Strontium-doped iridium-manganese solid solution nanoparticle-carbon nanotube composite and method of making same

By using strontium-doped iridium-manganese solid solution nanoparticles-carbon nanotube composite materials, the problems of low activity and poor stability of IrO₂ catalysts in the oxygen evolution reaction on the anodic side of water electrolysis were solved, achieving high-efficiency acidic OER electrocatalytic performance and long-term stability, while reducing the amount of precious metals used.

CN116732532BActive Publication Date: 2026-11-24SOUTH CHINA UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310631253.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-31
Publication Date
2026-11-24
Estimated Expiration
2043-05-31

AI Technical Summary

Technical Problem

Existing IrO₂ catalysts exhibit low activity and poor stability in the oxygen evolution reaction on the anodic side of water electrolysis, resulting in low utilization of precious metals and instability under acidic or alkaline working conditions.

Method used

A strontium-doped iridium-manganese solid solution nanoparticle-carbon nanotube composite material was adopted. By loading strontium-doped iridium-manganese solid solution nanoparticles onto carbon nanotubes, MnO₂ was used as a support to provide an acidic environment, Sr²⁺ doping was used to improve the electrocatalytic activity and stability of Ir, and CNTs were used to increase the catalytic active sites and conductivity.

Benefits of technology

It improves the catalytic activity and stability of oxygen evolution reaction on the anodic side of water electrolysis, reduces the amount of precious metal Ir used, exhibits excellent electrocatalytic performance under acidic conditions, has low overpotential and high stability, and can be used for a long time under acidic conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116732532B_ABST
    Figure CN116732532B_ABST
Patent Text Reader

Abstract

This invention discloses a strontium-doped iridium-manganese solid solution nanoparticle-carbon nanotube composite material, comprising strontium-doped iridium-manganese solid solution nanoparticles and carbon oxide nanotubes; the strontium-doped iridium-manganese solid solution nanoparticles are loaded on the surface of carbon oxide nanotubes; the composition of the strontium-doped iridium-manganese solid solution nanoparticles is Sr. x Ir y Mn 1‑x‑ y O2, where 0.08 ≤ x < 0.30, 0.08 ≤ y < 0.50, 0.16
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of preparation of anode catalysts for water electrolysis, and particularly to strontium-doped iridium-manganese solid solution nanoparticles-carbon nanotubes (Sr... x Ir y Mn 1-x-y O2 / CNTs composite materials and their preparation methods. Background Technology

[0002] Hydrogen, as a clean energy source, boasts advantages such as high energy density and pollution-free reaction products, making its application highly promising. Hydrogen can be obtained through water electrolysis, a process with widely available and inexpensive raw materials, producing high-purity hydrogen without other pollution. The reaction is driven by renewable electricity, making the entire process clean and efficient. The theoretical driving potential for water electrolysis is 1.23V, but due to kinetic losses in the anode and cathode half-reactions, the actual driving voltage is higher than the theoretical value. Compared to the hydrogen evolution reaction on the cathode side involving two electron transfers, the oxygen evolution reaction (OER) on the anode side of water electrolysis involves four electron / proton transfers, resulting in slow kinetics. The deprotonation step of the reaction intermediate *OH and the desorption process of *OOH are the rate-determining steps of the water electrolysis reaction. Lowering the rate-determining step energy barrier can effectively improve the overall reaction rate of water electrolysis; therefore, it is necessary to develop efficient catalysts to reduce kinetic losses in water electrolysis and increase the energy conversion efficiency. Iridium dioxide (IrO2) and ruthenium dioxide (RuO2) are currently recognized in the industry as catalysts with superior performance and stability; however, their high price and resource scarcity hinder their large-scale application. Although these two catalysts exhibit good activity and stability among OER candidate catalysts, harsh acid-base operating environments and high operating voltages in practical applications often cause Ir and Ru to degrade into higher valence states. Therefore, developing OER catalysts with high activity, low noble metal content, and long-term operational stability has become a current research hotspot.

[0003] Among many catalysts, although IrO2 has lower OER catalytic activity than RuO2, its catalytic durability is better than RuO2. In addition, Ir is more expensive than Ru. Therefore, further improving the utilization rate of Ir, enhancing its catalytic activity and long-term durability are still problems that cannot be solved by existing technologies. Summary of the Invention

[0004] In order to overcome the above-mentioned shortcomings and deficiencies of the prior art, the present invention aims to provide a strontium-doped iridium-manganese solid solution nanoparticle-carbon nanotube composite material, which reduces the amount of Ir used, achieves higher OER catalytic activity and stability, and solves the problems of low activity, poor stability and low utilization of precious metals of traditional IrO2 catalysts.

[0005] Another object of the present invention is to provide a method for preparing the above-mentioned strontium-doped iridium-manganese solid solution nanoparticle-carbon nanotube composite material.

[0006] The objective of this invention is achieved through the following technical solution:

[0007] A strontium-doped iridium-manganese solid solution nanoparticle-carbon nanotube composite material comprises strontium-doped iridium-manganese solid solution nanoparticles and carbon oxide nanotubes; the strontium-doped iridium-manganese solid solution nanoparticles are loaded on the surface of carbon oxide nanotubes; the composition of the strontium-doped iridium-manganese solid solution nanoparticles is Sr. x Ir y Mn 1-x-y O2, where 0.08≤x<0.30, 0.08≤y<0.50, and 0.16≤x+y<0.50.

[0008] Preferably, the value of x is between 0.1 and 0.42.

[0009] Preferably, the value of y is between 0.1 and 0.2.

[0010] The preparation method of the strontium-doped iridium-manganese solid solution nanoparticle-carbon nanotube composite material includes the following steps:

[0011] Carbon oxide nanotubes were dispersed in water and subjected to a hydrothermal reaction with soluble iridium salt, soluble manganese salt and soluble strontium salt to obtain carbon oxide nanotubes loaded with strontium-doped iridium-manganese solid solution nanoparticles.

[0012] Strontium-doped iridium-manganese solid solution nanoparticles were calcined in air to obtain a strontium-doped iridium-manganese solid solution nanoparticle-carbon nanotube composite material.

[0013] Preferably, the hydrothermal reaction is carried out at 120–160°C for 1–3 hours.

[0014] Preferably, the carbon oxide nanotubes are prepared as follows:

[0015] Carbon nanotubes are dispersed in an acid solution and subjected to acidification treatment to obtain carbon oxide nanotubes.

[0016] Preferably, the acid solution is a mixed acid prepared from concentrated sulfuric acid and concentrated nitric acid; the acidification treatment is carried out at 70-90°C for 2-6 hours.

[0017] Preferably, the acid solution is a mixed acid prepared from concentrated sulfuric acid and concentrated nitric acid.

[0018] Preferably, the calcination temperature is 200–400 °C. oC; More preferably, the calcination specifically involves: first controlling the heating rate at 2-5℃ / min to raise the temperature from room temperature to 200-400℃, then holding the temperature for 1-3 hours, and then controlling the cooling rate at 2-5℃ / min to cool down to room temperature.

[0019] Preferably, the mass ratio of the carbon oxide nanotubes, soluble iridium salt, soluble manganese salt, and soluble strontium salt is 1.00:0.08-0.83:0.26-0.45:0.20-1.40.

[0020] Preferably, the particle size of the strontium-doped iridium-manganese solid solution nanoparticles is 0.5–10.0 nm.

[0021] More preferably, the strontium-doped iridium-manganese solid solution nanoparticles have a particle size of 0.5–5.0 nm.

[0022] Preferably, the acid solution is a mixed acid prepared by combining sulfuric acid (95-98% by mass) and nitric acid (68-70% by mass) in a volume ratio of 2.8-3.2:1.

[0023] Preferably, the soluble iridium salt is at least one of iridium trichloride (IrCl3) and chloroiridium acid (H2IrCl6); more preferably, the soluble iridium salt is iridium trichloride.

[0024] Preferably, the soluble manganese salt is at least one of potassium permanganate (KMnO4) and manganese chloride (MnCl2); more preferably, the soluble manganese salt is potassium permanganate.

[0025] Preferably, the soluble strontium salt is at least one of strontium nitrate (Sr(NO3)2) and strontium chloride (SrCl2); more preferably, the soluble strontium salt is strontium nitrate.

[0026] The principle of this invention is as follows:

[0027] The Sr of the present invention x Ir y Mn 1-x-y In O2 / CNTs composites, MnO2 acts as a support, providing an acid-resistant environment for Ir; furthermore, relative to Ir... 4+ The electronegativity of Mn is even stronger. 4+ Able to Ir 4+ The surrounding electrons attract each other, reducing the charge density of the Ir5d orbitals. Due to the enhanced covalentity between Ir and O, the Ir-O bonds become stronger, thereby increasing the proton attack resistance of the lattice oxygen. After optimizing the optimal Ir doping level, Sr doping is then performed. 2+ In replacing Mn 4 +Subsequently, to maintain electroneutrality, the material generates some oxygen vacancies and increases the leaching energy consumption of Ir, further enhancing the electrocatalytic activity and stability of the material while reducing the amount of Ir used. Furthermore, this invention combines CNTs with catalyst particles. CNTs act as conductive pathways, transporting electrons, and their high specific surface area exposes more catalytically active sites. This increases the contact area between the catalyst and reactants, further enhancing catalytic activity. Moreover, it allows for the use of less catalyst supported on carbon nanotubes to achieve the same current density, further reducing the use of precious metals.

[0028] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0029] (1) The Sr of the present invention x Ir y Mn 1-x-y O2 / CNTs composite materials exhibit excellent electrocatalytic activity and stability under acidic conditions for OER, and can be used as OER electrocatalysts under acidic conditions.

[0030] (2) Low overpotential

[0031] The acidic OER electrocatalytic test results show that the Sr of this invention x Ir y Mn 1-x-y The overpotential of O2 / CNT composites is between 235.0 and 300.0 mV, for example, Sr 0.13 Ir 0.27 Mn 0.60 O2 / CNTs, at 10 mA cm -2 At the given current density, the overpotential is only 237.0 mV.

[0032] (3) Excellent OER stability

[0033] Stability tests were conducted in 0.5 M H₂SO₄ (current density 10 mA cm⁻¹). -2 Loading capacity 2.0 mg cm -2 The Sr disclosed in this invention 0.13 Ir 0.26 Mn 0.61 The O2 / CNTs composite material maintained high catalytic activity without significant degradation even after 300 hours of continuous operation.

[0034] (4) The Sr of the present invention x Ir y Mn 1-x-yIn O2 / CNTs composite materials, Sr acts as a dopant in the oxide, which can reduce the overpotential of OER and enhance the stability of the catalyst under acidic conditions.

[0035] (5) The Sr of the present invention x Ir y Mn 1-x-y The O2 / CNTs composite material uses carbon nanotubes as a carrier and Ir and Sr as dopants incorporated into the MnO2 lattice. This dual-element doping method reduces the anodic overpotential of the OER, while simultaneously reducing the amount of noble metal Ir used and improving the OER stability under acidic conditions.

[0036] (6) The present invention solves the problem of the instability of Ir-based catalysts as OER anodes under acidic conditions and at high potentials. Attached Figure Description

[0037] Figure 1 Sr prepared for embodiments of the present invention 0.13 Ir 0.26 Mn 0.61 SEM image of O2 / CNTs OER catalyst;

[0038] Figure 2 Sr prepared for embodiments of the present invention 0.13 Ir 0.26 Mn 0.61 Powder XRD pattern of O2 / CNTs OER catalyst;

[0039] Figure 3 Sr prepared for embodiments of the present invention 0.13 Ir 0.26 Mn 0.61 (a) TEM image of O2 / CNTs OER catalyst; (b) HAADF-STEM image; (c) magnified HAADF-STEM image.

[0040] Figure 4 Sr prepared for embodiments of the present invention 0.13 Ir 0.26 Mn 0.61 EDS mapping diagram of O2 / CNTs OER catalyst.

[0041] Figure 5 Sr prepared for embodiments of the present invention 0.13 Ir 0.26 Mn 0.61 OER test results of O2 / CNTs OER catalyst in 0.5M H2SO4: (a) LSV polarization curve; (b) Tafel slope; (c) EIS curve.

[0042] Figure 6 (a) shows the LSV polarization curves of iridium-manganese solid solution nanoparticle-carbon nanotube composites with different Ir contents prepared in the embodiments of the present invention in 0.5M H2SO4; (b) shows the LSV polarization curves of iridium-manganese solid solution nanoparticle-carbon nanotube composites with different Sr doping in 0.5M H2SO4.

[0043] Figure 7 For Sr 0.13 Ir 0.26 Mn 0.61 O2 / CNTs and Ir 0.30 Mn 0.70 Comparison of the stability of O2 / CNT catalysts in 0.5 M H2SO4. (Carbon paper 1.0 × 1.0 cm) 2 The catalyst loading is approximately 2.0 mg cm⁻¹ -2 ). Detailed Implementation

[0044] The present invention will be further described in detail below with reference to the embodiments, but the implementation of the present invention is not limited thereto.

[0045] Example 1

[0046] An iridium-manganese solid solution nanoparticle-carbon nanotube composite material doped with 11.0% Ir atomic weight (named Ir) 0.11 Mn 0.89 Preparation of O2 / CNTs:

[0047] Preparation method of carbon nanotube oxide: In this work, carbon nanotube oxide (CNTs) was prepared by surface oxidation of carbon nanotubes (CNTs). The specific steps are as follows: First, 30.0-60.0 mL of 98% concentrated sulfuric acid and 10.0-30.0 mL of 68% concentrated nitric acid were mixed evenly to form a homogeneous solution. The volume ratio of sulfuric acid to nitric acid was 3:1. A reaction flask was assembled in a water bath apparatus, and the above-mentioned homogeneous acid mixture was added. Then, under stirring, 200.0-500.0 mg of dried CNTs were dissolved in the above-mentioned acid mixture. The solution was stirred vigorously at 40-80°C. o The reaction proceeds at C for 2-4 hours. A large quantity of pure water is prepared beforehand. After the reaction is complete, the above black mixed solution is slowly poured into the pure water under mechanical stirring to dilute it. The diluted reaction liquid is then poured into a vacuum filter and washed repeatedly with pure water until neutral. Carbon oxide nanotubes are collected. Finally, the washed carbon oxide nanotubes are dispersed in water to a concentration of 5.0 mg / mL. -1 .

[0048] Ir0.11 Mn 0.89 Preparation of O2 / CNTs: First, weigh out certain amounts of IrCl3 (Ir≥62.0%) and KMnO4 (≥99.5%) and prepare 0.005 M and 0.02 M aqueous solutions, respectively. Then, add 0.50-6.0 mL of 0.005 M IrCl3 solution and 1.0-5.0 mL of 5.0 mg / mL... -1 IrCl3 nanotubes were dispersed in 15.0 mL of deionized water to form a homogeneous solution. Then, 2.0–5.0 mL of 0.02 M KMnO4 was gradually added dropwise to the solution under continuous mechanical stirring. Next, pure water was added to the solution to prepare a homogeneous solution of 30.0–40.0 mL. The molar ratio of IrCl3 to KMnO4 was 1:9. The homogeneous solution was then sealed in a 50.0 mL reactor and incubated at 100–140 °C. o The reaction was carried out at C for 2-5 hours. After the reaction was complete, the product was separated by centrifugation and washed with pure water. The product was then incubated at 60-80°C. o Keep in a constant temperature oven at C for 2-5 hours until completely dry. Finally, heat the dried solid powder at 300-500°C. o Heat treatment in a muffle furnace of C for 2-5 hours yields Ir 0.11 Mn 0.89 O2 / CNTs.

[0049] Example 2

[0050] An iridium-manganese solid solution nanoparticle-carbon nanotube composite material doped with 17.0% Ir atomic weight (named Ir) 0.17 Mn 0.83 Preparation of O2 / CNTs:

[0051] The preparation method of carbon oxide nanotubes is the same as that in Example 1.

[0052] Ir 0.17 Mn 0.83 Preparation of O2 / CNTs: First, weigh out certain amounts of IrCl3 (Ir≥62.0%) and KMnO4 (≥99.5%) and prepare 0.005 M and 0.02 M aqueous solutions, respectively. Then, add 0.50-6.0 mL of 0.005 M IrCl3 solution and 1.0-5.0 mL of 5.0 mg / mL... -1IrCl3 nanotubes were dispersed in 15.0 mL of deionized water to form a homogeneous solution. Then, 2.0–5.0 mL of 0.02 M KMnO4 was gradually added dropwise to the solution under continuous mechanical stirring. Next, pure water was added to the solution to prepare a homogeneous solution of 30.0–40.0 mL. The molar ratio of IrCl3 to KMnO4 was 1:4. The homogeneous solution was then sealed in a 50.0 mL reactor and incubated at 100–140 °C. o The reaction was carried out at C for 2-5 hours. After the reaction was complete, the product was separated by centrifugation and washed with pure water. The product was then incubated at 60-80°C. o Keep in a constant temperature oven at C for 2-5 hours until completely dry. Finally, heat the dried solid powder at 300-500°C. o Heat treatment in a muffle furnace of C for 2-5 hours yields Ir 0.17 Mn 0.83 O2 / CNTs.

[0053] Example 3

[0054] An iridium-manganese solid solution nanoparticle-carbon nanotube composite material doped with 30.0% Ir atomic weight (named Ir) 0.30 Mn 0.70 Preparation of O2 / CNTs:

[0055] The preparation method of carbon oxide nanotubes is the same as that in Example 1.

[0056] Ir 0.30 Mn 0.70 Preparation of O2 / CNTs: First, weigh out certain amounts of IrCl3 (Ir≥62.0%) and KMnO4 (≥99.5%) and prepare 0.005 M and 0.02 M aqueous solutions, respectively. Then, add 0.50-6.0 mL of 0.005 M IrCl3 solution and 1.0-5.0 mL of 5.0 mg / mL... -1 IrCl3 nanotubes were dispersed in 15.0 mL of deionized water to form a homogeneous solution. Then, 2.0-5.0 mL of 0.02 M KMnO4 was gradually added dropwise to the solution under continuous mechanical stirring. Next, pure water was added to the solution to prepare a homogeneous solution of 30.0-40.0 mL. The molar ratio of IrCl3 to KMnO4 was 1:2. The homogeneous solution was then sealed in a 50.0 mL reactor and incubated at 100-140 °C. o The reaction was carried out at C for 2-5 hours. After the reaction was complete, the product was separated by centrifugation and washed with pure water. The product was then incubated at 60-80°C. o Keep in a constant temperature oven at C for 2-5 hours until completely dry. Finally, heat the dried solid powder at 300-500°C. oHeat treatment in a muffle furnace of C for 2-5 hours yields Ir 0.30 Mn 0.70 O2 / CNTs.

[0057] Example 4

[0058] An iridium-manganese solid solution nanoparticle-carbon nanotube composite material with an Ir atomic weight percentage of 41.0% (named Ir) 0.41 Mn 0.59 Preparation of O2 / CNTs:

[0059] The preparation method of carbon oxide nanotubes is the same as that in Example 1.

[0060] Ir 0.41 Mn 0.59 Preparation of O2 / CNTs: First, weigh out certain amounts of IrCl3 (Ir≥62.0%) and KMnO4 (≥99.5%) and prepare 0.005 M and 0.02 M aqueous solutions, respectively. Then, add 0.50-6.0 mL of 0.005 M IrCl3 solution and 1.0-5.0 mL of 5.0 mg / mL... -1 IrCl3 nanotubes were dispersed in 15.0 mL of deionized water to form a homogeneous solution. Then, 2.0–5.0 mL of 0.02 M KMnO4 was gradually added dropwise to the solution under continuous mechanical stirring. Next, pure water was added to the solution to prepare a homogeneous solution of 30.0–40.0 mL. The molar ratio of IrCl3 to KMnO4 was 3:4. The homogeneous solution was then sealed in a 50.0 mL reactor and incubated at 100–140 °C. o The reaction was carried out at C for 2-5 hours. After the reaction was complete, the product was separated by centrifugation and washed with pure water. The product was then incubated at 60-80°C. o Keep in a constant temperature oven at C for 2-5 hours until completely dry. Finally, heat the dried solid powder at 300-500°C. o Heat treatment in a muffle furnace of C for 2-5 hours yields Ir 0.41 Mn 0.59 O2 / CNTs.

[0061] Example 5

[0062] Preparation of manganese oxide nanoparticle-carbon nanotube composite material (named MnO2 / CNTs):

[0063] The preparation method of carbon oxide nanotubes is the same as that in Example 1.

[0064] Preparation of MnO2 / CNTs: First, a certain amount of KMnO4 (≥99.5%) was weighed and prepared into a 0.02 M aqueous solution. Then, 1.0–5.0 mL of a 5.0 mg / mL solution was added. -1 Carbon nanotubes were dispersed in 15.0 mL of deionized water to form a homogeneous solution. Then, 2.0-5.0 mL of 0.02 M KMnO4 was gradually added dropwise to the solution under continuous mechanical stirring. Next, pure water was added to the solution to prepare a homogeneous solution of 30.0-40.0 mL. The homogeneous solution was then sealed in a 50.0 mL reactor and incubated at 100-140 °C. o The reaction was carried out at C for 2-5 hours. After the reaction was complete, the product was separated by centrifugation and washed with pure water. The product was then incubated at 60-80°C. o Keep in a constant temperature oven at C for 2-5 hours until completely dry. Finally, heat the dried solid powder at 300-500°C. o MnO2 / CNTs were obtained by heat treatment in a muffle furnace of C for 2-5 h.

[0065] Example 6

[0066] Preparation of Sr-doped iridium-manganese solid solution nanoparticle-carbon nanotube composites with Sr atomic weights of 10.0%, 13.0%, and 17.0%:

[0067] The preparation method of carbon oxide nanotubes is the same as that in Example 1.

[0068] A strontium-doped iridium-manganese solid solution nanoparticle-carbon nanotube composite material with an Ir atomic percentage of 26.0% and a Sr atomic percentage of 13.0% (named Sr) 0.13 Ir 0.26 Mn 0.61 Preparation of O2 / CNTs: First, weigh certain amounts of IrCl3 (Ir≥62.0%), Sr(NO3)2 (≥99.5%), and KMnO4 (≥99.5%) to prepare 0.005 M, 0.02 M, and 0.02 M aqueous solutions, respectively. Then, add 0.50–6.0 mL of 0.005 M IrCl3 solution, 2.0–5.0 mL of 0.02 M Sr(NO3)2, and 1.0–5.0 mL of a 5.0 mg / mL solution. -1Sr(NO3)2, IrCl3, and KMnO4 were dispersed in 15.0 mL of deionized water to form a homogeneous solution. Then, 2.0–5.0 mL of 0.02 M KMnO4 was gradually added dropwise to the solution while maintaining continuous mechanical stirring. Finally, pure water was added to the solution to prepare a homogeneous solution of 30.0–40.0 mL. The molar ratio of Sr(NO3)2, IrCl3, and KMnO4 was 3:1:2. The homogeneous solution was then sealed in a 50.0 mL reactor and incubated at 100–140 °C. o The reaction was carried out at C for 2-5 hours. After the reaction was complete, the product was separated by centrifugation and washed with pure water. The product was then incubated at 60-80°C. o Keep in a constant temperature oven at C for 2-5 hours until completely dry. Finally, heat the dried solid powder at 300-500°C. o Heat treatment of C in a muffle furnace for 2-5 hours yields Sr 0.13 Ir 0.26 Mn 0.61 O2 / CNTs.

[0069] By changing the molar ratio of Sr(NO3)2, IrCl3, and KMnO4 to 1:2:1, 3:1:2, or 4:2:1, strontium-doped iridium-manganese solid solution nanoparticle-carbon nanotube composites (named Sr) with different atomic percentages can be obtained using the same steps. 0.10 Ir 0.27 Mn 0.63 O2 / CNTs, Sr 0.13 Ir 0.26 Mn 0.61 O2 / CNTs and Sr 0.17 Ir 0.25 Mn 0.58 O2 / CNTs).

[0070] Test results:

[0071] Figure 1 Sr prepared for embodiments of the present invention 0.13 Ir 0.26 Mn 0.61 SEM image of O2 / CNTs OER catalyst; From the image, we can see that: Sr 0.13 Ir 0.26 Mn 0.61 O2 / CNTs are produced by Sr 0.13 Ir 0.26 Mn 0.61 It consists of O2 nanoparticles and carbon nanotubes, with the particles uniformly distributed on the surface of the carbon nanotubes and no aggregation.

[0072] Figure 2 Sr prepared for embodiments of the present invention 0.13 Ir 0.26Mn 0.61 Powder XRD pattern of O2 / CNTs solid solution material; From the figure, it can be seen that: Sr 0.13 Ir 0.26 Mn 0.61 The XRD pattern of O2 / CNTs is formed by superimposing the XRD patterns of carbon nanotubes and MnO2.

[0073] Figure 3 Sr prepared for embodiments of the present invention 0.13 Ir 0.26 Mn 0.61 (a) TEM image of O2 / CNTs OER catalyst; (b) HAADF-STEM image; (c) magnified HAADF-STEM image; From the images, it can be seen that Sr 0.13 Ir 0.26 Mn 0.61 The O2 / CNTs nanoparticles are composed of single crystals with an average particle size of 1.56 nanometers. They have distinct lattice fringes and correspond to XRD standard cards.

[0074] Figure 4 Sr prepared for embodiments of the present invention 0.13 Ir 0.26 Mn 0.61 EDS mapping diagram of O2 / CNTs OER catalyst. It can be seen that Sr... 0.13 Ir 0.26 Mn 0.61 O2 / CNTs are composed of C, Sr, Ir, Mn and O elements, and each element is uniformly distributed along the material profile.

[0075] Figure 5 Sr prepared for embodiments of the present invention 0.13 Ir 0.26 Mn 0.61 OER test results of O2 / CNTs OER catalyst in 0.5 M H2SO4: (a) LSV polarization curve; (b) Tafel slope; (c) EIS curve.

[0076] Figure 6(a) shows the LSV polarization curves of iridium-manganese solid solution nanoparticle-carbon nanotube composites with different Ir contents prepared in the embodiments of the present invention in 0.5 M H2SO4; (b) shows the LSV polarization curves of strontium-doped iridium-manganese solid solution nanoparticle-carbon nanotube composites with different Sr doping amounts in 0.5 M H2SO4. As can be seen from the figures, the performance of the iridium-manganese solid solution nanoparticle-carbon nanotube composites shows a trend of first increasing and then decreasing with increasing Ir content. When Ir:(Ir+Mn)=0.30, the iridium-manganese solid solution nanoparticle-carbon nanotube composite exhibits relatively good catalytic activity, with a current density of 10 mA cm⁻¹. -2 The overpotential variation range was 253–590 mV. The performance of the strontium-doped iridium-manganese solid solution nanoparticle-carbon nanotube composite material showed a trend of first increasing and then decreasing with the Sr doping amount. When Sr:(Sr+Ir+Mn)=0.13, the strontium-doped iridium-manganese solid solution nanoparticle-carbon nanotube composite material exhibited relatively good catalytic activity, with a current density of 10 mA cm⁻¹. -2 The overpotential variation range was 237–253 mV. Sr doping slightly enhanced the catalytic activity of iridium-manganese solid solution nanoparticle-carbon nanotube composites, but significantly improved their catalytic stability. Figure 6 As shown in (b), Sr 0.13 Ir 0.26 Mn 0.61 O2 / CNTs at a current density of 10 mA cm⁻¹ -2 The overpotential at that time is only greater than Ir 0.31 Mn 0.69 O2 / CNTs are about 16 mV lower, but their stability is better than Ir. 0.30 Mn 0.70 O2 / CNTs significantly increased ( Figure 7 ).

[0077] Figure 7 Sr prepared for embodiments of the present invention 0.13 Ir 0.26 Mn 0.61 O2 / CNTs and Ir 0.30 Mn 0.70 Comparison of the stability of O2 / CNT catalysts in 0.5 M H2SO4. (Carbon paper 1.0 × 1.0 cm) 2 The catalyst loading is approximately 2.0 mg cm⁻¹ -2 This indicates that Sr doping can effectively improve the catalytic stability of iridium-manganese solid solution nanoparticle-carbon nanotube composite materials.

[0078] In the above embodiments, the volume ratio of sulfuric acid to nitric acid should not be limited to the 3:1 ratio, but can be other ratios, and the carbon nanotubes with surface oxidation can be obtained in the same way.

[0079] The Sr(NO3)2 used in the above embodiments is not limited to Sr(NO3)2, and SrCl2 can also be used. The IrCl3 used is not limited to IrCl3, and Ir precursors such as H2IrCl6 can also be used instead.

[0080] The above embodiments are preferred embodiments of the present invention, but the embodiments of the present invention are not limited to the embodiments described above. Any changes, modifications, substitutions, combinations, or simplifications made without departing from the spirit and principle of the present invention shall be considered equivalent substitutions and shall be included within the protection scope of the present invention.

Claims

1. A strontium-doped iridium-manganese solid solution nanoparticle-carbon nanotube composite material, characterized in that, It includes strontium-doped iridium-manganese solid solution nanoparticles and carbon oxide nanotubes; the strontium-doped iridium-manganese solid solution nanoparticles are supported on the surface of carbon oxide nanotubes; in the strontium-doped iridium-manganese solid solution nanoparticles, Ir and Sr are incorporated as dopants into the MnO2 lattice, and the composition is Sr x Ir y Mn 1-x-y O2, where 0.08≤x<0.30, 0.08≤y<0.50, and 0.16≤x+y<0.

50.

2. The strontium-doped iridium-manganese solid solution nanoparticle-carbon nanotube composite material according to claim 1, characterized in that, The value of x ranges from 0.1 to 0.

30.

3. The strontium-doped iridium-manganese solid solution nanoparticle-carbon nanotube composite material according to claim 1, characterized in that, The value of y is between 0.1 and 0.

2.

4. The method for preparing the strontium-doped iridium-manganese solid solution nanoparticle-carbon nanotube composite material according to any one of claims 1 to 3, characterized in that, Includes the following steps: Carbon oxide nanotubes were dispersed in water and subjected to a hydrothermal reaction with soluble iridium salt, soluble manganese salt and soluble strontium salt to obtain carbon oxide nanotubes loaded with strontium-doped iridium-manganese solid solution nanoparticles. Strontium-doped iridium-manganese solid solution nanoparticles were calcined in air to obtain a strontium-doped iridium-manganese solid solution nanoparticle-carbon nanotube composite material.

5. The method for preparing the strontium-doped iridium-manganese solid solution nanoparticle-carbon nanotube composite material according to claim 4, characterized in that, The hydrothermal reaction is carried out at 120–160°C for 1–3 hours.

6. The method for preparing the strontium-doped iridium-manganese solid solution nanoparticle-carbon nanotube composite material according to claim 4, characterized in that, The carbon oxide nanotubes are prepared as follows: Carbon nanotubes are dispersed in an acid solution and subjected to acidification treatment to obtain carbon oxide nanotubes.

7. The method for preparing the strontium-doped iridium-manganese solid solution nanoparticle-carbon nanotube composite material according to claim 6, characterized in that, The acid solution is a mixed acid prepared from concentrated sulfuric acid and concentrated nitric acid; the acidification treatment is carried out at 70-90°C for 2-6 hours.

8. The method for preparing the strontium-doped iridium-manganese solid solution nanoparticle-carbon nanotube composite material according to claim 4, characterized in that, The calcination temperature is 200–400°C. o C.

9. The method for preparing the strontium-doped iridium-manganese solid solution nanoparticle-carbon nanotube composite material according to claim 4, characterized in that, The mass ratio of the carbon oxide nanotubes, soluble iridium salt, soluble manganese salt, and soluble strontium salt is 1.00:0.08~0.83:0.26~0.45:0.20~1.40.