A heating method for relieving high carbon steel center carbon segregation

By using a controllable temperature slow cooling device and heating regime in the production of high carbon steel, the problem of uneven microstructure in high carbon steel products is alleviated, thus achieving high-quality product stability.

CN116716467BActive Publication Date: 2026-11-24BAOTOU IRON & STEEL (GROUP) CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310649590.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-02
Publication Date
2026-11-24
Estimated Expiration
2043-06-02

AI Technical Summary

Technical Problem

High-carbon steel is prone to central carbon segregation during production, resulting in uneven microstructure of finished hot-rolled wire rods and affecting product quality stability. Existing technologies are unable to effectively control the distribution of carbon elements.

Method used

A temperature-controlled slow cooling device and a controllable heating furnace time and temperature are used to slowly cool the billet and adjust the heating time and temperature according to the cross-section of the billet. Combined with the secondary heating system of the billet, the central carbon segregation is reduced.

Benefits of technology

The macroscopic segregation of hypereutectoid steel is effectively controlled, with the center segregation index optimally below 1.03, thus improving the stability of product quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116716467B_ABST
    Figure CN116716467B_ABST
Patent Text Reader

Abstract

This invention discloses a heating method to alleviate central carbon segregation in high-carbon steel. After the billet produced by continuous casting exits the production line, it enters a temperature-controlled slow cooling device. The heating time and temperature are determined based on the billet's cross-section for slow cooling, and the temperature after exiting the slow cooling device is controlled. Then, the billet undergoes secondary heating, similarly based on the billet's cross-section. The purpose of this invention is to provide a heating method to alleviate central carbon segregation in high-carbon steel by adding a slow cooling device and controlling the heating furnace time and temperature to reduce central carbon segregation in hypereutectoid steel.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of steelmaking continuous casting process, and in particular to a heating method for alleviating carbon segregation in the center of high-carbon steel. Background Technology

[0002] Hypereutectoid steel with a carbon content greater than 0.77% is a primary raw material for high-strength, high-toughness, low-relaxation prestressed steel wire or strand. It is mainly used in important construction projects such as viaducts, long-span bridges, high-rise buildings, dams, nuclear power plants, and tunnels. Therefore, wire rod manufacturers have very strict requirements for its raw materials. Due to the high carbon content and low distribution coefficient in high-carbon steel, it is prone to segregation, which significantly affects its composition and microstructure. When the central carbon segregation index is too high, even rapid cooling during rolling cannot prevent the formation of a central network of cementite. The uneven carbon distribution caused by segregation is inherited by the finished product, affecting the microstructure of hot-rolled wire rods and their use in drawing. Therefore, the uneven distribution of carbon along the drawing direction severely restricts the product quality stability. Controlling carbon segregation in continuously cast billets is a key focus in the production of hypereutectoid steel. To address this, a production method to alleviate central carbon segregation in hypereutectoid steel is proposed. Summary of the Invention

[0003] The purpose of this invention is to provide a heating method to alleviate central carbon segregation in high-carbon steel by adding a slow cooling device and controlling the time and temperature of the heating furnace to slow down central carbon segregation in hypereutectoid steel.

[0004] To solve the above-mentioned technical problems, the present invention adopts the following technical solution:

[0005] This invention discloses a heating method for alleviating carbon segregation in the center of high-carbon steel. After the billet produced by continuous casting comes off the production line, it enters a temperature-controlled slow cooling device. The heating time and temperature are determined according to the billet cross-section for slow cooling, and the temperature after exiting the slow cooling device is controlled. Then, the billet is reheated, and the heating regime is determined according to the billet cross-section.

[0006] Furthermore, specifically including:

[0007] 1) Temperature-controlled slow cooling device

[0008] A controllable temperature slow cooling device that uses gas heating to increase the slow cooling temperature of the billet;

[0009] The temperature-controlled slow cooling device mainly includes:

[0010] (1) The slow cooling pit body is made of steel structure frame and lined with high temperature rock wool. The high temperature rock wool is required to withstand a high temperature of more than 1200℃. The slow cooling pit is a sealed device with a top cover design. The billet is lifted in and out by a crane.

[0011] (2) Heating system: The internal mixing burners are evenly distributed on the four walls of the slow cooling pit. Automatic ignition design is used. Inspection holes are installed on the four walls of the slow cooling pit to visually inspect the situation inside the slow cooling pit. A fan-assisted smoke exhaust system is used to heat the cold air to improve thermal efficiency.

[0012] (3) The control system adopts an automatic temperature control design. After the temperature control curve is preset, it is controlled by thermocouples and PLC system installed on the wall of the slow cooling pit.

[0013] 2) Temperature-controlled slow cooling process

[0014] The temperature and slow cooling time for different cross sections are determined based on the temperature at which carbon diffuses in iron.

[0015] The billet is immediately placed in a slow cooling pit after it comes off the production line, and the temperature of the billet after it comes off the production line is 500-550℃.

[0016] 150mm×150mm cross-section temperature-controlled slow cooling process: Heat to 950℃ and stop heating, keep warm for 48 hours, then open the cover for slow cooling, and exit the slow cooling device when the temperature reaches below 400℃.

[0017] 160mm×160mm cross-section temperature-controlled slow cooling process: Heat to 950℃ and stop heating, keep warm for 56 hours, then open the cover for slow cooling, and exit the slow cooling device when the temperature reaches below 400℃.

[0018] 240mm×240mm cross-section temperature control slow cooling process: Heat to 950℃ and stop heating, keep warm for 64 hours, then open the cover for slow cooling, and exit the slow cooling device when the temperature reaches below 400℃.

[0019] 280mm×380mm cross-section temperature-controlled slow cooling process: heating is stopped at 950℃, and the temperature is held for 72 hours. After holding for 72 hours, the lid is opened for slow cooling. When the temperature of the billet reaches below 400℃ after cooling, it is removed from the slow cooling device.

[0020] 3) Secondary heating system for cast billets

[0021] After slow cooling, the billet enters the rolling line for rolling. The temperature in the preheating section of the furnace is controlled below 600℃, the temperature in the heating section is controlled between 980 and 1200℃, and the billet exiting the furnace is 1050 to 1150℃. The holding time is set differently depending on the cross-section, with varying heating time and total furnace time.

[0022] 150mm×150mm cross-section, heating time 40min, total furnace time 2h;

[0023] 160mm×160mm cross-section, heating time 1 hour, total furnace time 2 hours and 30 minutes;

[0024] 240mm×240mm, heating time 1 hour 30 minutes, total furnace time 3 hours;

[0025] 280mm×380mm cross-section, heating time 2h30min, total furnace time 3h30min.

[0026] Furthermore, the chemical composition of the high-carbon steel by mass percentage is C: 0.79%–0.95%, Si: 0.15%–0.90%, Mn: 0.60%–1.00%, P≤0.010%, S≤0.010%, V: 0.01%–0.05%, Cr: 0.15%–0.45%, with the remainder being Fe and unavoidable impurities.

[0027] Compared with the prior art, the beneficial technical effects of the present invention are as follows:

[0028] Through the implementation of this invention, the macrosegregation control of hypereutectoid steel is optimal, the overall segregation evaluation is best, and the center segregation index is optimally within 1.03. Attached Figure Description

[0029] The present invention will be further described below with reference to the accompanying drawings.

[0030] Figure 1 This is a map showing the location of the points. Detailed Implementation

[0031] The chemical composition of the hypereutectoid steel in this example is as described above. The process route is: hot metal pretreatment—converter—refining—continuous casting. The key points are the temperature of the continuously cast billet entering the slow cooling device and the subsequent heating temperature and time. In this specific example, the billet cross-section is 150mm × 150mm. After selecting a controllable temperature slow cooling device and choosing the appropriate temperature and time, the slow cooling process was finally determined: the billet enters the slow cooling device at a temperature of 503–520℃, is heated to 950℃ and then stopped, held at that temperature for 48 hours, and then slowly cooled until it reaches below 400℃ before exiting the slow cooling device. The secondary heating process for the billet involves controlling the furnace time to 2 hours, 1.5 hours, and 1 hour, with a heating temperature of 1130–1150℃, and an exit temperature of 1080–1123℃. After exiting the furnace, the macroscopic carbon segregation of the billet is inspected, and the inspection points are as follows... Figure 1 As shown in Table 1, the specific test values ​​show that when the furnace time is 1 hour and 1 hour 30 minutes, the carbon element in the core does not diffuse; when the furnace time exceeds 2 hours, the carbon element in the center diffuses evenly, and the carbon segregation is controlled optimally. Finally, the total furnace time for the 150mm×150mm cross-section billet was determined to be 2 hours.

[0032] Table 1. Test results of carbon content at different locations

[0033]

[0034] Note: The carbon content of the steel smelting composition in this furnace is 0.82%.

[0035] #1 — Furnace time: 1 hour;

[0036] #2 — Furnace time: 1 hour and 30 minutes;

[0037] #3 — Furnace time: 2 hours.

[0038] Through the implementation of this invention patent, the macrosegregation control of hypereutectoid steel is optimal, the overall segregation evaluation is best, and the center segregation index is optimally within 1.03.

[0039] The embodiments described above are merely preferred embodiments of the present invention and are not intended to limit the scope of the present invention. Various modifications and improvements made by those skilled in the art to the technical solutions of the present invention without departing from the spirit of the present invention should fall within the protection scope defined by the claims of the present invention.

Claims

1. A heating method for mitigating carbon segregation in the center of high-carbon steel, characterized in that, After the billet produced by continuous casting comes off the production line, it enters a temperature-controlled slow cooling device. The heating time and temperature are determined according to the billet cross-section for slow cooling, and the temperature after exiting the slow cooling device is controlled. Then the billet is heated a second time, and the heating regime is determined according to the cross-section of the billet. Specifically, it includes: 1) Temperature-controlled slow cooling device A controllable temperature slow cooling device that uses gas heating to increase the slow cooling temperature of the billet; The temperature-controlled slow cooling device mainly includes: (1) The slow cooling pit body adopts a steel structure frame and is lined with high-temperature rock wool. The high-temperature rock wool is required to withstand a high temperature of more than 1200℃. The slow cooling pit is a sealed device with a top opening design. A crane is used to lift the billet in and out. (2) Heating system: The internal mixing burners are evenly distributed on the four walls of the slow cooling pit. Automatic ignition design is used. Inspection holes are installed on the four walls of the slow cooling pit to visually inspect the situation inside the slow cooling pit. A fan-assisted smoke exhaust system is used to heat the cold air to improve thermal efficiency. (3) The control system adopts an automatic temperature control design. After the temperature control curve is preset, it is controlled by thermocouples and PLC system installed on the wall of the slow cooling pit. 2) Temperature-controlled slow cooling process The temperature and slow cooling time for different cross sections are determined based on the temperature at which carbon diffuses in iron. The billet is immediately placed in a slow cooling pit after it comes off the production line, and the temperature of the billet after it comes off the production line is 500-550℃. 150mm×150mm cross-section temperature-controlled slow cooling process: Heat to 950℃ and stop heating, keep warm for 48 hours, then open the cover for slow cooling, and exit the slow cooling device when the temperature reaches below 400℃. 160mm×160mm cross-section temperature-controlled slow cooling process: Heat to 950℃ and stop heating, keep warm for 56 hours, then open the cover for slow cooling, and exit the slow cooling device when the temperature reaches below 400℃. 240mm×240mm cross-section temperature control slow cooling process: Heat to 950℃ and stop heating, keep warm for 64 hours, then open the cover for slow cooling, and exit the slow cooling device when the temperature reaches below 400℃. 280mm×380mm cross-section temperature-controlled slow cooling process: heating is stopped at 950℃, and the temperature is held for 72 hours. After holding for 72 hours, the lid is opened for slow cooling. When the temperature of the billet reaches below 400℃ after cooling, it is removed from the slow cooling device. 3) Secondary heating system for cast billets After slow cooling, the billet enters the rolling line for rolling. The temperature in the preheating section of the furnace is controlled below 600℃, the temperature in the heating section is controlled between 980 and 1200℃, and the billet exiting the furnace is 1050 to 1150℃. The holding time is set differently depending on the cross-section, with varying heating time and total furnace time. 150mm×150mm cross-section, heating time 40min, total furnace time 2h; 160mm×160mm cross-section, heating time 1 hour, total furnace time 2 hours and 30 minutes; 240mm×240mm, heating time 1 hour 30 minutes, total furnace time 3 hours; 280mm×380mm cross section, heating time 2h30min, total furnace time 3h30min.

2. The heating method for mitigating central carbon segregation in high-carbon steel according to claim 1, characterized in that, The chemical composition of the high-carbon steel by mass percentage is: C: 0.79%–0.95%, Si: 0.15%–0.90%, Mn: 0.60%–1.00%, P≤0.010%, S≤0.010%, V: 0.01%–0.05%, Cr: 0.15%–0.45%, with the remainder being Fe and unavoidable impurities.

Citation Information

Patent Citations

  • B2 ultra-low carbon segregation index control method for high-grade mine mill ball

    CN105132787A

  • Production process for improving flaw detection quality of billet-rolled thick plate without dehydrogenation

    CN108165703A