Composite foam and method for manufacturing the same, electronic device
By dividing the thickness direction and preparing the graphene composite foam, the problems of low thermal conductivity and poor buffering and shock absorption of high-power devices in electronic devices are solved, achieving efficient heat dissipation and protection, reducing the temperature of electronic devices and simplifying the processing technology.
Patent Information
- Application Number
- CN202310572918.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-19
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-05-19
AI Technical Summary
High-power devices in existing electronic devices have low thermal conductivity, resulting in excessively high local temperatures and limited buffering and shock absorption effects. Existing material processing technology is complex and costly.
Graphene composite foam is used, which is divided into a first part and a second part along the thickness direction. The first part has high expansion and good compression resilience, while the second part has low expansion and high thermal conductivity. The composite foam is prepared by preparing a slurry containing graphene oxide, foaming pre-expansion treatment and carbonization graphitization treatment.
It achieves excellent buffering, shock absorption, and heat dissipation performance, reduces the temperature of electronic devices, simplifies the manufacturing process, and lowers costs.
Smart Images

Figure CN116717556B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of heat dissipation materials technology, and in particular to composite foam and its preparation method, and electronic devices. Background Technology
[0002] With the current trend towards lightweighting and highly integrated electronic devices, including high-power components (such as camera lenses, chips, batteries, and RF modules), current integration solutions often employ conductive cloth and polymer foam products. However, these materials have low thermal conductivity, leading to overheating in localized areas of the camera and limited cushioning and shock absorption, failing to provide adequate protection. To achieve heat dissipation and cushioning, existing technologies typically employ a multi-layered structure of foam and thermally conductive materials bonded together with adhesives. This process is complex and costly. Summary of the Invention
[0003] The purpose of this application is to provide a composite foam and its preparation method, as well as an electronic device. The composite foam has both excellent heat dissipation and cushioning performance, which is beneficial to the miniaturization and weight reduction of electronic devices.
[0004] In a first aspect, this application provides a composite foam comprising graphene, wherein the composite foam is divided into a first part and a second part along the thickness direction, the compression resilience of the first part is greater than that of the second part, the thermal conductivity of the first part is less than that of the second part, and the thermal conductivity includes at least one of horizontal thermal conductivity and vertical thermal conductivity.
[0005] In some embodiments, the thickness ratio of the first portion to the second portion is (1-3):1.
[0006] In some implementations, the compression rebound rate of the first portion is P1, where P1 > 90.
[0007] In some embodiments, the compression rebound rate of the second part is P2%, where P1-P2 > 20.
[0008] In some embodiments, the compression rebound rate of the second part is P2%, where P2 > 70.
[0009] In some implementations, the compression ratio of the first portion is Q1%, where 70 ≤ Q1 ≤ 95.
[0010] In some implementations, the compression rate of the second part is Q2%, where 40 ≤ Q2 < 70.
[0011] In some embodiments, the density of the first portion is A1 g / cm³. 3 , 0.05≤A1<0.5.
[0012] In some embodiments, the density of the second portion is A2 g / cm³. 3 , 0.5≤A2≤1.0.
[0013] In some embodiments, the density of the first portion is A1 g / cm³. 3 The density of the second part is A2 g / cm³. 3 A2 > A1.
[0014] In some embodiments, the density of the first portion is A1 g / cm³. 3 The density of the second part is A2 g / cm³. 3 , 0 < A2 - A1 ≤ 0.5.
[0015] In some embodiments, the horizontal thermal conductivity of the first portion is greater than 50 W / m·K, and the vertical thermal conductivity of the first portion is greater than 5 W / m·K.
[0016] In some embodiments, the horizontal thermal conductivity of the second part is greater than 100 W / m·K, and the vertical thermal conductivity of the second part is greater than 5 W / m·K.
[0017] In some embodiments, the density of the first portion is A1 g / cm³. 3 The value of A1 ranges from 0.05 to 0.5.
[0018] In some embodiments, the density of the first portion is A1 g / cm³. 3 The density of the second part is A2 g / cm³. 3 , 0 < A2 - A1 ≤ 0.5.
[0019] In some embodiments, the composite foam includes a one-dimensional support material.
[0020] In some embodiments, the one-dimensional support material is a nanomaterial.
[0021] In some embodiments, the one-dimensional support material includes at least one of carbon nanotubes, carbon fibers, and polymer fibers.
[0022] In some embodiments, the composite foam has a porous structure.
[0023] In some embodiments, the composite foam has a porous structure, wherein at least a portion of the pores are formed by overlapping two-dimensional sheets of graphene and a one-dimensional support material.
[0024] In some embodiments, the length of the one-dimensional support material is 5 μm to 400 μm and the diameter is 5 nm to 20 μm.
[0025] In some embodiments, the first portion has a first hole structure, wherein the ratio of the transverse hole diameter to the longitudinal hole diameter of the first hole structure is 1 to 2.
[0026] In some embodiments, the first portion has a first hole structure, the lateral diameter of which is 30 μm to 200 μm.
[0027] In some embodiments, the second part has a second hole structure, wherein the ratio of the transverse hole diameter to the longitudinal hole diameter of the second hole structure is 2 to 4.
[0028] In some embodiments, the second part has a second hole structure, the lateral diameter of which is 100 μm to 200 μm.
[0029] In some embodiments, the thickness of the composite foam is 0.15 mm to 3.0 mm.
[0030] In some embodiments, the density of the composite foam is 0.05 g / cm³. 3 ~1.0g / cm 3 .
[0031] In some embodiments, the composite foam has a horizontal thermal conductivity of 50–200 W / m·K and a vertical thermal conductivity of 5–30 W / m·K.
[0032] Secondly, this application provides a method for preparing composite foam, comprising the following preparation steps:
[0033] A slurry containing graphene oxide is prepared, and the slurry is subjected to a film-forming treatment to obtain a primary film;
[0034] A portion of the original film is subjected to a foaming and pre-expansion treatment to obtain a pre-expanded film;
[0035] The pre-expanded membrane is subjected to carbonization and graphitization treatment to obtain composite foam.
[0036] In some embodiments, the slurry further includes a one-dimensional support material.
[0037] In some embodiments, the mass ratio of the graphene oxide to the one-dimensional support material is 100:(1-20).
[0038] In some embodiments, the one-dimensional support material is a nanomaterial.
[0039] In some embodiments, the one-dimensional support material includes at least one of carbon nanotubes, carbon fibers, and polymer fibers.
[0040] In some embodiments, the particle size of the graphene oxide in the slurry is 1 μm to 5 μm.
[0041] In some embodiments, the viscosity of the slurry is 10,000 cps to 50,000 cps.
[0042] In some embodiments, the thickness of the original film is 100 μm to 400 μm.
[0043] In some embodiments, the mass ratio of carbon atoms to oxygen atoms in the graphene oxide is 1.6 to 2.4.
[0044] In some embodiments, the mass content of solid particles in the slurry is 0.5% to 5%.
[0045] In some embodiments, the step of foaming and pre-expanding a portion of the original film includes: immersing half or less of the thickness of the original film in a foaming agent solution, and then washing with water to remove the solvent.
[0046] In some embodiments, the wetting time of the foaming agent solution is 5s to 60s.
[0047] In some embodiments, the solvent removal method includes washing with water and drying.
[0048] In some embodiments, the drying temperature is 40°C to 400°C.
[0049] In some embodiments, the foaming agent solution includes a chemical foaming agent, which includes at least one of hydrazine hydrate, sodium hydroxide, sodium borohydride, and vitamin C.
[0050] In some embodiments, the foaming agent solution includes a physical foaming agent, which includes at least one selected from sodium bicarbonate, sodium carbonate, calcium carbonate, and magnesium carbonate.
[0051] In some embodiments, the mass concentration of the foaming agent solution is 1 wt% to 9 wt%.
[0052] In some embodiments, the carbonization temperature is 900°C to 1200°C.
[0053] In some embodiments, the carbonization process takes 5 to 20 hours.
[0054] In some embodiments, the temperature of the graphitization treatment is 2600°C to 3100°C.
[0055] In some embodiments, the graphitization process takes 10 to 40 hours.
[0056] In some embodiments, the ratio of the thickness of the upper half of the original film to the thickness of the upper half of the pre-expanded film to the thickness of the upper half of the composite foam along the thickness direction is 1:(2-5):(1-2.5).
[0057] In some embodiments, the ratio of the thickness of the lower half of the original film to the thickness of the lower half of the pre-expanded film to the thickness of the lower half of the composite foam is 1:(1.2 to 1.5):(0.7 to 1).
[0058] Thirdly, an electronic device comprising electronic components and the composite foam described above or the composite foam prepared by the method described above.
[0059] Compared with the prior art, the present invention has at least the following beneficial effects:
[0060] The composite foam proposed in this application possesses excellent compression resilience and thermal conductivity. The first part of the composite foam exhibits high expansion and a good compression resilience rate, providing excellent cushioning and shock absorption, and protecting electronic devices attached to it. Simultaneously, the first part rapidly transfers heat longitudinally to the second part, which has low expansion and high thermal conductivity, quickly dissipating the heat absorbed by the first part, thus improving the heat dissipation performance of the graphene foam surface and reducing the overall temperature of the electronic device. Furthermore, the composite foam of this application has advantages such as high temperature resistance, light weight, high thermal conductivity, strong chemical stability, and low coefficient of thermal expansion, making it suitable for a wide range of applications.
[0061] The method for preparing composite foam provided in this application involves forming a graphene oxide-containing slurry into a primary film, then subjecting a portion of the primary film to a foaming pre-expansion treatment to obtain a pre-expansion film. The pre-expansion treated portion of the primary film exhibits high expansibility, while the untreated portion has lower expansibility but higher thermal conductivity. Finally, the pre-expansion film undergoes carbonization and graphitization treatments to obtain a graphene composite foam. The first part of the composite foam (i.e., the pre-expansion treated portion) exhibits high expansibility, good compression resilience, and longitudinal thermal conductivity. This first part can rapidly transfer heat longitudinally to the second part. The second part, with low expansibility and high thermal conductivity, can quickly dissipate the heat absorbed by the first part, improving the heat dissipation performance of the graphene foam surface and reducing the temperature of the entire electronic device.
[0062] The electronic device provided in this application utilizes composite foam to improve the cushioning and shock absorption effect of internal electronic components, which can effectively protect the electronic components and also has good heat dissipation performance, thereby reducing the manufacturing cost of the electronic device and simplifying the assembly process. Attached Figure Description
[0063] The present invention will be further described below with reference to the accompanying drawings and embodiments.
[0064] Figure 1 SEM image of the composite foam provided in the embodiments of this application;
[0065] Figure 2 A schematic flowchart illustrating the preparation method of the composite foam provided in the embodiments of this application;
[0066] Figure 3 A partial structural schematic diagram of the electronic device provided in an embodiment of this application;
[0067] Figure 4 This is a SEM image of the first part of the composite foam obtained in Example 1 of the present invention at a magnification of 500x.
[0068] Figure 5 This is a SEM image of the second part of the composite foam obtained in Example 1 of the present invention at a magnification of 500x.
[0069] Figure 6 This is a SEM image of the first part of the composite foam obtained in Example 1 of the present invention at a magnification of 1000x.
[0070] Figure 7 The compression rate curves of the composite foam obtained in Example 1 of the present invention under different pressures are shown. Detailed Implementation
[0071] To better understand the technical solution of the present invention, the embodiments of the present invention will be described in detail below with reference to the accompanying drawings.
[0072] It should be understood that the described embodiments are merely some, not all, of the embodiments of the present invention. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without inventive effort are within the scope of protection of the present invention.
[0073] The terminology used in the embodiments of this invention is for the purpose of describing particular embodiments only and is not intended to limit the invention. The singular forms “a,” “the,” and “the” as used in the embodiments of this invention and the appended claims are also intended to include the plural forms unless the context clearly indicates otherwise.
[0074] It should be understood that the term "and / or" used in this article is merely a description of the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent: A existing alone, A and B existing simultaneously, and B existing alone. Additionally, the character " / " in this article generally indicates that the preceding and following related objects have an "or" relationship.
[0075] With the current trend towards lightweighting and highly integrated electronic devices, including high-power components (such as camera lenses, chips, batteries, and RF modules), current integration solutions often employ conductive cloth and polymer foam products. However, these materials have low thermal conductivity, leading to localized overheating in electronic devices and limited cushioning and shock absorption, failing to provide adequate protection. To achieve heat dissipation and cushioning, existing technologies typically employ a multi-layered structure of foam and thermally conductive materials bonded together with adhesives. This process is complex and costly.
[0076] Existing graphene foams are generally produced using chemical vapor deposition, solution mixing, porous template methods, lyotropic plasticizing foaming, or a combination of these methods. The resulting graphene foams exhibit limited structural properties, failing to simultaneously achieve optimal compressibility and thermal conductivity, thus making them unsuitable for practical applications.
[0077] In some embodiments, solution evaporation-induced physical adsorption can be used to precipitate graphene oxide onto a template, achieving three-dimensional assembly of graphene oxide on the template. Then, a template-containing three-dimensional porous graphene material is prepared by reduction. After removing the template and cleaning, the three-dimensional porous graphene material is obtained. The graphene three-dimensional porous material obtained by this method has advantages such as low density, high specific surface area, and high thermal conductivity. However, the graphene oxide is adsorbed in the pores of the porous template, forming a tightly bound network structure. During template removal, the graphene three-dimensional porous material may break, failing to retain its integrity and exhibiting poor compression resilience.
[0078] In some implementations, a composite functional material is prepared by physically bonding compressed rebound foam with a thermally conductive graphite sheet. However, this physical bonding method requires adhesive to bond the two materials together. The presence of adhesive leads to higher interfacial thermal resistance, affecting the overall thermal conductivity, and also results in complex and costly downstream processing.
[0079] Therefore, how to achieve composite foam that combines compressibility and thermal conductivity is a key demand at this stage.
[0080] This application provides a composite foam comprising graphene, wherein the composite foam is divided into a first part and a second part along the thickness direction, the compression resilience of the first part is greater than that of the second part, the thermal conductivity of the first part is less than that of the second part, and the thermal conductivity includes at least one of horizontal thermal conductivity and vertical thermal conductivity.
[0081] The aforementioned composite foam exhibits excellent compression resilience and thermal conductivity. The first part of the composite foam has high expansion and good compression resilience, providing excellent cushioning and shock absorption, thus protecting the electronic devices attached to it. Simultaneously, the first part rapidly transfers heat vertically to the second part, which has low expansion and high thermal conductivity, quickly dissipating the heat absorbed by the first part, improving the heat dissipation performance of the graphene foam surface and reducing the overall temperature of the electronic device. Furthermore, the composite foam of this application possesses advantages such as high temperature resistance, light weight, high thermal conductivity, strong chemical stability, and low coefficient of thermal expansion, making it suitable for a wide range of applications.
[0082] Figure 1 SEM images of the composite foam provided in the embodiments of this application, such as Figure 1 As shown, the composite foam is divided into a first part and a second part along the thickness direction, and the thickness ratio of the first part to the second part is (1~3):1. Figure 1 As shown, the thickness ratio of the first part to the second part can be 3:1, 2.5:1, 2:1, 1.5:1, or 1:1, etc., and is not limited here. It should be noted that this division is only a regional division, and the composite foam is not physically divided.
[0083] In some implementations, the compression rebound rate of the first part is P1, where P1 > 90. Specifically, P1 can be 91, 92, 93, 94, 95, 96, 97, 98, 99, 100, etc., and is not limited here.
[0084] In some implementations, the compression rate of the first part is Q1%, where 70 ≤ Q1 ≤ 95; Q1 can specifically be 70, 72, 75, 78, 80, 85, 87, 89, 90, 92, 95, etc., and is not limited here.
[0085] In some embodiments, the density of the first portion is A1 g / cm³. 3 0.05≤A1<0.5, specifically it can be 0.05, 0.08, 0.09, 0.1, 0.2, 0.3, 0.4, 0.49, etc., without limitation here. The first part has high expansibility and low density.
[0086] In some embodiments, the horizontal thermal conductivity of the first portion is greater than 50 W / m·K, and the vertical thermal conductivity of the first portion is greater than 5 W / m·K.
[0087] In some embodiments, the first part has a first hole structure, and the ratio of the transverse hole diameter to the longitudinal hole diameter of the first hole structure is 1 to 2, specifically 1, 1.1, 1.5, 1.6, 1.7, 1.8, 1.9, etc., which are not limited here.
[0088] In some embodiments, the lateral aperture of the first hole structure is 30μm to 200μm; specifically, it can be 30μm, 50μm, 60μm, 80μm, 100μm, 120μm, 150μm, 180μm or 200μm, etc., and is not limited here.
[0089] In some embodiments, the first part has a first hole structure with a large aperture.
[0090] In some embodiments, the horizontal thermal conductivity of the second part is greater than 100 W / m·K, and the vertical thermal conductivity of the second part is greater than 5 W / m·K.
[0091] In some embodiments, the compression rebound rate of the second part is P2, where P2 > 70; the compression rebound rate of the second part is less than that of the first part.
[0092] In some embodiments, the compression rebound rate of the second part is P2%, and P1-P2 > 20; that is, the compression rebound rate of the second part is less than that of the first part because the first part has high expansibility. The specific values of P1-P2 can be 21, 22, 25, 27, 28, 29, etc., and are not limited here.
[0093] In some implementations, the compression rate of the second part is Q2%, where 40 ≤ Q2 < 70. Specifically, it can be 40, 50, 55, 60, 65, 69, etc., and is not limited here.
[0094] In some embodiments, the density of the second portion is A2 g / cm³. 3 0.5≤A2≤1.0, where A2 can be 0.5, 0.6, 0.7, 0.8, 0.9, 0.95, 1, etc., and is not limited here. The second part has low expansion, its structure is relatively compact, and its density is greater than that of the first part, that is, A2>A1.
[0095] In some implementations, 0 < A2 - A1 ≤ 0.5, specifically 0.1, 0.2, 0.3, 0.4, 0.5, etc., which are not limited here.
[0096] In some embodiments, the second part has a second hole structure, and the ratio of the transverse hole diameter to the longitudinal hole diameter of the second hole structure is 2 to 4; specifically, it can be 2, 2.1, 2.5, 2.8, 3.0, 3.5, 3.8, 4.0, etc., which are not limited here.
[0097] In some embodiments, the lateral aperture of the second pore structure is 100μm to 200μm, specifically 100μm, 120μm, 140μm, 150μm, 160μm, 180μm, or 200μm, etc., and is not limited here.
[0098] In some implementations, the composite foam includes a one-dimensional support material.
[0099] In some embodiments, the one-dimensional support material is a nanomaterial. The one-dimensional support material is fibrous, has extensibility and stretchability, and can provide strong rigidity. The one-dimensional support material can support composite foam with a porous structure, which is beneficial to maintaining the structural stability of the pore structure.
[0100] In some embodiments, the one-dimensional support material includes at least one of carbon nanotubes, carbon fibers, and polymer fibers. Specifically, the carbon nanotubes may be multi-walled carbon nanotubes or single-walled carbon nanotubes; the carbon fibers may be polyacrylonitrile-based carbon fibers or mesophase pitch-based carbon fibers; and the polymer-based fibers may be aramid fibers.
[0101] In some embodiments, the first part includes a one-dimensional support material, and at least a portion of the pores are formed by overlapping two-dimensional sheets of graphene and the one-dimensional support material. Understandably, the pore structure formed by the overlapping of the one-dimensional support material and graphene has strong stability; during normal use, the pore structure is less prone to collapse, which is beneficial for improving the compression resilience of the composite foam.
[0102] In some embodiments, the composite foam has a porous structure.
[0103] In some embodiments, the length of the one-dimensional support material is 5 μm to 400 μm, and the diameter is 5 nm to 20 μm;
[0104] In some embodiments, the thickness of the composite foam is 0.15mm to 3.0mm, specifically 0.15mm, 0.18mm, 0.25mm, 0.5mm, 1.0mm, 1.5mm, 1.8mm, 2.0mm, 2.5mm or 3.0mm, etc., and is not limited here.
[0105] In some embodiments, the density of the composite foam is 0.05 g / cm³. 3 ~1.0g / cm 3 Specifically, it can be 0.05 g / cm³. 3 0.08g / cm 3 0.15g / cm 3 0.29g / cm 3 0.37g / cm 3 0.5g / cm 30.7g / cm 3 0.8g / cm 3 0.9g / cm 3 or 1.0g / cm 3 etc. are not specified here.
[0106] In some embodiments, the composite foam has a horizontal thermal conductivity of 50–200 W / m·K and a vertical thermal conductivity of 5–30 W / m·K.
[0107] Secondly, this application provides a method for preparing composite foam, comprising the following preparation steps:
[0108] Step S10: Prepare a slurry containing graphene oxide, and perform a film-forming treatment on the slurry to obtain the original film;
[0109] Step S20: A portion of the original film is subjected to a foaming pre-expansion treatment to obtain a pre-expanded film;
[0110] Step S30: The pre-expanded film is subjected to carbonization and graphitization treatment to obtain composite foam.
[0111] The method for preparing composite foam provided in this application involves forming a graphene oxide-containing slurry into a primary film, and then subjecting a portion of the primary film to a foaming pre-expansion treatment to obtain a pre-expansion film. The pre-expansion treated portion of the primary film exhibits high expansibility, while the untreated portion has lower expansibility but higher thermal conductivity. Finally, the pre-expansion film undergoes carbonization and graphitization treatments to obtain a graphene composite foam. The first part of the composite foam (i.e., the pre-expansion treated portion) has high expansibility, good compression resilience, and longitudinal thermal conductivity. The first part can rapidly transfer heat vertically to the second part. The second part has low expansibility and high thermal conductivity, enabling it to quickly dissipate the heat absorbed by the first part horizontally, thereby improving the heat dissipation performance of the graphene foam surface and reducing the temperature of the entire electronic device.
[0112] The following is a detailed introduction to this solution:
[0113] Step S10: Prepare a slurry containing graphene oxide, and perform a film-forming treatment on the slurry to obtain the original film.
[0114] In some embodiments, the slurry further includes a one-dimensional support material. Adding a graphitizable one-dimensional support material to a graphene oxide-containing slurry helps repair lattice defects in the graphene during high-temperature graphitization. Furthermore, the one-dimensional support material enhances the mechanical properties of the composite foam skeleton, providing support between the upper and lower layers of the graphene sheet structure and giving the composite foam better compressibility and resilience.
[0115] In some embodiments, the mass ratio of the graphene oxide to the one-dimensional support material is 100:(1-20), specifically 100:1, 100:5, 100:6, 100:10, 100:12, 100:15, 100:18, 100:20, etc., which are not limited here.
[0116] In some embodiments, the one-dimensional support material is a nanomaterial.
[0117] In some embodiments, the one-dimensional support material is formulated into a dispersion, and then the dispersion is added to a slurry containing graphene oxide. Liquid phase mixing is beneficial for the uniform dispersion and mixing of the one-dimensional support material and graphene oxide to form a uniform slurry.
[0118] In some embodiments, the one-dimensional support material includes at least one of carbon nanotubes, carbon fibers, and polymer fibers.
[0119] In some embodiments, the particle size of graphene oxide in the slurry is 1μm to 5μm, specifically 1μm, 2μm, 2.5μm, 3μm, 3.5μm, 4μm, 4.5μm or 5μm, etc., and is not limited here.
[0120] In some embodiments, the viscosity of the slurry is 10,000 cps to 50,000 cps, specifically 10,000 cps, 20,000 cps, 30,000 cps, 35,000 cps, 40,000 cps, 45,000 cps or 50,000 cps, etc., and is not limited here.
[0121] In some embodiments, the thickness of the original film is 100μm to 400μm, specifically 100μm, 150μm, 200μm, 250μm, 300μm, 350μm or 400μm, etc., and is not limited here.
[0122] In some embodiments, the mass ratio of carbon atoms to oxygen atoms in the graphene oxide is 1.6 to 2.4, specifically 1.6, 1.7, 1.8, 2.0, 2.2, 2.3, 2.4, etc., and is not limited here.
[0123] In some embodiments, the mass content of solid particles in the slurry is 0.5% to 5%, specifically 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, etc., and is not limited here.
[0124] Step S20: A portion of the original film is foamed and pre-expanded to obtain a pre-expanded film.
[0125] In some embodiments, a foaming agent solution is used to wet half or less of the thickness of the original film, and then the solvent is removed to obtain a pre-expanded film.
[0126] In some embodiments, the thickness of the original film can be H, and the wetting thickness can be 0.2H, 0.3H, 0.4H, 0.5H, etc., which are not limited here. Understandably, the wetting portion can foam to form a highly expansive area, while the remaining portion retains low expansibility.
[0127] In some embodiments, the wetting time of the foaming agent solution is 5s to 60s, specifically 5s, 10s, 20s, 35s, 50s, 60s, etc., which are not limited here.
[0128] In some embodiments, the solvent removal method includes washing with water and drying. Understandably, thorough washing with water can dilute and remove most of the residual foaming agent solution in the pre-expanded film, and low-temperature drying can effectively remove the solvent in the original film, including water and the solvent in the foaming agent solution.
[0129] In some embodiments, the drying temperature is 40℃ to 400℃, specifically 40℃, 50℃, 100℃, 150℃, 200℃, 250℃, 300℃ or 400℃, etc., and is not limited here.
[0130] In some embodiments, the foaming agent solution includes a chemical foaming agent, which includes at least one of hydrazine hydrate, sodium hydroxide, sodium borohydride, and vitamin C.
[0131] In some embodiments, the foaming agent solution includes a physical foaming agent, which includes at least one selected from sodium bicarbonate, sodium carbonate, calcium carbonate, and magnesium carbonate.
[0132] In some embodiments, the mass concentration of the foaming agent solution is 1 wt% to 9 wt%. The specific mass concentration can be 1 wt%, 2 wt%, 3 wt%, 5 wt%, 7 wt%, or 9 wt%, etc., and is not limited thereto. If the mass concentration of the foaming agent solution is too high, the foaming expansion of the original film will be excessive, resulting in a decrease in the toughness of the original film and an increase in its brittleness. If the mass concentration is too low, the foaming effect of the original film will be insignificant.
[0133] Understandably, by controlling the wetting time, concentration, and drying process of the foaming agent solution, the degree of foaming of the original film can be controlled, resulting in parts of the original film exhibiting high expansion and others exhibiting low expansion. Furthermore, during the pre-expansion foaming process, as the original film expands in volume, the pore structure formed by the overlap between some of the supporting material and graphene helps maintain the structural stability of the pore structure. During normal use, the pore structure is less prone to collapse, which helps improve the compression resilience of the composite foam.
[0134] Step S30: The pre-expanded film is subjected to carbonization and graphitization treatment to obtain composite foam.
[0135] In some embodiments, the carbonization temperature is 900℃ to 1200℃, specifically 900℃, 950℃, 1000℃, 1050℃, 1100℃, 1150℃ or 1200℃, etc., and is not limited here.
[0136] In some embodiments, the carbonization treatment time is 5h to 20h, specifically 5h, 8h, 10h, 15h, 18h or 20h, etc., and is not limited here.
[0137] In some embodiments, the temperature of the graphitization treatment is 2600℃~3100℃, specifically 2600℃, 2700℃, 2800℃, 2900℃, 3000℃, 3050℃ or 3100℃, etc., and is not limited here.
[0138] In some embodiments, the graphitization treatment time is 10h to 40h, specifically 10h, 15h, 20h, 25h, 30h or 40h, etc., and is not limited here.
[0139] In some embodiments, the ratio of the thickness of the upper half of the original film to the thickness of the upper half of the pre-expanded film to the thickness of the upper half of the composite foam along the thickness direction is 1:(2-5):(1-2.5), specifically 1:2:1, 1:3:1, 1:3.5:1, 1:4:1, 1:5:1, 1:5:2 or 1:4:2.5, etc., which are not limited here.
[0140] In some embodiments, the ratio of the thickness of the lower half of the original film to the thickness of the lower half of the pre-expanded film to the thickness of the lower half of the composite foam is 1:(1.2~1.5):(0.7~1), specifically it can be 1:1.2:0.7, 1:1.2:1, 1:1.3:1, 1:1.4:1, 1:1.5:1, 1:1.5:0.7 or 1:1.5:0.8, etc., and is not limited here.
[0141] This application also provides an electronic device, which includes electronic components and composite foam. Figure 3 This is a partial structural diagram of the electronic device provided in the embodiments of this application, such as... Figure 3 As shown, composite foam is placed on the surface of electronic devices, with the first part adhering to the surface of the electronic devices. This improves the cushioning and shock absorption effect of the internal electronic devices, effectively protecting them while also providing excellent heat dissipation. This reduces the manufacturing cost of electronic devices and simplifies the assembly process.
[0142] Electronic devices can be any of the following: mobile phones, computers, laptops, iPads, wearable devices, or in-vehicle electronic devices. These devices are highly integrated and require strong heat dissipation. For example... Figure 3 As shown, when the electronic device is a mobile phone, the mobile phone includes composite foam 10, camera module 20 and mid-frame 30. Composite foam 10 can be attached to one side of camera module 20 and connect camera module 20 and mid-frame 30, thereby improving the buffering and shock absorption effect of camera module 20 and conducting the heat of camera module 20 to mid-frame 30.
[0143] In some embodiments, the mobile phone also includes a graphite heat dissipation layer 40, which is disposed on the side of the mid-frame 30 away from the camera module 20. The composite foam further conducts the heat generated by the camera module 20 to the graphite heat dissipation layer 40 on the other side of the mid-frame 30 for heat dissipation.
[0144] In some implementations, composite foam can also be used in combination with heat spreaders, heat-conducting sheets, etc., which is not limited here.
[0145] The above are merely preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
[0146] Example 1
[0147] Carbon nanotube dispersion was added to a graphene oxide slurry with a carbon-to-oxygen ratio of 1.6. The mass ratio of graphene oxide slurry to carbon nanotubes was 100:10, and the viscosity of the slurry was 10000 cps. The slurry was then coated to form a film with a dry film thickness of 300 μm.
[0148] A 9 wt% sodium bicarbonate solution was brushed onto the surface of the original film and allowed to soak for 15 seconds, so that the sodium bicarbonate solution could penetrate half the thickness of the original film. Then, the foaming agent solution was washed off with water and the film was dried in an oven at 90°C to obtain a pre-expanded film.
[0149] The pre-expanded film was carbonized at 900℃ for 10 hours and then graphitized at 3000℃ for 20 hours to obtain composite foam.
[0150] Figure 1 Here is a low-magnification SEM image of the composite foam prepared in Example 1, as shown. Figure 1 As shown, the composite foam is divided into a first part and a second part along the thickness direction, with a thickness ratio of 3:1 between the first part and the second part. The total thickness of the composite foam is 0.9 mm, and its density is 0.19 g / cm³. 3 The horizontal thermal conductivity is 100 W / (m·K), and the vertical thermal conductivity is 8 W / (m·K).
[0151] Figure 4 Here is a 500x magnification SEM image of the first part of the composite foam prepared in Example 1, as shown. Figure 4 As shown, the first part of the composite foam has a highly expandable porous and fluffy structure. Figure 5 This is a 500x SEM image of the second part of the composite foam prepared in Example 1. Compared to the first part, the second part has a lower expansion structure.
[0152] Figure 6 Here is a 1000x magnification SEM image of the first part of the composite foam prepared in Example 1, as shown. Figure 6 As shown, the second part of the composite foam shows that carbon nanotubes are uniformly distributed in the graphene sheet structure, and the graphene layers are cross-linked to form thermally conductive channels.
[0153] Figure 7 The compression rate curves of the composite foam prepared in Example 1 under different pressures are shown. The compression rate is 75% and the compression recovery rate is 90%.
[0154] Example 2
[0155] Carbon nanotube dispersion was added to a graphene oxide slurry with a carbon-to-oxygen ratio of 1.6. The mass ratio of graphene oxide slurry to carbon nanotubes was 100:4, and the viscosity of the slurry was 4000 cps. The slurry was then coated to form a film with a dry film thickness of 500 μm.
[0156] A 7wt% hydrazine hydrate solution was gently brushed onto the surface of the original membrane and allowed to soak for 10 seconds, so that the hydrazine hydrate solution could penetrate half the thickness of the original membrane. Then, the foaming agent solution was washed off with water and dried in an oven at 60°C to obtain a pre-expanded membrane.
[0157] The pre-expanded film was carbonized at 900℃ for 9 hours and then graphitized at 2900℃ for 40 hours to obtain composite foam.
[0158] The composite foam is divided into a first part and a second part along its thickness direction, with a thickness ratio of 3:1 between the first part and the second part. The total thickness of the composite foam is 1.0 mm, and its density is 0.16 g / cm³. 3 The horizontal thermal conductivity is 75 W / (m·K), and the vertical thermal conductivity is 5 W / (m·K).
[0159] Example 3
[0160] Carbon nanotube dispersion was added to a graphene oxide slurry with a carbon-to-oxygen ratio of 2.0. The mass ratio of graphene oxide slurry to carbon nanotubes was 100:10, and the viscosity of the slurry was 10000 cps. The slurry was then coated to form a film with a dry film thickness of 100 μm.
[0161] A 3 wt% hydrazine hydrate solution was gently brushed onto the surface of the original film and allowed to soak for 5 seconds, so that the hydrazine hydrate solution could penetrate half the thickness of the original film. Then, the foaming agent solution was washed off with water, and the film was dried in a 90°C oven. The solvent was then removed to obtain a pre-expanded film.
[0162] The pre-expanded film was carbonized at 800℃ for 15 hours and then graphitized at 2950℃ for 20 hours to obtain composite foam.
[0163] The composite foam was divided into a first part and a second part along its thickness direction, with a thickness ratio of 2:1 between the first part and the second part. The measured thickness of the composite foam was 0.8 mm, and its density was 0.16 g / cm³. 3 The horizontal thermal conductivity is 54 W / (m·K), the vertical thermal conductivity is 10 W / (m·K), the compression resilience is 90%, and the compression ratio is 70%.
[0164] Example 4
[0165] Unlike Example 1, a 5 wt% sodium borohydride solution was gently brushed onto the surface of the original film, and the wetting time was 40 seconds, so that the sodium borohydride solution wetted half of the thickness of the original film, thus obtaining a pre-expanded film.
[0166] Example 5
[0167] Unlike Example 1, an 8 wt% magnesium carbonate solution was gently brushed onto the surface of the original film, and the wetting time was 20 seconds, so that the magnesium carbonate solution wetted half the thickness of the original film, thus obtaining a pre-expanded film.
[0168] Example 6
[0169] Unlike Example 1, a 7wt% sodium bicarbonate solution was brushed onto the surface of the original film, and the wetting time was 60s, so that the sodium bicarbonate solution wetted half the thickness of the original film, thus obtaining a pre-expanded film.
[0170] Example 7
[0171] Unlike Example 1, carbon fiber dispersion was added to graphene oxide slurry with a carbon-to-oxygen ratio of 1.6. The mass ratio of graphene oxide slurry to carbon fiber was 100:20, and the viscosity of the slurry was 10000 cps. The slurry was coated to form a film to obtain a base film with a dry film thickness of 300 μm.
[0172] Example 8
[0173] Unlike Example 1, an aramid fiber dispersion was added to a graphene oxide slurry with a carbon-to-oxygen ratio of 1.6. The mass ratio of graphene oxide slurry to aramid fiber was 100:5, and the viscosity of the slurry was 5000 cps. The slurry was then coated to form a film to obtain a base film with a dry film thickness of 300 μm.
[0174] Example 9
[0175] Unlike Example 1, a 9 wt% sodium bicarbonate solution was brushed onto the surface of the original film, and the wetting time was 5 seconds, so that the sodium bicarbonate solution wetted 1 / 3 of the thickness of the original film, thus obtaining a pre-expanded film.
[0176] Example 10
[0177] Unlike Example 1, a graphene oxide slurry with a carbon-to-oxygen ratio of 1.6 was prepared, without the addition of carbon nanotube dispersion. The viscosity of the slurry was 3000 cps. The slurry was coated to form a film to obtain a base film with a dry film thickness of 400 μm.
[0178] Comparative Example 1
[0179] Unlike Example 1, after the slurry was formed into a film, it was directly placed in an oven at 400°C for 30 hours to dry, then placed at 900°C for 10 hours to carbonize, and then further heated to 3000°C for graphitization treatment for 20 hours to obtain composite foam.
[0180] Test method:
[0181] The testing methods corresponding to the performance mentioned above.
[0182] 1. Horizontal thermal conductivity test
[0183] The equipment used was an LFA-467 Hyper Flash; referring to ASTM-E1461, "Standard Test Method for Determination of Fixed Thermal Conductivity by Flash Method", the sample was cut into a circular piece with a diameter of 25.4 mm to measure the thermal diffusivity of graphene foam. Thermal conductivity = thermal diffusivity * density * specific heat capacity (specific heat capacity: 0.85) was calculated.
[0184] 2. Vertical thermal conductivity test
[0185] The equipment used was the LW-9389 steady-state heat flow thermal conductivity tester; referring to ASTM-D5470 "Standard Test Method for Thermal Transfer Properties of Thermally Conductive and Electrically Insulating Materials", the sample was cut into a 3mm×3mm square piece, and the thermal conductivity of the graphene foam was tested by selecting the thermally conductive sheet-thermal conductivity test mode.
[0186] 3. Compression ratio
[0187] The equipment used was an LW-9389 steady-state heat flow thermal conductivity tester; referring to ASTM-D575 "Test Method for Compression Properties of Rubber", the sample was cut into a 3mm×3mm square piece, and the thermal conductivity sheet-compression ratio test mode was selected to test the compression ratio of graphene foam under different pressures.
[0188] Using the above method, the compression ratio of the first and second parts obtained from the segmentation is tested separately.
[0189] 4. Compression rebound rate
[0190] The equipment used was an AGS-X electronic universal tensile testing machine. Referring to GB / T 34336-2017 "Test Method for Compression Rebound Rate of Nanoporous Aerogel Composite Thermal Insulation Materials", the samples were cut into 100mm × 100mm square pieces. The initial thickness h1 of the samples was measured using a thickness gauge, accurate to 0.01mm. The compression speed of the testing machine was 2mm / min. Compression was stopped when the sample was compressed to (100±5) kPa, and the testing machine was held in this position for 5 minutes. After 5 minutes of recovery, the recovered thickness h2 of the sample was measured using a thickness gauge, accurate to 0.01mm. Compression rebound rate = (h2 / h1) × 100%.
[0191] Using the above method, compression rebound rate tests were conducted on the half of the first part and the half of the second part that are far apart from each other.
[0192] Table 1. Performance of materials in comparative examples and embodiments.
[0193]
[0194]
[0195] Comparing Examples 1 to 9 in Table 1, it can be seen that the composite foam prepared in these examples has good compression resilience and thermal conductivity. The first part of the composite foam has high expansion and a compression resilience rate >90%, which is good. The first part can play a good role in buffering and shock absorption, and can provide shock absorption protection for electronic devices attached to the first part of the composite foam. At the same time, the first part can quickly transfer heat to the second part in the longitudinal direction. The second part has low expansion and high thermal conductivity, and can quickly dissipate the heat absorbed by the first part in the horizontal direction, thereby improving the heat dissipation performance of the graphene foam surface and reducing the temperature of the entire electronic device.
[0196] Compared to Example 1, Example 10 did not add any supporting material. The cross-linking between the pure graphene layers after carbonization and graphitization was reduced, and the film compression performance was lower than that of Example 1.
[0197] Compared to Example 1, Comparative Example 1, the original film after coating did not undergo a pretreatment foaming process, but directly underwent post-processing carbonization and graphitization. Foaming was performed through the carbonization and graphitization processes, resulting in a film with no difference in structure in the thickness direction. Compared to the pretreatment foaming process, the first part has a lower expansion rate and lower film compression performance.
[0198] The above description is merely a preferred embodiment of this application and is not intended to limit this application. Various modifications and variations can be made to this application by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the protection scope of this application.
Claims
1. A composite foam, characterized in that, The composite foam is prepared by partially foaming and pre-expanding the same graphene oxide-containing original film. The composite foam includes graphene. The composite foam is divided into a first part and a second part along the thickness direction. The compression resilience of the first part is P1, P1>90. The compression resilience of the first part is greater than that of the second part. The thermal conductivity of the first part is less than that of the second part, and the thermal conductivity includes at least one of horizontal thermal conductivity and vertical thermal conductivity.
2. The composite foam according to claim 1, characterized in that, The composite foam includes at least one of the following characteristics: (1) The thickness ratio of the first part to the second part is (1~3):1; (2) The compression rebound rate of the second part is P2%, P1-P2>20; (3) The compression rebound rate of the second part is P2%, P2 > 70; (4) The compression rate of the first part is Q1%, 70≤Q1≤95; (5) The compression rate of the second part is Q2%, 40≤Q2<70; (6) The density of the first part is A1 g / cm³. 3 , 0.05≤A1<0.5; (7) The density of the second part is A2 g / cm³. 3 , 0.5≤A2≤1.0; (8) The density of the first part is A1 g / cm³. 3 The density of the second part is A2 g / cm³. 3 A2 > A1; (9) The density of the first part is A1 g / cm³. 3 The density of the second part is A2 g / cm³. 3 , 0 < A2 - A1 ≤ 0.5; (10) The horizontal thermal conductivity of the first part is greater than 50 W / m•K, and the vertical thermal conductivity of the first part is greater than 5 W / m•K; (11) The horizontal thermal conductivity of the second part is greater than 100 W / m•K, and the vertical thermal conductivity of the second part is greater than 5 W / m•K; (12) The density of the first part is A1 g / cm³. 3 The value of A1 ranges from 0.05 to 0.5; (13) The density of the first part is A1 g / cm³. 3 The density of the second part is A2 g / cm³. 3 , 0 < A2 - A1 ≤ 0.
5.
3. The composite foam according to claim 1, characterized in that, The composite foam includes a one-dimensional support material, and the composite foam includes at least one of the following characteristics: (1) The one-dimensional support material is a nanomaterial; (2) The one-dimensional support material includes at least one of carbon nanotubes, carbon fibers and polymer fibers; (3) The composite foam has a porous structure; (4) The composite foam has a porous structure, and at least some of the pores are formed by overlapping two-dimensional sheets of graphene and one-dimensional support material. (5) The length of the one-dimensional support material is 5μm~400μm and the diameter is 5nm~20μm; (6) The first part has a first hole structure, wherein the ratio of the transverse hole diameter to the longitudinal hole diameter of the first hole structure is 1 to 2; (7) The first part has a first hole structure, and the transverse diameter of the first hole structure is 30μm ~ 200μm; (8) The second part has a second hole structure, wherein the ratio of the transverse hole diameter to the longitudinal hole diameter of the second hole structure is 2 to 4; (9) The second part has a second hole structure, and the transverse pore diameter of the second hole structure is 100μm~200μm.
4. The composite foam according to any one of claims 1 to 3, characterized in that, The composite foam includes at least one of the following characteristics: (1) The thickness of the composite foam is 0.15mm~3.0mm; (2) The density of the composite foam is 0.05 g / cm³. 3 ~1.0g / cm 3 ; (3) The horizontal thermal conductivity of the composite foam is 50~200 W / m•K and the vertical thermal conductivity is 5~30 W / m•K.
5. A method for preparing composite foam, characterized in that, The preparation steps include the following: A composite slurry containing graphene oxide is prepared, and the slurry is subjected to film-forming treatment to obtain the original film; A portion of the original film is subjected to a foaming and pre-expansion treatment to obtain a pre-expanded film; The pre-expanded membrane is subjected to carbonization and graphitization treatment to obtain composite foam.
6. The preparation method according to claim 5, characterized in that, The slurry further includes a one-dimensional support material, and the method includes at least one of the following features: (1) The mass ratio of the graphene oxide to the one-dimensional support material is 100:(1~20); (2) The one-dimensional support material is a nanomaterial; (3) The one-dimensional support material includes at least one of carbon nanotubes, carbon fibers and polymer fibers; (4) The particle size of the graphene oxide in the slurry is 1 μm ~ 5 μm; (5) The viscosity of the slurry is 10000cps~50000cps; (6) The thickness of the original film is 100μm~400μm; (7) The mass ratio of carbon atoms to oxygen atoms in the graphene oxide is 1.6 to 2.4; (8) The mass content of solid particles in the slurry is 0.5%~5%.
7. The preparation method according to claim 5, characterized in that, The method includes at least one of the following features: (1) The step of foaming and pre-expanding a portion of the original film includes: wetting half or less of the thickness of the original film with a foaming agent solution, and then removing the solvent; (2) The wetting time of the foaming agent solution is 5s~60s; (3) The solvent removal methods include water washing and drying. (4) The solvent removal method includes water washing and drying treatment, wherein the temperature of the drying treatment is 40℃~400℃; (5) The foaming agent solution includes a chemical foaming agent, which includes at least one of hydrazine hydrate, sodium hydroxide, sodium borohydride and vitamin C; (6) The foaming agent solution includes a physical foaming agent, which includes at least one of sodium bicarbonate, sodium carbonate, calcium carbonate and magnesium carbonate; (7) The mass concentration of the foaming agent solution is 1wt%~9wt%.
8. The preparation method according to claim 6, characterized in that, The method includes at least one of the following features: (1) The carbonization temperature is 900℃~1200℃; (2) The carbonization treatment time is 5h~20h; (3) The temperature of the graphitization treatment is 2600℃~3100℃; (4) The graphitization treatment time is 10h~40h.
9. The preparation method according to claim 8, characterized in that, Along the thickness direction, the ratio of the thickness of the upper half of the original film: the thickness of the upper half of the pre-expanded film: the thickness of the upper half of the composite foam is 1:(2~5):(1~2.5); and / or, The ratio of the thickness of the lower half of the original film to the thickness of the lower half of the pre-expanded film to the thickness of the lower half of the composite foam is 1:(1.2~1.5):(0.7~1).
10. An electronic device, characterized in that, The electronic device includes electronic components and the composite foam as described in any one of claims 1 to 4 or the composite foam prepared by the method described in any one of claims 5 to 9.
Citation Information
Patent Citations
Carbon-based composite with high rebound resilience and high heat conductivity coefficient along thickness direction and preparation method of carbon-based composite
CN104961464A
Composite film, preparation method thereof and electronic equipment
CN114394585A
Graphene composite heat dissipation thin film and preparation method therefor
WO2022261912A1