A method for preparing a high specific capacity low voltage anode foil
By combining thermal spraying and ultrasonic atomization spraying, a multilayer aluminum powder layer and a high dielectric constant layer are formed on the surface of aluminum foil, which solves the problems of improving the specific capacitance and bonding strength of the anode foil and realizes the efficient and stable preparation of aluminum electrolytic capacitor anode foil.
Patent Information
- Application Number
- CN202310792451.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-30
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-06-30
AI Technical Summary
The current method for improving the specific capacitance of aluminum electrolytic capacitor anode foil is difficult to ensure both uniformity and bonding strength. Furthermore, the low efficiency of the manufacturing process leads to easy delamination and peeling of the electrode foil during application, which limits its application scenarios.
A combination of thermal spraying and ultrasonic atomization spraying is used to form multiple layers of aluminum powder and a high dielectric constant layer on the surface of aluminum foil. Combined with annealing and anodizing treatment, the bonding strength between each layer and the uniform distribution of dielectric material are ensured.
It improves the specific capacity of the anode foil, enhances its mechanical and electrical properties, simplifies the preparation process, and is suitable for industrial production.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] This invention relates to the field of electrode foil manufacturing technology, and in particular to a method for preparing a high specific capacity, low pressure anode foil. Background Technology
[0002] With the increasing demand for miniaturization and weight reduction in aluminum electrolytic capacitors, higher requirements are being placed on the specific capacitance of the aluminum anode foil.
[0003] As is generally known, increasing the specific surface area and adding dielectric material can both effectively improve the specific capacitance of anode foil. Regarding increasing the specific surface area, corrosion-based surface area expansion technology has reached its limits after many years of development, making further breakthroughs difficult. Therefore, increasing the dielectric content while increasing the specific surface area has become a research hotspot in recent years. For example, Chinese invention patent CN2022109209854 discloses a method for preparing a high-dielectric composite powder sintered foil. This method involves mixing aluminum powder, binder, and additives in an organic solvent to obtain a slurry, coating it onto the surface of an aluminum foil, drying and curing it into a film, and then sintering it at high temperature to obtain a powder sintered foil. The powder sintered foil is then immersed in a titanium-containing precursor solution, drained, and sintered at high temperature to obtain a composite sintered foil. Specific experimental data demonstrate that the above technical solution not only achieves a larger specific surface area but also ensures the doping amount of metal oxides in the alumina layer of the electrode foil. Combining these two factors significantly improves the specific capacitance of the aluminum electrode foil. However, there are two significant shortcomings: 1) During the coating process, it is difficult to ensure that the mixed slurry is uniformly and evenly coated on the aluminum foil surface, easily leading to sagging. Furthermore, a considerable amount of time is required for subsequent sintering and curing, hindering the improvement of finished product efficiency. 2) Due to limitations in the manufacturing process, the bonding strength between the powder sintered layer and the aluminum foil, as well as between the titanium dioxide film and the powder sintered layer, is insufficient. This inevitably leads to delamination and peeling of the electrode foil in practical applications, weakening its electrical performance. Moreover, while the bending performance of the electrode foil is acceptable, repeated bending drastically exacerbates the delamination and peeling problems, severely limiting the expansion of electrode foil application scenarios. Therefore, it is imperative for technical personnel to address these issues. Summary of the Invention
[0004] Therefore, in view of the above-mentioned existing problems and defects, the designers of this invention collected relevant information, conducted multiple evaluations and considerations, and carried out continuous experiments and modifications by technical personnel with many years of R&D experience in this industry, which ultimately led to the emergence of this method for preparing high specific capacity low pressure anode foil.
[0005] To address the aforementioned technical problems, the present invention relates to a method for preparing a high specific capacity, low pressure anode foil, comprising the following steps: S1. Select aluminum foil; the thickness of the aluminum foil should be controlled between 50 and 60 μm, and the purity should be above 99.95%; S2. Perform surface cleaning treatment on the aluminum foil obtained in step S1; S3. Immerse the aluminum foil obtained in step S2 into an acid solution to simultaneously etch its front and back surfaces, and control the etching depth on one side to 3-5 μm. S4. Use clean water to perform high-pressure rinsing on the aluminum foil obtained in step S3, and then dry it. S5. Simultaneously, using the first thermal spraying equipment and the second thermal spraying equipment, high-purity aluminum powder is sprayed onto the front and back sides of the aluminum foil obtained in step S4 to form the first aluminum powder layer and the second aluminum powder layer; the thickness of the first aluminum powder layer and the second aluminum powder layer are both controlled to be 5-8 μm. S6. Using the first ultrasonic atomizing device and the second ultrasonic atomizing device, the high dielectric sol is attached to the front and back sides of the aluminum foil obtained in step S5, so as to continue to grow along the thickness direction of the first aluminum powder layer and the second aluminum powder layer respectively to form the first high dielectric constant layer and the second high dielectric constant layer; the thickness of the first high dielectric constant layer and the second high dielectric constant layer are both controlled at 2 to 3 μm; S7. Simultaneously, using the third and fourth thermal spraying devices, high-purity aluminum powder is sprayed onto the front and back sides of the aluminum foil obtained in step S6, respectively, to continue growing along the thickness direction of the first high dielectric constant layer and the second high dielectric constant layer to form the third aluminum powder stack and the fourth aluminum powder stack; the thickness of the third aluminum powder stack and the fourth aluminum powder stack are both controlled at 5 to 8 μm. S8. Perform annealing treatment on the aluminum foil obtained in step S7; S9. Immerse the aluminum foil obtained in step S8 in an aqueous solution of 10-20% (by mass) ammonium adipate, and maintain the temperature at 65-95°C and a current density of 20 mA / cm². 2 Anodizing process S10 is performed under a voltage of 8-36V. The aluminum foil obtained in step S9 is then washed and dried to obtain a high specific capacity low pressure anode foil product.
[0006] As a further improvement to the technical solution disclosed in this invention, step S2 includes the following sub-steps: S21. Immerse the aluminum foil obtained in step S1 in a 0.5-1.0 mol / L NaOH solution to remove impurities and oil stains from its front and back surfaces. S22. Use clean water to clean the aluminum foil obtained in step S21 and then dry it.
[0007] As a further improvement to the technical solution disclosed in this invention, in step S3, the acid solution is preferably any one or a mixture of several of hydrochloric acid, sulfuric acid, nitric acid, and phosphoric acid.
[0008] As a further improvement to the technical solution disclosed in this invention, in steps S5 and S7, the purity of the high-purity aluminum powder is controlled at 99.95% or higher, and the particle size is controlled at 50–100 nm. The operating parameters of the first, second, third, and fourth thermal spraying devices are all controlled as follows: output power 60–80 kW, rated current 185–250 A, and powder feeding speed 80–120 g / min.
[0009] As a further improvement to the technical solution disclosed in this invention, in step S6, the high-dielectric sol is formed by mixing a solute and a solvent, wherein the solute is BaTiO3 or Bi4Ti3O3. 12 Ba 0.5 Sr 0.5 TiO3, SrTiO3, CaCu3Ti4O 12 It can be any one or a mixture of several of the following, and the solvent is one or more of the following solvents: deionized water, ethanol, ethylene glycol, and acetone.
[0010] As a further improvement to the technical solution disclosed in this invention, step S6a is added between step S6 and step S7 to perform a temperature rise process on the first high dielectric constant layer and the second high dielectric constant layer.
[0011] As a further improvement to the technical solution disclosed in this invention, in step S6a, a scanning temperature rise operation is performed simultaneously on the first high dielectric constant layer and the second high dielectric constant layer by means of a first laser and a second laser, respectively. During the laser scanning process, the power P of the first laser and the second laser is controlled at 120-150W, the spot diameter d is controlled at 0.3-0.35 mm, the grating scanning is performed, and the scanning speed v < 850 mm / min.
[0012] In the technical solution disclosed in this invention, high-purity aluminum powder is heated to a molten state using thermal spraying equipment, and a high-speed atomization of the airflow is used to form a microparticle mist deposition layer (i.e., the first aluminum powder layer, the second aluminum powder layer, the third aluminum powder layer, and the fourth aluminum powder layer mentioned in the text) on the aluminum foil according to the process requirements. Before performing the first thermal spraying operation (to form the first and second aluminum powder layers), the front and back sides of the aluminum foil are pre-etched. Furthermore, during the first and second thermal spraying operations, a high-dielectric sol mist is atomized using an ultrasonic atomizing device to uniformly adhere to the first and second aluminum powder layers to grow and form a first high-dielectric-constant layer and a second high-dielectric-constant layer, respectively.
[0013] Compared with traditional preparation methods, the preparation method of high specific capacity low pressure anode foil disclosed in this invention has achieved at least several beneficial technical effects in practical applications, specifically: 1) In this application, a combination of thermal spraying and ultrasonic atomization spraying is used to obtain high specific capacity and low pressure anode foil. The preparation process is simple, more efficient, green and environmentally friendly, and conducive to large-scale industrial production. 2) The use of thermal spraying allows for the rapid acquisition of powder-laminated foils, effectively simplifying the fabrication process and shortening the total fabrication time. More importantly, the resulting first, second, third, and fourth aluminum powder laminates exhibit a denser internal microstructure and extremely high structural stability. This effectively ensures higher bonding strength between the first and second aluminum powder laminates and the front and back sides of the aluminum foil substrate, as well as between the third aluminum powder laminate and the first high-dielectric-constant layer, and between the fourth aluminum powder laminate and the second high-dielectric-constant layer. 3) Using ultrasonic atomization spraying to obtain the first high dielectric constant layer and the second high dielectric constant layer can effectively ensure the consistency of the thickness of the regional layer, the thickness is controllable, and the internal microstructure is more compact, which is conducive to increasing the content of high dielectric oxides doped in it. 4) Because the first high dielectric constant layer is sandwiched between the first and third aluminum powder layers, and the second high dielectric constant layer is sandwiched between the second and fourth aluminum powder layers, it is beneficial for the aluminum ions and high dielectric ions to migrate and interact fully in the subsequent anodizing process, so that the doped high dielectric material is more evenly distributed in the composite layer, which lays a good foundation for improving the capacity of the anode foil. 5) Compared with ordinary etched foil or powder laminated foil, its mechanical properties such as the ultimate bending number and tensile strength have been effectively improved. Detailed Implementation
[0014] The present invention will be further described in detail below with reference to embodiments. These embodiments are only used to explain the present invention and do not constitute a limitation on the scope of protection of the present invention. Unless otherwise specified, the methods described are conventional methods.
[0015] To more intuitively demonstrate the beneficial effects of the technical solution of this invention, a set of comparative experiments are also provided below, as mentioned in the background section of this paper.
[0016] A method for preparing a high-dielectric composite powder sintered foil includes the following steps: S1. Aluminum powder, epoxy resin, and sodium dodecylbenzenesulfonate are mixed in ethanol and stirred evenly to obtain a mixed slurry. The mass ratio of each component in the mixed slurry is as follows: aluminum powder: 60-85%, epoxy resin: 5-10%, sodium dodecylbenzenesulfonate: 1-5%, ethanol: 6-30%. The purity of aluminum powder is controlled at above 99.9%, and the particle size is controlled at 1-50 μm. S2. The mixed slurry obtained in step S1 is coated onto the surface of an aluminum foil with a thickness of 30 μm and a surface roughness value Ra controlled between 0.2 and 0.25 μm, and then dried and cured into a film to obtain a sintered foil substrate; and the drying temperature of the mixed slurry curing into a film is controlled at 150℃. S3. Forming of powder sintered foil, which includes the following sub-steps: S31. Place the sintered foil substrate obtained in step S2 in an argon atmosphere, control the temperature at 300℃, and maintain it for 2 hours. S32. The sintered foil substrate obtained in step S31 is placed in an argon atmosphere and heated to 500°C for 5 hours. S4. The powder sintered foil obtained in step S3 is immersed in a titanium-containing precursor solution, drained, and then heat-treated to form a titanium dioxide film on the surface of the powder sintered foil to obtain a composite sintered foil. After the titanium-containing precursor solution is drained, the heat treatment temperature required to prepare the composite sintered foil is controlled at 550℃ and the holding time is controlled at 30min. The preparation method of the titanium-containing precursor solution includes the following sub-steps: S41. Add tetrabutyl titanate solution dropwise to lactic acid solution and stir for 3-5 minutes to form a mixed solution. The volume ratio of tetrabutyl titanate solution to lactic acid solution is 1:6, and the concentration of tetrabutyl titanate solution is 0.05-0.1 mol / L. S42. Add deionized water to the mixed solution obtained in step S41 to dilute it, and stir well; S43. Continue to add a polyvinyl alcohol aqueous solution with a concentration of 0.2-0.5 g / L to the mixed solution and stir for 3-5 minutes until the mixture is uniform. S5. The composite sintered foil obtained in step S4 is processed using a traditional chemical formation process to obtain a high-dielectric composite powder sintered foil.
[0017] S5 includes the following sub-steps: S51. The composite sintered foil obtained in step S4 is placed in a solution containing 25 wt% ammonium diacid for formation, and a current density of 10 mA / cm² is added during formation. 2 The temperature inside the solution bath is controlled at 90℃ to obtain a primary electrolytic foil; S52. Form the primary foil in a solution containing 25 wt% ammonium disulfide, and add a current density of 30 mA / cm² during the formation process. 2 The temperature inside the solution bath is controlled at 90℃ to obtain a two-stage electrolytic foil; S53. The secondary forming foil is formed in a solution containing 5 wt% ammonium dicarboxylate, and a current density of 40 mA / cm² is added during the forming process. 2The temperature inside the solution bath is controlled at 90℃ to obtain a three-stage electrolytic foil; S54. Form the tertiary foil in a solution containing 25 wt% ammonium disulfide, and add a current density of 50 mA / cm² during the formation process. 2 The temperature inside the solution bath is controlled at 60℃, and multi-stage formation is repeated. The current density for stages four to six is 50 mA / cm². 2 Obtain a level 6 electrolytic foil; S55. The obtained six-level electrolytic foil is subjected to depolarization treatment. Example
[0018] The preparation method of high specific capacity low pressure anode foil includes the following steps: S1. Select aluminum foil; the aluminum foil should be 50μm thick and have a purity of 99.95% or higher. S2. Perform surface cleaning treatment on the aluminum foil obtained in step S1, which includes the following sub-steps; S21. Immerse the aluminum foil obtained in step S1 in a 0.5 mol / L NaOH solution to remove impurities and oil stains from its front and back surfaces. S22. Use clean water to clean the aluminum foil obtained in step S21 and then dry it. S3. Immerse the aluminum foil obtained in step S2 in hydrochloric acid solution to simultaneously etch its front and back surfaces, and control the etching depth on one side to 3-5 μm. S4. Use clean water to perform high-pressure rinsing on the aluminum foil obtained in step S3 and then dry it. In this way, during the rinsing process, the residual hydrochloric acid solution can be removed from the corrosion holes by the impact force of the water flow, which provides a good foundation for the subsequent growth of the first aluminum powder layer and the second aluminum powder layer, and helps to ensure that the first aluminum powder layer, the second aluminum powder layer and the aluminum foil have excellent bonding strength. S5. Simultaneously, using the first thermal spraying equipment and the second thermal spraying equipment, high-purity aluminum powder is sprayed onto the front and back sides of the aluminum foil obtained in step S4 to form the first aluminum powder layer and the second aluminum powder layer; the thickness of the first aluminum powder layer and the second aluminum powder layer are both controlled to be 5-8 μm. The purity of the high-purity aluminum powder is controlled at over 99.95%, and the particle size is controlled at 50-100nm. The operating parameters of the first and second thermal spraying equipment are both controlled at: output power 60KW, rated current 185A, and powder feeding speed 80g / min. S6. Using the first ultrasonic atomizing device and the second ultrasonic atomizing device, the high dielectric sol is attached to the front and back sides of the aluminum foil obtained in step S5, so as to continue to grow along the thickness direction of the first aluminum powder layer and the second aluminum powder layer respectively to form the first high dielectric constant layer and the second high dielectric constant layer; the thickness of the first high dielectric constant layer and the second high dielectric constant layer are both controlled at 2 to 3 μm; The high-dielectric sol is composed of a solute and a solvent, wherein the solute is preferably BaTiO3, and the solvent is preferably acetone, and the volume percentage concentration of BaTiO3 is controlled at 5%; S7. Simultaneously, using the third and fourth thermal spraying devices, high-purity aluminum powder is sprayed onto the front and back sides of the aluminum foil obtained in step S6, respectively, to continue growing along the thickness direction of the first high dielectric constant layer and the second high dielectric constant layer to form the third aluminum powder stack and the fourth aluminum powder stack; the thickness of the third aluminum powder stack and the fourth aluminum powder stack are both controlled at 5 to 8 μm. The purity of the high-purity aluminum powder is controlled at over 99.95%, and the particle size is controlled at 50-100nm. The operating parameters of the third and fourth thermal spraying equipment are controlled at: output power 70KW, rated current 200A, and powder feeding speed 95g / min. S8. Annealing is performed on the aluminum foil obtained in step S7 to eliminate its internal stress and improve the structural stability of the aluminum foil, which lays a good foundation for further improvement of its ultimate bending strength. S9. Immerse the aluminum foil obtained in step S8 in a 15% (w / w) ammonium adipate aqueous solution, and maintain the temperature at 95°C and a current density of 20 mA / cm². 2 Anodizing is performed under a voltage of 10V. S10. Perform water washing and drying treatment on the aluminum foil obtained in step S9 to obtain the high specific capacity low pressure anode foil product.
[0019] The preparation method of high specific capacity low pressure anode foil includes the following steps: S1. Select aluminum foil; the aluminum foil should be 50μm thick and have a purity of 99.95% or higher. S2. Perform surface cleaning treatment on the aluminum foil obtained in step S1, which includes the following sub-steps; S21. Immerse the aluminum foil obtained in step S1 in a 0.5 mol / L NaOH solution to remove impurities and oil stains from its front and back surfaces. S22. Use clean water to clean the aluminum foil obtained in step S21 and then dry it. S3. Immerse the aluminum foil obtained in step S2 in hydrochloric acid solution to simultaneously etch its front and back surfaces, and control the etching depth on one side to 3-5 μm. S4. Use clean water to perform high-pressure rinsing on the aluminum foil obtained in step S3 and then dry it. In this way, during the rinsing process, the residual hydrochloric acid solution can be removed from the corrosion holes by the impact force of the water flow, which provides a good foundation for the subsequent growth of the first aluminum powder layer and the second aluminum powder layer, and helps to ensure that the first aluminum powder layer, the second aluminum powder layer and the aluminum foil have excellent bonding strength. S5. Simultaneously, using the first thermal spraying equipment and the second thermal spraying equipment, high-purity aluminum powder is sprayed onto the front and back sides of the aluminum foil obtained in step S4 to form the first aluminum powder layer and the second aluminum powder layer; the thickness of the first aluminum powder layer and the second aluminum powder layer are both controlled to be 5-8 μm. The purity of the high-purity aluminum powder is controlled at over 99.95%, and the particle size is controlled at 50-100nm. The operating parameters of the first and second thermal spraying equipment are both controlled at: output power 70KW, rated current 210A, and powder feeding speed 100g / min. S6. Using the first ultrasonic atomizing device and the second ultrasonic atomizing device, the high dielectric sol is attached to the front and back sides of the aluminum foil obtained in step S5, so as to continue to grow along the thickness direction of the first aluminum powder layer and the second aluminum powder layer respectively to form the first high dielectric constant layer and the second high dielectric constant layer; the thickness of the first high dielectric constant layer and the second high dielectric constant layer are both controlled at 2 to 3 μm; The high-dielectric sol is composed of a solute and a solvent, wherein the solute is preferably BaTiO3, and the solvent is preferably acetone, and the volume percentage concentration of BaTiO3 is controlled at 8%; S7. Simultaneously, using the third and fourth thermal spraying devices, high-purity aluminum powder is sprayed onto the front and back sides of the aluminum foil obtained in step S6, respectively, to continue growing along the thickness direction of the first high dielectric constant layer and the second high dielectric constant layer to form the third aluminum powder stack and the fourth aluminum powder stack; the thickness of the third aluminum powder stack and the fourth aluminum powder stack are both controlled at 5 to 8 μm. The purity of the high-purity aluminum powder is controlled at over 99.95%, and the particle size is controlled at 50-100nm. The operating parameters of the third and fourth thermal spraying equipment are controlled at: output power 75KW, rated current 220A, and powder feeding speed 100g / min. S8. Annealing is performed on the aluminum foil obtained in step S7 to eliminate its internal stress and improve the structural stability of the aluminum foil, which lays a good foundation for further improvement of its ultimate bending strength. S9. Immerse the aluminum foil obtained in step S8 in a 15% (w / w) ammonium adipate aqueous solution, and maintain the temperature at 95°C and a current density of 20 mA / cm². 2 Anodizing is performed under a voltage of 10V. S10. Perform water washing and drying treatment on the aluminum foil obtained in step S9 to obtain the high specific capacity low pressure anode foil product.
[0020] The preparation method of high specific capacity low pressure anode foil includes the following steps: S1. Select aluminum foil; the aluminum foil should be 50μm thick and have a purity of 99.95% or higher. S2. Perform surface cleaning treatment on the aluminum foil obtained in step S1, which includes the following sub-steps; S21. Immerse the aluminum foil obtained in step S1 in a 0.5 mol / L NaOH solution to remove impurities and oil stains from its front and back surfaces. S22. Use clean water to clean the aluminum foil obtained in step S21 and then dry it. S3. Immerse the aluminum foil obtained in step S2 in hydrochloric acid solution to simultaneously etch its front and back surfaces, and control the etching depth on one side to 3-5 μm; S4. Use clean water to perform high-pressure rinsing on the aluminum foil obtained in step S3 and dry it. In this way, during the rinsing process, the residual hydrochloric acid solution can be removed from the etching holes by the impact force of the water flow, which provides a good foundation for the subsequent growth of the first aluminum powder layer and the second aluminum powder layer, and helps to ensure that the first aluminum powder layer, the second aluminum powder layer and the aluminum foil have excellent bonding strength; S5. Simultaneously, using the first thermal spraying equipment and the second thermal spraying equipment, high-purity aluminum powder is sprayed onto the front and back sides of the aluminum foil obtained in step S4 to form the first aluminum powder layer and the second aluminum powder layer; the thickness of the first aluminum powder layer and the second aluminum powder layer are both controlled to be 5-8 μm. The purity of the high-purity aluminum powder is controlled at over 99.95%, and the particle size is controlled at 50-100nm. The operating parameters of the first and second thermal spraying equipment are both controlled at: output power 80KW, rated current 250A, and powder feeding speed 120g / min. S6. Using the first ultrasonic atomizing device and the second ultrasonic atomizing device, the high dielectric sol is attached to the front and back sides of the aluminum foil obtained in step S5, so as to continue to grow along the thickness direction of the first aluminum powder layer and the second aluminum powder layer respectively to form the first high dielectric constant layer and the second high dielectric constant layer; the thickness of the first high dielectric constant layer and the second high dielectric constant layer are both controlled at 2 to 3 μm; The high-dielectric sol is composed of a solute and a solvent, wherein the solute is preferably TiO2, and the solvent is preferably acetone, and the volume percentage concentration of TiO2 is controlled at 1%; S7. Simultaneously, using the third and fourth thermal spraying devices, high-purity aluminum powder is sprayed onto the front and back sides of the aluminum foil obtained in step S6, respectively, to continue growing along the thickness direction of the first high dielectric constant layer and the second high dielectric constant layer to form the third aluminum powder stack and the fourth aluminum powder stack; the thickness of the third aluminum powder stack and the fourth aluminum powder stack are both controlled at 5 to 8 μm. The purity of the high-purity aluminum powder is controlled at over 99.95%, and the particle size is controlled at 50-100nm. The operating parameters of the third and fourth thermal spraying equipment are controlled at: output power 80KW, rated current 250A, and powder feeding speed 110g / min. S8. Annealing is performed on the aluminum foil obtained in step S7 to eliminate its internal stress and improve the structural stability of the aluminum foil, which lays a good foundation for further improvement of its ultimate bending strength. S9. Immerse the aluminum foil obtained in step S8 in a 15% (w / w) ammonium adipate aqueous solution, and maintain the temperature at 95°C and a current density of 20 mA / cm². 2 S10. Perform anodizing treatment under a voltage of 10V; S111. Perform water washing and drying treatment on the aluminum foil obtained in step S9 to obtain the high specific capacity low pressure anode foil product.
[0021] Example 4 The preparation method of high specific capacity low pressure anode foil includes the following steps: S1. Select aluminum foil; the aluminum foil should be 50μm thick and have a purity of 99.95% or higher. S2. Perform surface cleaning treatment on the aluminum foil, which includes the following sub-steps; S21. Immerse the aluminum foil obtained in step S1 in a 0.5 mol / L NaOH solution to remove impurities and oil stains from its front and back surfaces. S22. Use clean water to clean the aluminum foil obtained in step S21 and then dry it. S3. Immerse the aluminum foil obtained in step S2 in hydrochloric acid solution to simultaneously etch its front and back surfaces, and control the etching depth on one side to 3-5 μm. S4. Use clean water to perform high-pressure rinsing on the aluminum foil obtained in step S3 and then dry it. In this way, during the rinsing process, the residual hydrochloric acid solution can be removed from the corrosion holes by the impact force of the water flow, which provides a good foundation for the subsequent growth of the first aluminum powder layer and the second aluminum powder layer, and helps to ensure that the first aluminum powder layer, the second aluminum powder layer and the aluminum foil have excellent bonding strength. S5. Simultaneously, using the first thermal spraying equipment and the second thermal spraying equipment, high-purity aluminum powder is sprayed onto the front and back sides of the aluminum foil obtained in step S4 to form the first aluminum powder layer and the second aluminum powder layer; the thickness of the first aluminum powder layer and the second aluminum powder layer are both controlled to be 5-8 μm. The purity of the high-purity aluminum powder is controlled at over 99.95%, and the particle size is controlled at 50-100nm. The operating parameters of the first and second thermal spraying equipment are both controlled at: output power 80KW, rated current 250A, and powder feeding speed 120g / min. S6. In the initial stage of the formation of the first and second aluminum powder layers, they contain a relatively large amount of amorphous Al2O3, resulting in a relatively loose film structure. This will affect the electrical properties of the finished anode foil to some extent. Therefore, the aluminum foil obtained in step S5 is subjected to a first annealing treatment. The detailed conditions for the first annealing are as follows: the temperature is controlled at 550-570℃, and the duration is controlled at 3-5 minutes. In this way, after the first and second aluminum powder layers undergo annealing treatment, their film structure is transformed into a crystalline γ-ray film. , - Al2O3, which helps to improve the dielectric properties of the finished anode foil; S7. Using the first ultrasonic atomizing device and the second ultrasonic atomizing device, the high dielectric sol is attached to the front and back sides of the aluminum foil obtained in step S6, so as to continue to grow along the thickness direction of the first aluminum powder layer and the second aluminum powder layer respectively to form the first high dielectric constant layer and the second high dielectric constant layer; the thickness of the first high dielectric constant layer and the second high dielectric constant layer are both controlled at 2 to 3 μm; The high-dielectric sol is composed of a solute and a solvent, wherein the solute is preferably TiO2, and the solvent is preferably acetone, and the volume percentage concentration of TiO2 is controlled at 5%; S7a. Perform a temperature rise process on the first high dielectric constant layer and the second high dielectric constant layer; The first laser and the second laser are used to simultaneously perform scanning temperature rise operations on the first high dielectric constant layer and the second high dielectric constant layer, respectively. During the laser scanning process, the power P of the first laser and the second laser are both controlled at 120W, the spot diameter d is controlled at 0.3 mm, the grating scanning is used, and the scanning speed v = 820 mm / min. S8. Simultaneously, using the third and fourth thermal spraying devices, high-purity aluminum powder is sprayed onto the front and back sides of the aluminum foil obtained in step S7a, respectively, to continue growing along the thickness direction of the first high dielectric constant layer and the second high dielectric constant layer to form the third aluminum powder stack and the fourth aluminum powder stack; the thickness of the third aluminum powder stack and the fourth aluminum powder stack are both controlled at 5 to 8 μm. The purity of the high-purity aluminum powder is controlled at over 99.95%, and the particle size is controlled at 50-100nm. The operating parameters of the third and fourth thermal spraying equipment are controlled at: output power 80KW, rated current 250A, and powder feeding speed 110g / min. S9. Perform a second annealing treatment on the aluminum foil obtained in step S8; the detailed conditions for the second annealing are as follows: the temperature is controlled at 580-600℃, and the duration is controlled at 6-7 minutes; thus, after the third and fourth aluminum powder layers undergo annealing treatment, similar to the modification mechanism of the first and second aluminum powder layers mentioned above, their film structure is also transformed into crystalline γ-type. ,-Al2O3, which helps to improve the dielectric properties of the finished anode foil; S10. Immerse the aluminum foil obtained in step S9 in a 15% (w / w) ammonium adipate aqueous solution, and maintain the temperature at 95°C and a current density of 20 mA / cm². 2 Anodizing is performed under a voltage of 10V. S11. The aluminum foil obtained in step S10 is washed and dried to obtain the high specific capacity low pressure anode foil product.
[0022] It is important to emphasize that during the laser scanning process, the temperatures of the first and second high-dielectric-constant layers should be controlled between 60 and 85°C. This effectively shortens the curing time of the first and second high-dielectric-constant layers. Furthermore, acetone, the solvent for the high-dielectric sol, has a boiling point of 56.5°C. Therefore, acetone remains in a boiling state throughout the curing process, resulting in a large number of uniformly distributed pores within the first and second high-dielectric-constant layers. This not only improves the bonding stability with the subsequent third and fourth aluminum powder layers but also facilitates the relative migration and interaction between aluminum ions and high-dielectric ions during the subsequent anodizing process.
[0023] The method for preparing high specific capacitance and low pressure anode foil disclosed in this invention has achieved at least several beneficial technical effects in practical applications, specifically: 1) In this application, a combination of thermal spraying and ultrasonic atomization spraying is used to obtain high specific capacity and low pressure anode foil. The preparation process is simple, more efficient, green and environmentally friendly, and conducive to large-scale industrial production. 2) The use of thermal spraying allows for the rapid acquisition of powder-laminated foils, effectively simplifying the fabrication process and shortening the total fabrication time. More importantly, the resulting first, second, third, and fourth aluminum powder laminates exhibit a denser internal microstructure and extremely high structural stability. This effectively ensures higher bonding strength between the first and second aluminum powder laminates and the front and back sides of the aluminum foil substrate, as well as between the third aluminum powder laminate and the first high-dielectric-constant layer, and between the fourth aluminum powder laminate and the second high-dielectric-constant layer. 3) Using ultrasonic atomization spraying to obtain the first high dielectric constant layer and the second high dielectric constant layer can effectively ensure the consistency of the thickness of the regional layer, the thickness is controllable, and the internal microstructure is more compact, which is conducive to increasing the content of high dielectric oxides doped in it. 4) Because the first high dielectric constant layer is sandwiched between the first and third aluminum powder layers, and the second high dielectric constant layer is sandwiched between the second and fourth aluminum powder layers, it is beneficial for the aluminum ions and high dielectric ions to migrate and interact fully in the subsequent anodizing process, so that the doped high dielectric material is more evenly distributed in the composite layer, which lays a good foundation for improving the capacity of the anode foil. 5) Compared with ordinary etched foil or powder laminated foil, its mechanical properties such as the ultimate bending number and tensile strength have been effectively improved.
[0024] Summary of experimental data
[0025] Summary of Ti content test results in the anode foils prepared by the above five examples (1 conventional comparative example + 4 examples of this application)
[0026] Summary of various performance test results of the anode foils prepared in the above five examples (1 conventional comparative example + 4 examples of this application) The above description of the disclosed embodiments enables those skilled in the art to make or use the invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the invention is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for preparing a high specific capacity, low pressure anode foil, characterized in that, Includes the following steps: S1. Select aluminum foil; the thickness of the aluminum foil should be controlled between 50 and 60 μm, and the purity should be above 99.95%; S2. Perform surface cleaning treatment on the aluminum foil obtained in step S1; S3. Immerse the aluminum foil obtained in step S2 into an acid solution to simultaneously etch its front and back surfaces, and control the etching depth on one side to 3-5 μm. S4. Use clean water to perform high-pressure rinsing on the aluminum foil obtained in step S3, and then dry it. S5. Simultaneously, using the first thermal spraying equipment and the second thermal spraying equipment, high-purity aluminum powder is sprayed onto the front and back sides of the aluminum foil obtained in step S4 to form a first aluminum powder layer and a second aluminum powder layer; the thickness of the first aluminum powder layer and the second aluminum powder layer are both controlled to be 5-8 μm. S6. Using a first ultrasonic atomizing device and a second ultrasonic atomizing device, a high-dielectric sol is attached to the front and back sides of the aluminum foil obtained in step S5, so as to continue growing along the thickness direction of the first aluminum powder layer and the second aluminum powder layer respectively to form a first high-dielectric constant layer and a second high-dielectric constant layer; the thickness of the first high-dielectric constant layer and the second high-dielectric constant layer are both controlled at 2 to 3 μm; S7. Simultaneously, using a third thermal spraying device and a fourth thermal spraying device, high-purity aluminum powder is sprayed onto the front and back sides of the aluminum foil obtained in step S6, respectively, to continue growing along the thickness direction of the first high dielectric constant layer and the second high dielectric constant layer to form a third aluminum powder layer and a fourth aluminum powder layer; the thickness of the third aluminum powder layer and the fourth aluminum powder layer are both controlled to be 5-8 μm; S8. Perform annealing treatment on the aluminum foil obtained in step S7; S9. Immerse the aluminum foil obtained in step S8 in an aqueous solution of 10-20% (by mass) ammonium adipate, and maintain the temperature at 65-95°C and a current density of 20 mA / cm². 2 Anodizing is performed under a voltage of 8-36V. S10. Perform water washing and drying treatment on the aluminum foil obtained in step S9 to obtain the high specific capacity low pressure anode foil product.
2. The method for preparing high specific capacity low pressure anode foil according to claim 1, characterized in that, Step S2 includes the following sub-steps: S21. Immerse the aluminum foil obtained in step S1 in a 0.5-1.0 mol / L NaOH solution to remove impurities and oil stains from its front and back surfaces. S22. Use clean water to clean the aluminum foil obtained in step S21 and then dry it.
3. The method for preparing high specific capacitance low pressure anode foil according to claim 1, characterized in that, In step S3, the acid solution is any one or a mixture of several of hydrochloric acid, sulfuric acid, nitric acid, and phosphoric acid.
4. The method for preparing high specific capacity low pressure anode foil according to claim 1, characterized in that, In steps S5 and S7, the purity of the high-purity aluminum powder is controlled at 99.95% or higher, and the particle size is controlled at 50-100nm; the operating parameters of the first thermal spraying equipment, the second thermal spraying equipment, the third thermal spraying equipment, and the fourth thermal spraying equipment are all controlled at: output power 60-80KW, rated current 185-250A, and powder feeding speed 80-120g / min.
5. The method for preparing high specific capacitance low pressure anode foil according to claim 1, characterized in that, In step S6, the high-dielectric sol is formed by mixing a solute and a solvent, wherein the solute is BaTiO3 or Bi4Ti3O3. 12 Ba 0.5 Sr 0.5 TiO3, SrTiO3, CaCu3Ti4O 12 The solvent is any one or a mixture of several of the solvents, wherein the solvent is one or more of deionized water, ethanol, ethylene glycol, and acetone.
6. The method for preparing high specific capacitance low pressure anode foil according to claim 1, characterized in that, Step S6a is added between steps S6 and S7 to perform a temperature rise process on the first high dielectric constant layer and the second high dielectric constant layer.
7. The method for preparing high specific capacity low pressure anode foil according to claim 6, characterized in that, In step S6a, a scanning temperature rise operation is performed simultaneously on the first high dielectric constant layer and the second high dielectric constant layer by means of a first laser and a second laser, respectively. During the laser scanning process, the power P of the first laser and the second laser is controlled at 120-150W, the spot diameter d is controlled at 0.3-0.35 mm, the grating scanning is performed, and the scanning speed v < 850 mm / min.
Citation Information
Patent Citations
Method for production of solid electrolyte and solid electrolytic capacitor
CN101379571A
Pretreatment process for preparing formed foil containing TiO2 medium layer
CN109183116A