An electrolyte based on taurine or a derivative thereof modified, a soft package water-based zinc ion battery and a preparation method
By using taurine or its derivatives as an electrolyte additive in aqueous zinc-ion batteries, an in-situ protective layer is formed, which solves the problems of dendrite growth and corrosion on the zinc anode surface and improves the stability and cycle life of the battery.
Patent Information
- Application Number
- CN202310721801.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-16
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-06-16
AI Technical Summary
Side reactions such as dendrite growth, corrosion, and hydrogen evolution on the zinc anode surface limit the cycle life and safety of aqueous zinc-ion batteries, and existing interface engineering methods are complex and difficult to control.
Taurine or its derivatives are used as electrolyte additives to form an in-situ protective layer, which is preferentially adsorbed on the negative electrode surface to generate a water-poor double layer, thereby regulating the zinc ion deposition environment and inhibiting dendrite growth and side reactions.
It significantly improves the stability and cycle life of aqueous zinc-ion batteries, inhibits corrosion and hydrogen evolution reaction on the negative electrode surface, promotes uniform zinc ion deposition, and optimizes battery performance.
Smart Images

Figure CN116722232B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of chemical power source technology, specifically relating to an electrolyte modified with taurine or its derivatives, a soft-pack aqueous zinc-ion battery, and a preparation method thereof. Background Technology
[0002] The commercial development of lithium-ion batteries is currently limited by the global shortage of lithium resources. Simultaneously, safety issues such as flammability and explosiveness caused by the use of organic electrolytes in lithium-ion batteries hinder their application in large-scale energy storage. Aqueous zinc-ion batteries, due to their inherent safety, ease of operation, and low material cost, have broad application prospects in large-scale energy storage and flexible wearable devices. Metallic zinc possesses advantages such as high theoretical capacity, low electrochemical potential, and abundant raw material reserves, making it an ideal negative electrode material for aqueous zinc-ion batteries. Metallic zinc exhibits better stability in water than other metal negative electrodes. However, the zinc negative electrode surface also suffers from severe dendrite growth, surface corrosion passivation, and hydrogen evolution reactions, hindering the practical application of aqueous zinc-ion batteries. The hydrogen evolution reaction increases the pH value near the negative electrode and leads to the formation of electrochemically inert byproducts on the surface. The uneven and loose deposition of these byproducts alters the local electric field distribution, leading to severe dendrite growth, thus affecting cycle life and battery safety. All these problems are closely related to the electrode / electrolyte interface. Therefore, interface engineering of the zinc anode from both structural and compositional perspectives is of great significance for solving these problems. Currently, researchers mainly construct non-in-situ solid electrolyte interface (SEI) layers on the negative electrode surface through methods such as physical coating or chemical deposition. This process is complex and difficult to control in terms of precision, making it unsuitable for practical applications. Summary of the Invention
[0003] The purpose of this invention is to provide an electrolyte modified with taurine or its derivatives, a soft-pack aqueous zinc-ion battery, and a preparation method thereof, in order to overcome problems such as dendrite formation, corrosion, passivation, and hydrogen evolution in zinc anodes. Compared with existing electrolyte additives, the aqueous zinc-ion battery electrolyte additives used in this invention have the advantages of high biocompatibility, low cost, and excellent electrochemical performance. When applied to aqueous zinc-ion batteries, they can achieve stable battery cycle life.
[0004] This invention is achieved through the following technical solution:
[0005] An electrolyte modified with taurine or its derivatives includes a zinc salt, water, and an electrolyte additive; the concentration of the zinc salt is 1-3 mol / L, the electrolyte additive is taurine or a taurine derivative, the taurine derivative is ethyl taurate or sodium N-methyltaurate, and the concentration of the electrolyte additive is 0.1-2 mol / L.
[0006] Furthermore, the zinc salt is zinc sulfate, and the concentration of the zinc salt is 1-2 mol / L.
[0007] Furthermore, the concentration of the electrolyte additive is 1–2 mol / L.
[0008] A method for preparing an electrolyte modified with taurine or its derivatives includes the following steps:
[0009] Zinc salts were dissolved in water, stirred and sonicated at room temperature to obtain a zinc salt electrolyte.
[0010] Taurine or taurine derivatives are added to zinc salt electrolyte, and stirred and sonicated at room temperature to obtain an electrolyte modified with taurine or its derivatives, i.e., an aqueous zinc-ion battery electrolyte.
[0011] A soft-pack aqueous zinc-ion battery includes a positive electrode, a negative electrode, a separator, tabs, an aluminum-plastic film, and an electrolyte modified with taurine or its derivatives.
[0012] The internal structure of the soft-pack aqueous zinc-ion battery consists of a positive electrode, a separator containing electrolyte, and a negative electrode from top to bottom. The positive electrode is a current collector coated with positive electrode material. The positive and negative electrodes are led out through tabs to serve as the positive and negative electrodes for external connection of the battery. The internal structure is sealed by aluminum-plastic film packaging.
[0013] Furthermore, the positive electrode material is selected from manganese dioxide or ammonium vanadate.
[0014] Furthermore, the negative electrode is made of zinc foil with a purity greater than 99.9%, and the length of the negative electrode is 3-10 cm and the width is 3-10 cm.
[0015] The diaphragm is made of glass fiber and has a length of 5-10 cm and a width of 5-10 cm.
[0016] The current collector is made of carbon cloth, stainless steel foil, or titanium foil, and has a length of 3-10 cm and a width of 3-10 cm.
[0017] Furthermore, the negative electrode has a length of 3-5 cm and a width of 3-5 cm;
[0018] The diaphragm is 5cm long and 5cm wide;
[0019] The current collector has a length of 3-5 cm and a width of 3-5 cm.
[0020] Furthermore, the electrode tab is made of carbon cloth, stainless steel foil, titanium foil, or zinc foil.
[0021] A method for preparing a soft-pack aqueous zinc-ion battery includes the following steps:
[0022] The positive electrode material is uniformly mixed with conductive agent and binder, coated onto current collector, and dried to obtain the positive electrode of aqueous zinc-ion soft-pack battery;
[0023] The obtained positive electrode, the separator with electrolyte, and the negative electrode are stacked together in sequence. The positive and negative electrodes are led out separately with tabs. Finally, they are encapsulated with aluminum-plastic film to assemble an aqueous zinc-ion soft-pack battery.
[0024] Compared with the prior art, the present invention has the following beneficial technical effects:
[0025] This invention utilizes taurine or its derivatives as an electrolyte additive in aqueous zinc-ion batteries, effectively addressing issues such as dendrite growth, corrosion, and passivation on the negative electrode surface, significantly improving the stability and cycle life of aqueous zinc-ion batteries. Taurine or its derivatives contain amino and sulfonic acid functional groups, enabling them to preferentially adsorb onto the negative electrode surface to form a water-poor electrical double layer. Simultaneously, during repeated zinc deposition / stripping processes, taurine and its derivatives preferentially decompose on the negative electrode surface, generating an nitrogen-containing SEI protective layer. This in-situ protective layer fundamentally isolates the zinc metal negative electrode from direct contact with water molecules, thereby greatly suppressing side reactions on the negative electrode surface. Furthermore, taurine and its derivatives exhibit strong interaction with zinc ions in the electrolyte, replacing coordinated water molecules in the hydrated zinc ion solvent sheath, regulating the zinc ion solvent sheath structure, inducing uniform deposition of zinc ions on the negative electrode surface, and thus inhibiting the formation and growth of zinc dendrites.
[0026] The taurine or its derivative electrolyte additive provided by this invention can simultaneously regulate the electrolyte coordination environment and zinc anode / electrolyte interface characteristics of aqueous zinc-ion batteries. It can effectively suppress side reactions such as corrosion, hydrogen evolution, and passivation on the zinc metal anode surface, while promoting uniform deposition and stripping of zinc ions on the zinc anode surface and inhibiting the disordered growth of zinc dendrites. Therefore, electrolytes using the aqueous zinc-ion battery electrolyte additive provided by this invention can significantly improve the stability and reversibility of the zinc metal anode, optimizing the cycle performance and lifespan of aqueous zinc-ion batteries. Furthermore, the electrolyte additive provided by this invention is low-cost, highly biocompatible, and widely available, which helps promote the practical application of aqueous zinc-ion batteries. Attached Figure Description
[0027] Figure 1 The aqueous zinc-ion symmetric cells prepared for Examples 1, 5, and Comparative Example 1 were tested at a current density of 1 mA cm⁻¹. -2 The deposition capacity is 1 mAh cm⁻¹ -2 The time-voltage curves are shown below, where (a) is Example 5, (b) is Example 1, and (c) is Comparative Example 1;
[0028] Figure 2The aqueous zinc-ion symmetric cells prepared for Examples 2, 5, and Comparative Example 1 were tested at a current density of 5 mA cm⁻¹. -2 The deposition capacity is 5 mAh cm⁻¹ -2 The time-voltage curves are shown below, where (a) is Example 5, (b) is Example 2, and (c) is Comparative Example 1;
[0029] Figure 3 The rate performance curves of the aqueous zinc-ion symmetric batteries prepared in Example 5 and Comparative Example 1 at different current densities are shown.
[0030] Figure 4 The aqueous zinc-ion Zn / / Cu asymmetric cells prepared in Examples 3, 5, and Comparative Example 1 were tested at a current density of 1 mA cm⁻¹. -2 The deposition capacity is 0.5 mAh cm⁻¹. -2 The Coulomb efficiency curve below;
[0031] Figure 5 The aqueous zinc-ion Zn / / Cu asymmetric cells prepared for Examples 4, 5, and Comparative Example 1 were tested at a current density of 5 mA cm⁻¹. -2 The deposition capacity is 1 mAh cm⁻¹ -2 The Coulomb efficiency curve below;
[0032] Figure 6 The X-ray diffraction curves of the anode of the aqueous zinc-ion symmetric cells prepared in Example 5 and Comparative Example 1 are shown.
[0033] Figure 7 The aqueous zinc-ion full cells prepared for Example 5 and Comparative Example 1 were tested at a current density of 1 A g. -1 The following is a cycle performance curve;
[0034] Figure 8 The aqueous zinc-ion full cells prepared for Example 6 and Comparative Example 2 were tested at a current density of 1 A g. -1 The following is a cycle performance curve;
[0035] Figure 9 This is a schematic diagram illustrating the mechanism by which taurine and its derivatives enhance the stability of the zinc anode in this invention. Detailed Implementation
[0036] The present invention will now be described in further detail, but this description is intended to explain rather than limit the invention.
[0037] An electrolyte modified with taurine or its derivatives includes a zinc salt, water, and an electrolyte additive; the zinc salt is zinc sulfate, and the concentration of the zinc salt is 1-3 mol / L, preferably 1-2 mol / L; the electrolyte additive is taurine or a taurine derivative, the taurine derivative being ethyl taurate or sodium N-methyltaurate, and the concentration of the electrolyte additive is 0.1-2 mol / L, preferably 1-2 mol / L.
[0038] A method for preparing an electrolyte modified with taurine or its derivatives includes the following steps:
[0039] Zinc salts were dissolved in water and stirred at room temperature to obtain a zinc salt electrolyte.
[0040] Taurine or taurine derivatives are added to zinc salt electrolyte, and stirred and sonicated at room temperature to obtain an electrolyte modified with taurine or its derivatives, i.e., an aqueous zinc-ion battery electrolyte.
[0041] A soft-pack aqueous zinc-ion battery includes a positive electrode, a negative electrode, a separator, tabs, an aluminum-plastic film, and an electrolyte modified with taurine or its derivatives as described above; the amount of electrolyte added is 50-200 μL, preferably 200 μL.
[0042] The internal structure of the soft-pack aqueous zinc-ion battery, from top to bottom, consists of a positive electrode, a separator containing electrolyte, and a negative electrode. The positive electrode is a current collector coated with positive electrode material. The positive and negative electrodes are led out through tabs to serve as the positive and negative electrodes for external connection of the battery. The internal structure is sealed by aluminum-plastic film packaging.
[0043] The positive electrode material is manganese dioxide or ammonium vanadate;
[0044] The negative electrode is made of zinc foil with a purity greater than 99.9%, with a length of 3-10 cm and a width of 3-10 cm, preferably with a length of 3-5 cm and a width of 3-5 cm; the diaphragm is made of glass fiber, with a length of 5-10 cm and a width of 5-10 cm, preferably with a length of 5 cm and a width of 5 cm.
[0045] The current collector is made of carbon cloth, stainless steel foil or titanium foil, and the current collector is 3-10 cm long and 3-10 cm wide, preferably carbon cloth, and more preferably 3-5 cm long and 3-5 cm wide.
[0046] The electrode tabs are made of carbon cloth, stainless steel foil, titanium foil, or zinc foil.
[0047] A method for preparing a soft-pack aqueous zinc-ion battery includes:
[0048] The positive electrode material, conductive agent, and binder were uniformly stirred at 500 r / min for 24 h at a mass ratio of 7:2:1, and then coated onto the current collector. The mixture was then dried in an oven at 80℃ for 12 h to obtain the positive electrode of an aqueous zinc-ion soft-pack battery. The conductive agent was Super P, and the binder was polyvinylidene fluoride.
[0049] The obtained positive electrode is stacked together with a glass fiber separator with electrolyte and a negative electrode (zinc foil) in sequence. The positive and negative electrodes are led out separately with tabs. Finally, they are encapsulated with aluminum-plastic film to assemble an aqueous zinc-ion soft-pack battery.
[0050] Taurine and its derivatives contain amino and sulfonic acid functional groups, enabling them to preferentially adsorb onto the negative electrode surface and form a water-poor electrical double layer. Simultaneously, during repeated zinc deposition / stripping processes, taurine and its derivatives preferentially decompose on the negative electrode surface, generating an in-situ protective layer that fundamentally isolates the zinc metal negative electrode from direct contact with water molecules, suppressing side reactions on the negative electrode surface. Furthermore, taurine and its derivatives can regulate the electrolyte coordination environment and zinc negative electrode / electrolyte interface characteristics in aqueous zinc-ion batteries, effectively suppressing side reactions such as corrosion, hydrogen evolution, and passivation on the zinc metal negative electrode surface. This promotes uniform deposition and stripping of zinc ions on the zinc negative electrode surface, inhibits the disordered growth of zinc dendrites, and contributes to the practical application of aqueous zinc-ion batteries.
[0051] The embodiments of the present invention will be described in detail below with reference to the examples. These embodiments represent preferred solutions of the present invention and should not be construed as limiting the scope of the invention. Unless otherwise specified, the methods and experimental equipment used in the following embodiments are conventional methods and instruments.
[0052] Comparative Example 1
[0053] Step 1: Dissolve 2 mmol of ZnSO4·7H2O in 100 ml of deionized water, stir magnetically for 1 h at room temperature, and sonicate for 10 min to prepare a 2 M ZnSO4 electrolyte. Assemble aqueous zinc-ion symmetric cells and Zn / / Cu cells using zinc foil with a diameter of 16 mm and a thickness of 0.1 mm and a glass fiber membrane with a diameter of 16 mm and a thickness of 0.1 mm, respectively. The electrolyte used was a 2 mol / L ZnSO4 electrolyte, and the electrolyte addition amount was 80 μL.
[0054] Step 2: Add 0.585 g of NH4VO3 to 35 mL of deionized water. Add 0.9455 g of oxalic acid powder to the solution and stir magnetically. Transfer the solution to a 50 mL hydrothermal reactor and heat at 140 °C for 12 h. After cooling, collect the product, wash with deionized water, and then dry at 70 °C overnight to finally obtain NH4V4O. 10 powder.
[0055] Step 3: The product obtained from the drying process in Step 2 is mixed with a conductive agent and a binder at a mass ratio of 7:2:1 and stirred uniformly at 500 r / min for 24 hours. This mixture is then coated onto a 3cm x 3cm carbon cloth and dried in an oven at 80℃ for 12 hours to obtain the positive electrode sheet for an aqueous zinc-ion soft-pack battery. The conductive agent is Super P, and the binder is polyvinylidene fluoride.
[0056] In the fourth step, the positive electrode sheet obtained in the third step is stacked sequentially with a 5cm*5cm glass fiber separator with electrolyte dripped on it and a 3cm*3cm zinc foil. Carbon cloth is used as the positive electrode tab and the zinc foil as the negative electrode tab to lead out the positive and negative electrodes respectively. Finally, it is encapsulated with an aluminum-plastic film to assemble an aqueous zinc-ion soft-pack battery. The electrolyte used is 2mol / L ZnSO4, and the electrolyte addition amount is 200μL.
[0057] Comparative Example 2
[0058] Step 1: Dissolve 2 mmol of ZnSO4·7H2O in 100 ml of deionized water, stir magnetically for 1 h at room temperature, and sonicate for 10 min to prepare a 2 M ZnSO4 electrolyte. Assemble aqueous zinc-ion symmetric cells and Zn / / Cu cells using zinc foil with a diameter of 16 mm and a thickness of 0.1 mm and a glass fiber membrane with a diameter of 16 mm and a thickness of 0.1 mm, respectively. The electrolyte used was a 2 mol / L ZnSO4 electrolyte, and the electrolyte addition amount was 80 μL.
[0059] Step 2: Mix 500 mg KMnO4 with 80 ml deionized water to form a homogeneous suspension. Stir and sonicate the mixture for 30 min, then transfer it to a 100 ml reactor. Store the mixture in an autoclave at 180 °C for 12 h. Collect the brown product by high-speed centrifugation at 8000 rpm, wash several times with deionized water and ethanol, and dry in an oven at 80 °C to obtain the final product MnO2.
[0060] Step 3: The product obtained from the drying in Step 2 is mixed with a conductive agent and a binder at a mass ratio of 7:2:1 and stirred uniformly at 500 r / min for 24 h. This mixture is then coated onto a 3 cm x 3 cm carbon cloth and dried in an oven at 80 °C for 12 h to obtain the positive electrode sheet for an aqueous zinc-ion soft-pack battery. The conductive agent is Super P, and the binder is polyvinylidene fluoride.
[0061] In the fourth step, the positive electrode sheet obtained in the third step is stacked sequentially with a 5cm*5cm glass fiber separator with electrolyte dripped on it and a 3cm*3cm zinc foil. Carbon cloth is used as the positive electrode tab and the zinc foil as the negative electrode tab to lead out the positive and negative electrodes respectively. Finally, it is encapsulated with an aluminum-plastic film to assemble an aqueous zinc-ion soft-pack battery. The electrolyte used is 2mol / L ZnSO4, and the electrolyte addition amount is 200μL.
[0062] Example 1
[0063] Step 1: Dissolve 2 mmol of ZnSO4·7H2O in 100 ml of deionized water and stir magnetically for 1 h at room temperature to prepare a 2M ZnSO4 electrolyte. Add 1.5 mmol of sodium N-methyltaurate powder to the 2M ZnSO4 electrolyte, stir magnetically for 1 h at room temperature, and then sonicate for 10 min to obtain an aqueous zinc-ion battery electrolyte. Assemble aqueous zinc-ion symmetric batteries and Zn / / Cu batteries using zinc foil with a diameter of 16 mm and a thickness of 0.1 mm and a glass fiber membrane with a diameter of 16 mm and a thickness of 0.1 mm, respectively. The electrolyte used is 2 mol / L ZnSO4 + 1.5 mol / L sodium N-methyltaurate, and the electrolyte addition volume is 50 μL.
[0064] Step 2: Add 0.585 g of NH4VO3 to 35 mL of deionized water. Add 0.9455 g of oxalic acid powder to the solution and stir magnetically. Transfer the solution to a 50 mL hydrothermal reactor and heat at 140 °C for 12 h. After cooling, collect the product, wash with deionized water, and then dry at 70 °C overnight to finally obtain NH4V4O. 10 powder.
[0065] Step 3: The product obtained from the drying process in Step 2 is mixed with a conductive agent and a binder at a mass ratio of 7:2:1 and stirred uniformly at 500 r / min for 24 h. This mixture is then coated onto a 4 cm x 4 cm carbon cloth and dried in an oven at 80 °C for 12 h to obtain the positive electrode of an aqueous zinc-ion soft-pack battery. The conductive agent is Super P, and the binder is polyvinylidene fluoride.
[0066] In the fourth step, the positive electrode obtained in the third step is stacked sequentially with a 7cm*7cm glass fiber separator with electrolyte added and a 4cm*4cm zinc foil. Carbon cloth is used as the positive electrode tab and the zinc foil as the negative electrode tab to lead out the positive and negative electrodes respectively. Finally, it is encapsulated with an aluminum-plastic film to assemble an aqueous zinc-ion soft-pack battery. The electrolyte used is 2mol / L ZnSO4 + 1.5mol / L N-methyltaurate sodium, and the electrolyte addition amount is 50μL.
[0067] Example 2
[0068] Step 1: Dissolve 2 mmol of ZnSO4·7H2O in 100 ml of deionized water and stir magnetically for 1 h at room temperature to prepare a 2M ZnSO4 electrolyte. Add 1 mmol of taurine powder to the 2M ZnSO4 electrolyte, stir magnetically for 1 h at room temperature, and then sonicate for 10 min to obtain an aqueous zinc-ion battery electrolyte. Assemble aqueous zinc-ion symmetric batteries and Zn / / Cu batteries using zinc foil with a diameter of 16 mm and a thickness of 0.1 mm and a glass fiber membrane with a diameter of 16 mm and a thickness of 0.1 mm, respectively. The electrolyte used is 1 mol / L ZnSO4 + 1 mol / L taurine, and the electrolyte addition volume is 80 μL.
[0069] Step 2: Add 0.585 g of NH4VO3 to 35 mL of deionized water. Add 0.9455 g of oxalic acid powder to the solution and stir magnetically. Transfer the solution to a 50 mL hydrothermal reactor and heat at 140 °C for 12 h. After cooling, collect the product, wash with deionized water, and then dry at 70 °C overnight to finally obtain NH4V4O. 10 powder.
[0070] Step 3: The product obtained from the drying in Step 2 is mixed with a conductive agent and a binder at a mass ratio of 7:2:1 and stirred uniformly at 500 r / min for 24 h. This mixture is then coated onto a 10 cm * 10 cm carbon cloth and dried in an oven at 80 °C for 12 h to obtain the positive electrode of an aqueous zinc-ion soft-pack battery. The conductive agent is Super P, and the binder is polyvinylidene fluoride.
[0071] In the fourth step, the positive electrode obtained in the third step is stacked sequentially with a 10cm*10cm glass fiber separator and a 10cm*10cm zinc foil containing electrolyte. Carbon cloth is used as the positive electrode tab, and the zinc foil as the negative electrode tab to lead out the positive and negative electrodes respectively. Finally, the battery is encapsulated with an aluminum-plastic film to assemble an aqueous zinc-ion soft-pack battery. The electrolyte used is 1mol / L ZnSO4 + 1mol / L taurine, and the electrolyte addition amount is 80μL.
[0072] Example 3
[0073] Step 1: Dissolve 2 mmol of ZnSO4·7H2O in 100 ml of deionized water and stir magnetically for 1 h at room temperature to prepare a 2M ZnSO4 electrolyte. Add 1 mmol of ethyl taurate powder to the 2M ZnSO4 electrolyte, stir magnetically for 1 h at room temperature, and then sonicate for 10 min to obtain an aqueous zinc-ion battery electrolyte. Assemble aqueous zinc-ion symmetric batteries and Zn / / Cu batteries using zinc foil with a diameter of 16 mm and a thickness of 0.1 mm and a glass fiber membrane with a diameter of 16 mm and a thickness of 0.1 mm, respectively. The electrolyte used is 2 mol / L ZnSO4 + 1 mol / L ethyl taurate, and the electrolyte addition volume is 100 μL.
[0074] Step 2: Mix 500 mg KMnO4 with 80 ml deionized water to form a homogeneous suspension. Stir and sonicate the mixture for 30 minutes, then transfer it to a 100 ml reactor. Store the mixture in an autoclave at 180°C for 12 hours. Collect the brown product by high-speed centrifugation at 8000 rpm, wash several times with deionized water and ethanol, and dry in an oven at 80°C to obtain the final product MnO2.
[0075] Step 3: The product obtained from the drying in Step 2 is mixed with a conductive agent and a binder at a mass ratio of 7:2:1 and stirred uniformly at 500 r / min for 24 h. This mixture is then coated onto a 5 cm x 5 cm titanium foil and dried in an oven at 80 °C for 12 h to obtain the positive electrode sheet for an aqueous zinc-ion soft-pack battery. The conductive agent is Super P, and the binder is polyvinylidene fluoride.
[0076] In the fourth step, the positive electrode sheet obtained in the third step is stacked sequentially with an 8cm*8cm glass fiber separator with electrolyte droplets and a 5cm*5cm zinc foil. Titanium foil is used as the positive electrode tab, and zinc foil as the negative electrode tab to lead out the positive and negative electrodes respectively. Finally, it is encapsulated with an aluminum-plastic film to assemble an aqueous zinc-ion soft-pack battery. The electrolyte used is 2mol / L ZnSO4 + 1mol / L ethyl taurate, and the electrolyte addition amount is 100μL.
[0077] Example 4
[0078] Step 1: Dissolve 2 mmol of ZnSO4·7H2O in 100 ml of deionized water and stir magnetically for 1 h at room temperature to prepare a 2M ZnSO4 electrolyte. Add 2 mmol of taurine powder to the 2M ZnSO4 electrolyte, stir magnetically for 1 h at room temperature, and then sonicate for 10 min to obtain an aqueous zinc-ion battery electrolyte. Assemble aqueous zinc-ion symmetric batteries and Zn / / Cu batteries using zinc foil with a diameter of 16 mm and a thickness of 0.1 mm and a glass fiber membrane with a diameter of 16 mm and a thickness of 0.1 mm, respectively. The electrolyte used is 2 mol / L ZnSO4 + 2 mol / L taurine, and the electrolyte addition volume is 150 μL.
[0079] Step 2: Add 0.585 g of NH4VO3 to 35 mL of deionized water. Add 0.9455 g of oxalic acid powder to the solution and stir magnetically. Transfer the solution to a 50 mL hydrothermal reactor and heat at 140 °C for 12 h. After cooling, collect the product, wash with deionized water, and then dry at 70 °C overnight to finally obtain NH4V4O. 10 powder.
[0080] Step 3: The product obtained from the drying process in Step 2 is mixed with a conductive agent and a binder at a mass ratio of 7:2:1 and stirred uniformly at 500 r / min for 24 h. This mixture is then coated onto a 10 cm x 10 cm stainless steel foil and dried in an oven at 80 °C for 12 h to obtain the positive electrode of an aqueous zinc-ion soft-pack battery. The conductive agent is Super P, and the binder is polyvinylidene fluoride.
[0081] In the fourth step, the positive electrode obtained in the third step is stacked sequentially with a 10cm*10cm glass fiber separator and a 10cm*10cm zinc foil containing electrolyte. Stainless steel foil is used as the positive electrode tab, and zinc foil as the negative electrode tab, to lead out the positive and negative electrodes respectively. Finally, the assembly is completed using an aluminum-plastic film to form an aqueous zinc-ion soft-pack battery. The electrolyte used is 3mol / L ZnSO4 + 0.1mol / L taurine, and the electrolyte addition amount is 150μL.
[0082] Example 5
[0083] Step 1: Dissolve 2 mmol of ZnSO4·7H2O in 100 ml of deionized water and stir magnetically for 1 h at room temperature to prepare a 2M ZnSO4 electrolyte. Add 1 mmol of taurine powder to the 2M ZnSO4 electrolyte, stir magnetically for 1 h at room temperature, and then sonicate for 10 min to obtain an aqueous zinc-ion battery electrolyte. Assemble aqueous zinc-ion symmetric batteries and Zn / / Cu batteries using zinc foil with a diameter of 16 mm and a thickness of 0.1 mm and a glass fiber membrane with a diameter of 16 mm and a thickness of 0.1 mm, respectively. The electrolyte used is 2 mol / L ZnSO4 + 1 mol / L taurine, and the electrolyte addition volume is 80 μL.
[0084] Step 2: Add 0.585 g of NH4VO3 to 35 mL of deionized water. Add 0.9455 g of oxalic acid powder to the solution and stir magnetically. Transfer the solution to a 50 mL hydrothermal reactor and heat at 140 °C for 12 h. After cooling, collect the product, wash with deionized water, and then dry at 70 °C overnight to finally obtain NH4V4O. 10 powder.
[0085] Step 3: The product obtained from the drying in Step 2 is mixed with a conductive agent and a binder at a mass ratio of 7:2:1 and stirred uniformly at 500 r / min for 24 h. This mixture is then coated onto a 3 cm x 3 cm carbon cloth and dried in an oven at 80 °C for 12 h to obtain the positive electrode sheet for an aqueous zinc-ion soft-pack battery. The conductive agent is Super P, and the binder is polyvinylidene fluoride.
[0086] In the fourth step, the positive electrode sheet obtained in the third step is stacked sequentially with a 5cm*5cm glass fiber separator with electrolyte dripped on it and a 3cm*3cm zinc foil. Carbon cloth is used as the positive electrode tab and the zinc foil as the negative electrode tab to lead out the positive and negative electrodes respectively. Finally, it is encapsulated with an aluminum-plastic film to assemble an aqueous zinc-ion soft-pack battery. The electrolyte used is 2mol / L ZnSO4 + 1mol / L taurine, and the electrolyte addition amount is 200μL.
[0087] Example 6
[0088] Step 1: Dissolve 2 mmol of ZnSO4·7H2O in 100 ml of deionized water and stir magnetically for 1 h at room temperature to prepare a 2M ZnSO4 electrolyte. Add 1 mmol of taurine powder to the 2M ZnSO4 electrolyte, stir magnetically for 1 h at room temperature, and then sonicate for 10 min to obtain an aqueous zinc-ion battery electrolyte. Assemble aqueous zinc-ion symmetric batteries and Zn / / Cu batteries using zinc foil with a diameter of 16 mm and a thickness of 0.1 mm and a glass fiber membrane with a diameter of 16 mm and a thickness of 0.1 mm, respectively. The electrolyte used is 2 mol / L ZnSO4 + 1 mol / L taurine, and the electrolyte addition volume is 80 μL.
[0089] Step 2: Mix 500 mg KMnO4 with 80 ml deionized water to form a homogeneous suspension. Stir and sonicate the mixture for 30 min, then transfer it to a 100 ml reactor. Store the mixture in an autoclave at 180 °C for 12 h. Collect the brown product by high-speed centrifugation at 8000 rpm, wash several times with deionized water and ethanol, and dry in an oven at 80 °C to obtain the final product MnO2.
[0090] Step 3: The product obtained from the drying in Step 2 is mixed with a conductive agent and a binder at a mass ratio of 7:2:1 and stirred uniformly at 500 r / min for 24 h. This mixture is then coated onto a 3 cm x 3 cm carbon cloth and dried in an oven at 80 °C for 12 h to obtain the positive electrode sheet for an aqueous zinc-ion soft-pack battery. The conductive agent is Super P, and the binder is polyvinylidene fluoride.
[0091] In the fourth step, the positive electrode sheet obtained in the third step is stacked sequentially with a 5cm*5cm glass fiber separator with electrolyte dripped on it and a 3cm*3cm zinc foil. Carbon cloth is used as the positive electrode tab and the zinc foil as the negative electrode tab to lead out the positive and negative electrodes respectively. Finally, it is encapsulated with an aluminum-plastic film to assemble an aqueous zinc-ion soft-pack battery. The electrolyte used is 2mol / L ZnSO4 + 1mol / L taurine, and the electrolyte addition amount is 200μL.
[0092] The aqueous zinc-ion symmetric cells obtained in Comparative Example 1, Example 1, and Example 5 were compared at 1 mA cm⁻¹. -2 Current density, 1 mAh cm -2 Cyclic tests were conducted at sedimentation densities, and the results are as follows: Figure 1 As shown, aqueous zinc-ion symmetric batteries containing taurine additives exhibit better cycle stability.
[0093] The aqueous zinc-ion symmetric cells obtained in Comparative Examples 1, 2, and 5 were compared at 5 mA cm⁻¹. -2 Current density, 5mAh cm -2Cyclic tests were conducted at sedimentation densities, and the results are as follows: Figure 2 As shown, aqueous zinc-ion symmetric batteries containing taurine additives exhibit better cycle stability.
[0094] Cyclic tests were conducted on the aqueous zinc-ion symmetric batteries obtained in Comparative Example 1 and Example 5 at different current densities, and the results are as follows: Figure 3 As shown, aqueous zinc-ion symmetric batteries containing taurine additives exhibit better rate performance.
[0095] The aqueous zinc-ion Zn / / Cu batteries obtained in Comparative Examples 1, 3, and 5 were compared at 1 mA cm⁻¹. -2 The current density is 0.5 mAh cm⁻¹. -2 Cyclic tests were conducted at sedimentation densities, and the results are as follows: Figure 4 As shown, aqueous zinc-ion batteries containing taurine additives exhibit better stability in coulombic efficiency.
[0096] The aqueous zinc-ion Zn / / Cu batteries obtained in Comparative Examples 1, 4, and 5 were tested at 5 mA cm⁻¹. -2 Current density, 1 mAh cm -2 Cyclic tests were conducted at sedimentation densities, and the results are as follows: Figure 5 As shown, aqueous zinc-ion batteries containing taurine additives exhibit better stability in coulombic efficiency.
[0097] X-ray diffraction tests were performed on the electrodes of the aqueous zinc-ion Zn / / Cu batteries obtained in Comparative Example 1 and Example 5 after cycling. The results are as follows: Figure 6 As shown, the characteristic peak intensity of byproducts on the surface of the negative electrode of an aqueous zinc-ion battery containing taurine additive is smaller.
[0098] The aqueous zinc-ion pouch cells obtained in Comparative Example 1 and Example 5 were compared at 1 A g. -1 Cyclic tests were conducted at current densities, and the results are as follows: Figure 7 As shown, aqueous zinc-ion batteries containing taurine additives perform better.
[0099] The aqueous zinc-ion pouch cells obtained in Comparative Example 2 and Example 6 were compared at 1 A g. -1 Cyclic tests were conducted at current densities, and the results are as follows: Figure 8 As shown, aqueous zinc-ion batteries containing taurine additives perform better.
[0100] Figure 9 The mechanism of action of taurine additives on the zinc anode interface and electrolyte coordination environment was demonstrated.
[0101] The aqueous zinc-ion battery electrolyte additive proposed in this invention has advantages over existing electrolyte additives, including high biocompatibility, low cost, and excellent electrochemical performance, which is conducive to promoting the practical application of aqueous zinc-ion batteries.
[0102] Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Anyone skilled in the art can make various modifications and alterations without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be determined by the claims.
Claims
1. A soft-pack aqueous zinc-ion battery, characterized in that, Including positive electrode, negative electrode, separator, tabs, aluminum-plastic film, and electrolyte modified with taurine or its derivatives; The internal structure of the soft-pack aqueous zinc-ion battery, from top to bottom, consists of a positive electrode, a separator containing electrolyte, and a negative electrode. The positive electrode is a current collector coated with positive electrode material. The positive and negative electrodes are led out through tabs to serve as the positive and negative electrodes for external connection of the battery. The internal structure is sealed by aluminum-plastic film packaging. The electrolyte modified with taurine or its derivatives includes a zinc salt, water, and an electrolyte additive; the concentration of the zinc salt is 1–3 mol / L, the electrolyte additive is taurine or a taurine derivative, the taurine derivative is ethyl taurate or sodium N-methyltaurate, and the concentration of the electrolyte additive is 1–2 mol / L; the zinc salt is zinc sulfate, and the concentration of the zinc salt is 1–2 mol / L; the concentration of the electrolyte additive is 1–2 mol / L.
2. The soft-pack aqueous zinc-ion battery according to claim 1, characterized in that, The method for preparing the electrolyte modified with taurine or its derivatives includes the following steps: Zinc salts were dissolved in water, stirred and sonicated at room temperature to obtain a zinc salt electrolyte. Taurine or taurine derivatives are added to zinc salt electrolyte, and stirred and sonicated at room temperature to obtain an electrolyte modified with taurine or its derivatives, namely an aqueous zinc-ion battery electrolyte.
3. A soft-pack aqueous zinc-ion battery according to claim 1, characterized in that, The positive electrode material is selected from manganese dioxide or ammonium vanadate.
4. A soft-pack aqueous zinc-ion battery according to claim 1, characterized in that, The negative electrode is made of zinc foil with a purity greater than 99.9%, and the length and width of the negative electrode are 3-10 cm. The diaphragm is made of glass fiber and has a length of 5-10 cm and a width of 5-10 cm. The current collector is made of carbon cloth, stainless steel foil, or titanium foil, and has a length of 3–10 cm and a width of 3–10 cm.
5. A soft-pack aqueous zinc-ion battery according to claim 4, characterized in that, The negative electrode is 3-5 cm long and 3-5 cm wide; The diaphragm is 5 cm long and 5 cm wide; The current collector has a length of 3-5 cm and a width of 3-5 cm.
6. A soft-pack aqueous zinc-ion battery according to claim 1, characterized in that, The electrode tabs are made of carbon cloth, stainless steel foil, titanium foil, or zinc foil.
7. A method for preparing a soft-pack aqueous zinc-ion battery according to any one of claims 1-6, characterized in that, Includes the following steps: The positive electrode material is uniformly mixed with conductive agent and binder, coated onto current collector, and dried to obtain the positive electrode of aqueous zinc-ion soft-pack battery; The obtained positive electrode, the separator with electrolyte, and the negative electrode are stacked together in sequence. The positive and negative electrodes are led out separately with tabs. Finally, they are encapsulated with aluminum-plastic film to assemble an aqueous zinc-ion soft-pack battery.
Citation Information
Patent Citations
Electrolyte additive for zinc battery and application of electrolyte additive
CN115863799A
Negative electrode material for zinc ion battery as well as preparation method and application of negative electrode material
CN115939339A