitation method

    CN106044790A

  • Low hydroxyl content white carbon black and preparation method thereof

    CN106986348A

  • Method for preparing high-structure-dimension and high-reinforcing white carbon black and white carbon black obtained by same

    CN108101068A

  • Preparation method of high-structure degree, high-specific surface area and high-dispersion white carbon black

    CN110156033A