A zinc-manganese battery with no positive electrode and a weak acid water system and a preparation method thereof

By employing a cathode-free design and the application of a decoupled gel electrolyte, the challenges of high energy density and cycle stability in zinc-manganese batteries have been addressed, simplifying the fabrication process, improving battery performance, and making the batteries suitable for flexible electronic energy storage applications.

CN116742158BActive Publication Date: 2026-11-24ZHEJIANG SCI-TECH UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310880656.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-18
Publication Date
2026-11-24
Estimated Expiration
2043-07-18

AI Technical Summary

Technical Problem

Existing zinc-manganese batteries face challenges in terms of high energy density and cycle stability, especially due to severe corrosion and oxygen evolution reaction of the zinc anode in high-potential acidic electrolytes, and the active material paste coating process is cumbersome and prone to errors.

Method used

A cathode-free design is adopted, and manganese oxide is deposited on a conductive current collector using a decoupled gel electrolyte. The polyacrylamide gel electrolyte is prepared by UV light initiation, and a cathode-free zinc-manganese battery is prepared by constant voltage charging method, thus avoiding the active material paste coating step.

Benefits of technology

It simplifies the manufacturing process, reduces errors, improves the energy density and cycle stability of the battery, and lowers the manufacturing cost, making it suitable for the field of flexible electronic energy storage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116742158B_ABST
    Figure CN116742158B_ABST
Patent Text Reader

Abstract

This invention relates to a cathode-free, weakly acidic aqueous zinc-manganese battery and its preparation method. The preparation method of the cathode-free, weakly acidic aqueous zinc-manganese battery includes the following steps: S1, preparing a weakly acidic solution; S2, preparing an electrolyte; S3, preparing a decoupling gel electrolyte; S4, preparing a cathode-free coin cell; S5, loading active materials. The manganese ions in the battery electrolyte are oxidized to manganese oxide using an electrochemical workstation or a Blue Electric electrochemical workstation to obtain the cathode-free, weakly acidic aqueous zinc-manganese battery. Because this battery has no cathode, it eliminates the need for preparing active material paste and corresponding coating steps, thereby reducing the number of preparation steps and processing time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to an energy storage device, and more particularly to a cathode-free, weakly acidic aqueous zinc-manganese battery and its preparation method, belonging to the field of energy storage device technology. Background Technology

[0002] Zinc metal is considered an ideal anode material for aqueous rechargeable batteries due to its abundant resources, low anodic potential, and high theoretical capacity, and holds promise for applications in flexible electronic energy storage. Among aqueous zinc-ion batteries, zinc-vanadium batteries exhibit the best cycle stability, but their energy density is insufficient. Zinc-sulfur batteries possess the highest energy density due to the ultra-high specific capacity of the sulfur electrode. However, their side reactions limit cycle stability. Compared to other metal anodes and oxide cathodes, rechargeable aqueous zinc-manganese batteries offer advantages such as high theoretical capacity, non-toxicity, and low cost of zinc and manganese oxides.

[0003] The two-electron reaction of MnO2 with H + and Zn 2+ The combination of insertion / extraction single-electron reactions is a novel approach that not only suppresses Mn dissolution but also increases cathode capacity and discharge plateau. However, reversible deposition and dissolution of MnO2 typically occur in high-potential acidic electrolytes, posing a significant challenge to the corrosion resistance and oxygen evolution suppression of the zinc anode. Therefore, when designed for decoupling configurations, MnO2 / Mn... 2+ Zinc-manganese batteries with reactive electrolytes hold promise for improving energy density and cycle stability. However, decoupled electrolytes require expensive ion-selective membranes to prevent mixing of the two electrolytes during cycling, hindering their use in mainstream applications. Decoupling the gel electrolyte not only protects the zinc anode from corrosion but also, due to the gel's numerous hydrophilic functional groups that form hydrogen bonds with water, significantly reduces free water content, effectively inhibiting oxygen evolution reaction, reducing active material dissolution, and improving capacity retention. Furthermore, it can extend the voltage window to above 2V. Compared to strong acid conditions, weak acid conditions better meet green and safe standards. The basic zinc sulfate generated during discharge under weak acid conditions is crucial for discharge capacity, playing an auxiliary role in the discharge process.

[0004] Loading active materials is often the most time-consuming and costly step in battery fabrication. Furthermore, the organic solvents in the active material paste can further pollute the environment. However, choosing to fabricate a cathodeless battery simply requires using a conductive current collector as the positive electrode active material loading point during battery fabrication. After device fabrication, manganese ions from the gel electrolyte are oxidized and loaded onto the conductive current collector using constant voltage charging or chronoamperometry to serve as the battery's positive electrode. This method allows for high-energy-efficiency deposition of active materials and discharge at a high operating platform. This safe, economical, long-cycle, and high-energy aqueous zinc-manganese battery may be a promising candidate in the field of flexible batteries. Summary of the Invention

[0005] The purpose of this invention is to provide a cathode-free, weakly acidic aqueous zinc-manganese battery. Since this battery has no cathode, it does not require the preparation of active material paste and the corresponding coating steps, thereby reducing the number of preparation steps and the processing time. At the same time, it can reduce the errors caused by the coating process of active material paste (most active material paste coating is done manually, which has a large error).

[0006] The present invention also provides a method for preparing the aqueous zinc-manganese battery, which has the advantages of being simple, convenient, low-cost, and environmentally friendly, and provides new ideas for the subsequent preparation of novel structured batteries.

[0007] The technical solution adopted by this invention to solve its technical problem is:

[0008] A method for preparing a weakly acidic aqueous zinc-manganese battery without a positive electrode, the method comprising the following steps:

[0009] S1. Preparation of a weakly acidic solution:

[0010] Dissolve an appropriate amount of acid in water and stir for 1-5 hours to prepare a weakly acidic solution with a pH of 2-3.

[0011] The acid is selected from one or more of citric acid, concentrated sulfuric acid, carbonic acid, hydrochloric acid, malic acid, oxalic acid, or nitric acid;

[0012] S2. Preparation of electrolyte:

[0013] Acrylamide, zinc sulfate heptahydrate, and manganese sulfate are added to the weakly acidic solution prepared by S1 and mixed well. Then, NN methylenebisacrylamide and photoinitiator are added sequentially and mixed well to obtain a weakly acidic electrolyte. The weakly acidic electrolyte contains the following components by mass percentage: acrylamide 15-30%, zinc sulfate heptahydrate 25-30%, manganese sulfate 5-10%, NN methylenebisacrylamide 0.05-0.5%, photoinitiator 0.05-0.5%, and the balance is a weakly acidic solution with a pH of 3-5.

[0014] Acrylamide and zinc sulfate heptahydrate were added to water sequentially and mixed thoroughly. Then, NN methylenebisacrylamide and a photoinitiator were added sequentially and mixed thoroughly to obtain a neutral electrolyte. The neutral electrolyte contained the following components by mass percentage: 15-30% acrylamide, 25-30% zinc sulfate heptahydrate, 0.05-0.5% NN methylenebisacrylamide, 0.05-0.5% photoinitiator, and the balance being water.

[0015] S3. Preparation of decoupling gel electrolyte:

[0016] A weakly acidic electrolyte was injected into a polytetrafluoroethylene template, and a photoinitiated reaction was carried out by irradiation with a UV lamp. The resulting weakly acidic gel electrolyte was obtained after the reaction.

[0017] Neutral electrolyte is stacked on the surface of a weakly acidic gel electrolyte, and a photo-initiated reaction is carried out by irradiation with a UV lamp. After the reaction, a decoupled gel electrolyte is obtained.

[0018] S4, Preparation of cathodeless coin cell batteries

[0019] Using the decoupled gel electrolyte prepared by S3 as the electrolyte of the battery, a zinc-manganese button cell without a positive electrode was prepared by encapsulation. In the decoupled gel electrolyte, the weakly acidic gel electrolyte side is attached to the positive current collector of the battery, and the neutral gel electrolyte side is attached to the negative electrode of the battery.

[0020] S5, Active Material Loading

[0021] A weakly acidic aqueous zinc-manganese battery without a positive electrode is prepared by oxidizing manganese ions in the electrolyte of the battery to manganese oxide using an electrochemical workstation or a Blue Electric electrochemical workstation.

[0022] Preferably, the photoinitiator in S2 is selected from one or more of 2-hydroxy-2-methylphenylacetone, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, 2-methyl-2-(4-morpholino)-1-[4-(methylthio)phenyl]-1-propanone, and 1-hydroxycyclohexylphenyl ketone.

[0023] Preferably, the thickness of the weakly acidic gel electrolyte in S3 is 0.25-2 mm, the UV lamp initiation time is 2-30 min, the thickness of the neutral gel electrolyte is 0.25-2 mm, the UV lamp initiation time is 2-30 min, and the thickness of the decoupling gel electrolyte is 0.5-4 mm.

[0024] Preferably, the UV lamp wavelength is 250-400nm.

[0025] Preferably, the positive current collector in S4 is one of conductive carbon paper, carbon cloth, or graphite paper.

[0026] Preferably, the pressure used during encapsulation in S4 is 25-100 kg / cm².-2 .

[0027] Preferably, the constant voltage charging voltage of the S5 is 1.6-2.4V, and the constant voltage charging time is 1-120min.

[0028] As a preferred method, the preparation method of the S4 electrodeless coin cell is as follows:

[0029] Using zinc sheet as the negative electrode and hydrophilic carbon material as the positive electrode current collector, the negative electrode battery shell, spring sheet, gasket, zinc sheet, decoupling gel electrolyte, positive electrode current collector and positive electrode battery shell are stacked in sequence and then packaged using a hydraulic press.

[0030] As a preferred option, the conditions for loading the active substance in S5 are as follows:

[0031] Perform timing current method or constant voltage charging at 2.1-2.3V.

[0032] A weakly acidic aqueous zinc-manganese battery without a positive electrode, prepared by the method described in this invention.

[0033] This invention uses acrylamide as the polymer matrix, adding an electrolyte, crosslinking agent, photoinitiator, and weak acid solvent to prepare an electrolyte. A decoupled polyacrylamide gel electrolyte is obtained through UV photoinitiation. A weakly acidic zinc-manganese battery without a positive electrode is prepared using a zinc sheet as the negative electrode, a conductive carbon filament as the positive electrode current collector, and the decoupled gel electrolyte as the separator. The manganese ions in the electrolyte are oxidized and deposited onto the surface of the positive electrode current collector using constant voltage charging or chronoamperometry to form the final device. The battery prepared by this invention belongs to the field of semi-solid-state batteries, making it promising for application in wearable energy storage.

[0034] Photoinitiation offers advantages such as fast reaction time and low energy consumption. The resulting decoupled gel electrolyte not only allows the negative electrode to be in a neutral environment to suppress zinc dendrite formation, but also improves the operating voltage and capacity by placing the positive electrode in a weakly acidic environment. Furthermore, the gel electrolyte can form hydrogen bonds with free water to inhibit the oxygen evolution and hydrogen absorption reaction, thus improving the battery's cycle life. The absence of a positive electrode also reduces the steps involved in preparing the active material paste, significantly improving battery manufacturing efficiency. This invention achieves mechanical flexibility and excellent electrochemical performance in zinc-manganese batteries, providing a new approach for aqueous batteries.

[0035] Compared with the prior art, the method of the present invention has the following characteristics:

[0036] 1. This invention uses acrylamide to prepare polyacrylamide gel electrolyte via photoinitiation, which has advantages such as speed, low energy consumption, and ease of large-scale production compared to thermally initiated acrylamide method;

[0037] 2. The polyacrylamide gel electrolyte prepared by this invention can not only provide an electrolyte transport channel for the battery, but also act as a membrane for traditional glass fiber to prevent short circuits caused by contact between the positive and negative electrodes.

[0038] 3. This invention uses a decoupled gel electrolyte instead of an expensive ion-selective membrane to separate the electrolyte into two parts. On the positive electrode side, the gel electrolyte contains manganese ions, which can meet the requirements for the generation of manganese oxide. It also has weak acidity, which provides conditions for the generation of basic zinc sulfate during discharge and inhibits the occurrence of oxygen evolution reaction. On the negative electrode side, the conditions are neutral, and the gel electrolyte can reduce the free water content, which can effectively inhibit the hydrogen absorption reaction and the occurrence of zinc dendrite phenomenon.

[0039] 4. This invention uses current collectors without active materials to directly assemble batteries, which can reduce the time required to prepare active material paste, greatly accelerate the preparation speed, and lay the foundation for subsequent large-scale preparation.

[0040] 5. This invention uses constant voltage charging for depositing manganese oxide and charging, which can achieve fast charging and excellent cycle life compared to constant current charging. Attached Figure Description

[0041] Figure 1 To supplement the stress-strain curves in Example 1, where (1), (2), (3), and (4) represent citric acid gel electrolyte, sulfuric acid gel electrolyte, neutral gel electrolyte, and polyacrylamide gel, respectively.

[0042] Figure 2 To supplement the schematic diagram of the citric acid weakly acidic gel electrolyte molecule in Example 1;

[0043] Figure 3 To supplement the infrared spectrum curves in Example 1, where (1) and (2) are the infrared spectra of polyacrylamide gel and citric acid gel electrolyte, respectively;

[0044] Figure 4 To supplement the SEM image of the citric acid gel electrolyte after freeze-drying in Example 1;

[0045] Figure 5 To supplement the Nyquist curve of the stainless steel symmetrical cell in Example 2, Figure (a) is the overall view and Figure (b) is the detail view;

[0046] Figure 6 To supplement the SEM images of the conductive carbon paper in Example 3, Figure (a) shows the initial structure of the conductive carbon paper, and Figure (b) shows the conductive carbon paper after constant voltage charging;

[0047] Figure 7 To supplement Example 3, which describes the oxidation of manganese oxides on conductive carbon paper by constant voltage charging;

[0048] Figure 8 To supplement the XPS diagrams of manganese oxides oxidized on conductive carbon paper by constant voltage charging in Example 3, where Figure (a) is the O1s spectrum and Figure (b) is the Mn2p spectrum;

[0049] Figure 9 To supplement the discharge curve of the battery in Example 4;

[0050] Figure 10 To supplement the SEM images of conductive carbon paper after constant current discharge in Example 4, Figure (a) shows the conductive carbon paper discharged to 1.8V, Figure (b) shows the conductive carbon paper discharged to 1.4V, Figure (c) shows the conductive carbon paper discharged to 1.2V, and Figure (d) shows the conductive carbon paper discharged to 0.8V.

[0051] Figure 11 To supplement the mapping diagram of conductive carbon paper when discharged to 0.8V in Example 4, where (a) is the original diagram, (b) Mn element, (c) Zn element, and (d) O element;

[0052] Figure 12 To supplement the XPS O1s spectra of the conductive carbon paper after discharge in Example 4, Figure (a) shows the conductive carbon paper discharged to 1.8V, Figure (b) shows the conductive carbon paper discharged to 1.4V, and Figure (c) shows the conductive carbon paper discharged to 0.8V.

[0053] Figure 13 To supplement the XPS Mn2p spectra of the conductive carbon paper after discharge in Example 4, Figure (a) shows the conductive carbon paper discharged to 1.8V, Figure (b) shows the conductive carbon paper discharged to 1.4V, and Figure (c) shows the conductive carbon paper discharged to 0.8V.

[0054] Figure 14 To supplement the discharge curves of batteries with different gel electrolytes in Example 5, where (1), (2), and (3) are decoupled citric acid gel electrolyte, undecoupled citric acid gel electrolyte, and decoupled zinc sulfate-free gel electrolyte, respectively;

[0055] Figure 15 To supplement Example 5, batteries with different gel electrolytes were used, starting from 0.05 mA / cm. -2 -1mAcm -2 Rate performance at current density, where (1), (2), (3), and (4) are the undecoupled citric acid gel electrolyte, the undecoupled zinc sulfate gel electrolyte, the undecoupled zinc sulfate-free gel electrolyte, and the citric acid gel electrolyte prepared in Example 5, respectively.

[0056] Figure 16 To supplement Example 5, the battery was charged at a constant voltage of 2.2V for 5 minutes, with a current of 0.5mA / cm. -2Long-cycle curves at current densities;

[0057] Figure 17 To supplement Example 5, the battery was charged at a constant voltage of 2.2V for 5 minutes, with a current of 0.5mA / cm. -2 The charge-discharge curves at the current density are shown in Figure (a), which is the full figure, and Figure (b) is the charge-discharge curve for the first ten cycles and the last ten cycles. Detailed Implementation

[0058] It should be noted that the following detailed descriptions are illustrative and intended to provide further explanation of this application. Unless otherwise specified, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application pertains.

[0059] It should be noted that the terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the exemplary embodiments according to this application. As used herein, the singular form is intended to include the plural form as well, unless the context clearly indicates otherwise. Furthermore, it should be understood that when the terms "comprising" and / or "including" are used in this specification, they indicate the presence of features, steps, operations, devices, components, and / or combinations thereof.

[0060] The present invention will now be further illustrated with specific examples. The following embodiments are only for explaining the present invention and do not constitute a limitation thereof. The test samples and test procedures used in the following embodiments include the following (if the specific experimental conditions are not specified in the embodiments, they are usually performed according to conventional conditions or the conditions recommended by the reagent company; the reagents, consumables, etc. used in the following embodiments can be obtained commercially unless otherwise specified).

[0061] UV lamp, Qiwei UV analyzer (WFH-204B), wavelength 254nm / 365nm, 365nm.

[0062] Example 1

[0063] A method for preparing a decoupled electrolyte, the specific steps of which are as follows:

[0064] 1. Preparation of weakly acidic citric acid solution

[0065] Weigh 1.3g of citric acid and dissolve it in 500g of deionized water. Stir magnetically for 3 hours at room temperature to prepare a weak acid solution of citric acid.

[0066] 2. Preparation of electrolyte

[0067] Add 3g acrylamide, 5.6g zinc sulfate heptahydrate, and 1.7g manganese sulfate sequentially to 10g of the prepared citric acid weak acid solution, place on a magnetic stirrer and stir at room temperature for 5min. Then add 20μg N-N-methylenebisacrylamide and 20μL 2-hydroxy-2-methylphenylacetone sequentially, place on a stirrer and stir for 5min to obtain a weak acid electrolyte.

[0068] Add 3g of acrylamide and 5.6g of zinc sulfate heptahydrate to 10g of deionized water, place on a stirrer and stir at room temperature for 5min. Then add 20μg of NNmethylenebisacrylamide and 20μL of 2-hydroxy-2-methylphenylacetone, place on a stirrer and stir for 5min to obtain a neutral electrolyte.

[0069] 3. Preparation of decoupling gel electrolytes

[0070] 150 μL of weakly acidic electrolyte was transferred onto a 16 mm diameter polytetrafluoroethylene plate using a pipette. The plate was then photoinitiated for 5 min using a UV lamp with a wavelength of 254 nm to obtain a weakly acidic gel electrolyte. Subsequently, 150 μL of neutral electrolyte was added to the surface of the plate, and the plate was photoinitiated for 3 min using a UV lamp with a wavelength of 365 nm to obtain a decoupled gel electrolyte.

[0071] Example 2

[0072] A method for preparing a gel electrolyte, the specific steps of which are as follows:

[0073] 1. Preparation of weakly acidic solutions

[0074] Weigh 1.3g of citric acid and dissolve it in 500g of deionized water. Stir magnetically for 3 hours at room temperature to prepare a citric acid weak acid solution.

[0075] Weigh 20 μL of 98 wt% concentrated sulfuric acid and dissolve it in 500 g of deionized water. Stir magnetically for 5 h at room temperature to prepare a weak acid solution of sulfuric acid.

[0076] 2. Electrolyte preparation

[0077] Add 3g acrylamide, 5.6g zinc sulfate heptahydrate, and 1.7g manganese sulfate sequentially to 10g of the prepared citric acid weak acid solution, place on a magnetic stirrer and stir at room temperature for 5min. Then add 20μg N-N-methylenebisacrylamide and 20μL 2-hydroxy-2-methylphenylacetone sequentially, place on a stirrer and stir for 5min to obtain a citric acid weak acid electrolyte.

[0078] Add 3g acrylamide, 5.6g zinc sulfate heptahydrate, and 1.7g manganese sulfate to 10g of prepared sulfuric acid solution in sequence, place on a magnetic stirrer and stir at room temperature for 5min. Then add 20μg N-N-methylenebisacrylamide and 20μL 2-hydroxy-2-methylphenylacetone in sequence, place on a stirrer and stir for 5min to obtain a weakly acidic sulfuric acid electrolyte.

[0079] Add 3g acrylamide and 5.6g zinc sulfate heptahydrate to 10g deionized water, place on a stirrer and stir at room temperature for 5min. Then add 20μg NN methylenebisacrylamide and 20μL 2-hydroxy-2-methylphenylacetone, place on a stirrer and stir for 5min to obtain a neutral electrolyte.

[0080] Add 3g of acrylamide to 10g of deionized water, place on a stirrer and stir at room temperature for 5min. Then add 20μg of NNmethylenebisacrylamide and 20μL of 2-hydroxy-2-methylphenylacetone in sequence, place on a stirrer and stir for 5min to obtain acrylamide electrolyte.

[0081] 3. Preparation of gel electrolytes

[0082] 5000 μL of weakly acidic citric acid electrolyte was transferred onto a 4*5 cm polytetrafluoroethylene plate using a pipette, and photoinitiated by a UV lamp with a wavelength of 254 nm for 10 min to obtain citric acid gel electrolyte.

[0083] Sulfuric acid gel electrolyte, neutral gel electrolyte, and polyacrylamide gel were prepared using the same method with weakly acidic sulfuric acid electrolyte, neutral electrolyte, and acrylamide electrolyte, respectively.

[0084] Supplementary Example 1: Characterization of the structure and mechanical properties of gel electrolytes

[0085] 1. Mechanical property testing: The four types of gels prepared in Example 2 (citric acid gel electrolyte, sulfuric acid gel electrolyte, neutral gel electrolyte, and polyacrylamide gel) were cut into strips of 1*4cm and subjected to tensile strength testing using a universal testing machine. The test was conducted according to GB / T1040.1-2006 "Determination of Tensile Properties of Plastics" at a tensile speed of 10mm / s. The stress-strain diagram is attached. Figure 1 As shown,

[0086] according to Figure 1It can be seen that the tensile breaking stress of polyacrylamide gel is 0.385 MPa, that of sulfate gel electrolyte is 0.976 MPa, that of neutral gel electrolyte is 1.012 MPa, and that of citric acid gel electrolyte is 1.118 MPa. Compared with the other three gels, polyacrylamide gel electrolyte shows a significant difference in both breaking stress and tensile strength. This is because the presence of zinc or manganese ions in the electrolyte entangles with the polyacrylamide chains, providing more cross-linking sites and increasing the gel strength. Citric acid gel electrolyte, on the other hand, exhibits a higher breaking stress compared to neutral and sulfate gel electrolytes. This is because citric acid undergoes monohydrate condensation with the amide bonds in the initiated polyacrylamide, as shown in the attached figure. Figure 2 As shown, this provides more crosslinking sites, thus increasing mechanical strength;

[0087] 2. Infrared Spectroscopy Analysis: The polyacrylamide gel and citric acid gel electrolyte prepared in Example 2 were subjected to infrared spectroscopy analysis, and the results are shown in the appendix. Figure 3 As shown, by Figure 3 It can be known that 3339cm -1 The NH stretching peak is at 3192 cm⁻¹. -1 The NH stretching peak is 1656 cm⁻¹. -1 The characteristic peak of carbonyl group is 1603 cm⁻¹. -1 Amide II (NH bending vibration) 1458 cm -1 Methylene deformation 1121cm -1 The CN vibration peak is at 1057 cm⁻¹. -1 The peak for the CN vibration of tertiary amines is observed at 3339 cm⁻¹, compared to the infrared spectrum of pure PAM. This is more pronounced in the gel electrolyte with added citric acid. -1 The peak is not obvious because the amide bond in polyacrylamide undergoes monohydrate condensation with the carboxyl group in citric acid, resulting in a decrease in the content of primary amines. Meanwhile, the peak at 1057 cm⁻¹ is not obvious. -1 The obvious peak intensity is due to the fact that both hydrogens on the amide bond reacted with citric acid to form a tertiary amine, resulting in a blue shift of the CN bond.

[0088] 3. Morphology Analysis: To prevent the structure of the gel electrolyte from collapsing after dehydration, we freeze-dried the citric acid gel electrolyte prepared in Example 2. The SEM image of the freeze-dried citric acid gel electrolyte is attached. Figure 4 As shown, the freeze-dried gel electrolyte has a porous structure, which provides channels for the migration of electrolytes in the gel and promotes ion migration.

[0089] Example 3

[0090] A method for preparing a stainless steel symmetric battery, the specific steps of which are as follows:

[0091] 1. Preparation of weakly acidic citric acid solution, same as in Example 1;

[0092] 2. Preparation of electrolyte: The weakly acidic electrolyte and the neutral electrolyte are the same as in Example 1;

[0093] 3. Preparation of gel electrolytes

[0094] 150 μL of weakly acidic electrolyte was transferred onto a 16 mm diameter polytetrafluoroethylene plate using a pipette. The plate was then photoinitiated with a 254 nm UV lamp for 5 min to obtain a weakly acidic gel electrolyte. Subsequently, 150 μL of neutral electrolyte was added to the plate and the plate was photoinitiated with a 254 nm UV lamp for 3 min to obtain a decoupled gel electrolyte.

[0095] 300 μL of weakly acidic electrolyte was transferred onto a 16 mm diameter polytetrafluoroethylene plate using a pipette, and the weakly acidic gel electrolyte was obtained by photoinitiation with a 254 nm UV lamp for 8 min.

[0096] 300 μL of neutral electrolyte was transferred onto a 16 mm diameter polytetrafluoroethylene plate using a pipette, and the neutral gel electrolyte was obtained by photoinitiation with a 254 nm UV lamp for 8 min.

[0097] 4. Preparation of stainless steel symmetric cells

[0098] Each gel electrolyte is removed from the mold, and the negative electrode battery shell, spring sheet, gasket, gel electrolyte, gasket, and positive electrode battery shell are stacked in sequence. The mixture is then sealed using a hydraulic press with a pressure of 50 kg / cm². -2 A stainless steel symmetric cell was prepared.

[0099] Supplementary Example 2: Electrochemical Performance Characterization

[0100] Several stainless steel symmetrical cells prepared in Example 3 were subjected to EIS testing using an electrochemical workstation. The frequency range was generally 10 MHz to 10 kHz, and the amplitude was 5 mV, as shown in the attached figure. Figure 5 As shown, Nyquist plots for different gel electrolytes were obtained, and the ionic conductivity of the weakly acidic gel electrolyte was calculated to be 0.518 × 10⁻⁶. -2 S CM -2 The ionic conductivity of the neutral gel electrolyte is 4.284 × 10⁻⁶. -3 S CM -2 The ionic conductivity of the decoupled gel electrolyte is 1.171 × 10⁻⁶. -2 S CM -2 This indicates that decoupling has little effect on the ionic conductivity of the gel electrolyte, and both exhibit good ionic conductivity.

[0101] Example 4

[0102] A method for preparing a weakly acidic aqueous zinc-manganese battery without a positive electrode, the specific steps of which are as follows:

[0103] 1. Preparation of weakly acidic citric acid solution, same as in Example 1;

[0104] 2. Preparation of electrolyte: The weakly acidic electrolyte and the neutral electrolyte are the same as in Example 1;

[0105] 3. Preparation of the decoupling gel electrolyte is the same as in Example 1;

[0106] 4. Assembly of a weakly acidic aqueous zinc-manganese battery without a positive electrode.

[0107] The decoupling gel electrolyte is removed from the mold. Using a zinc sheet as the negative electrode and hydrophilic carbon paper as the positive electrode current collector, the negative electrode battery casing, spring contact, gasket, zinc sheet, decoupling gel electrolyte, conductive carbon paper, and positive electrode battery casing are stacked sequentially. The casing is then encapsulated using a hydraulic press with a pressure of 50 kg / cm². -2 A zinc-manganese button cell without a positive electrode was prepared, wherein the weakly acidic gel electrolyte side of the decoupled gel electrolyte is bonded to carbon paper, and the neutral gel electrolyte is bonded to a zinc sheet.

[0108] 5. Active substance loading

[0109] By using the Blue Electric Electrochemical Workstation to charge the electrolyte at a constant voltage of 2.2V for 30 minutes, the manganese ions in the electrolyte were oxidized to manganese oxide, and finally an aqueous zinc-manganese battery was prepared.

[0110] Supplementary Example 3 characterizes the manganese oxide in the weakly acidic aqueous zinc-manganese battery without a positive electrode in Example 4.

[0111] The electrodeless, weakly acidic aqueous zinc-manganese battery prepared in Example 4 was disassembled using a hydraulic press at a pressure of 50 kg / cm². -2 The conductive carbon paper was peeled off and washed with ethanol, and then dried in an oven at 70°C for 3 hours.

[0112] 1. Morphology Analysis: SEM images of the conductive carbon paper after constant voltage charging are attached. Figure 6 As shown, a dense layer of manganese oxide is attached to the surface of the carbon paper fiber, proving the successful deposition of manganese oxide. At the same time, the density of its deposition on the carbon paper surface provides a guarantee for the subsequent battery performance.

[0113] 2. Elemental Analysis: The deposits on the surface of the carbon paper after constant voltage charging were scraped off for XRD analysis, as shown in the attached figure. Figure 7As shown, analysis revealed that the manganese oxide consisted of MnO2 and MnOOH, with the MnO2 crystal form being β-type MnO2. XPS analysis was also performed on the carbon paper after constant voltage charging, as shown in the attached figure. Figure 8 As shown, Mn can be observed by fitting the Mn 2p spectrum. 4+ and Mn 3+ The presence of peaks, including Mn-O-Mn and Mn-OH peaks, can also be observed in the O1s spectrum, which further indicates that the manganese oxides deposited on the carbon paper surface by constant voltage charging are MnO2 and MnOOH.

[0114] Supplementary Example 4: Discharge Performance Characterization

[0115] 1. Characterization by discharge curve

[0116] The electrodeless, weakly acidic aqueous zinc-manganese battery prepared in Example 4 was tested at 0.5 mA / cm². -2 A constant current discharge was performed at a current density to 0.8V, and its discharge curve is shown in the attached figure. Figure 9 As shown, the discharge curve has two discharge plateaus. In the range of 2.0V-1.5V, MnO2 undergoes a two-electron reduction reaction to become manganese ions. In the range of 1.5V-1.2V, MnOOH undergoes single-ion migration and reaction with zinc ions to form zinc manganese oxide. Below 1.2V, the zinc manganese oxide continues to react and eventually forms basic zinc sulfate.

[0117] 2. Morphological characteristics

[0118] The battery, after constant voltage charging, was sequentially charged at 0.5mA cm. -2 The battery was subjected to constant current discharge at current densities up to 1.8V, 1.4V, 1.2V, and 0.8V, and then disassembled using a hydraulic press. The conductive carbon paper was removed, cleaned, and dried. (See attached image.) Figure 10 As shown, when discharged to 1.8V and 1.4V, the manganese oxide deposited on the carbon paper surface is gradually reduced to manganese ions, while at 1.2V, a plate-like structure gradually forms and eventually forms a large-area deposition at the end of the discharge. The conductive carbon paper mapping diagram at 0.8V is attached. Figure 11 As shown, this demonstrates the successful deposition of basic zinc sulfate.

[0119] 3. Elemental Analysis

[0120] XPS analysis was performed on carbon paper discharged to different voltages, and the Mn 2p spectra are shown in the attached figure. Figure 12 As shown, the Mn4+ peak essentially disappears after discharging from 2.2V to 1.4V, while the Mn peak essentially disappears after discharging to 0.8V. This proves that the manganese oxide deposited on the carbon paper surface through constant voltage charging is almost completely reduced back to manganese ions. The O 1s spectrum is shown in the attached figure. Figure 13As shown, the Mn-O-Mn peak gradually weakens and disappears, which also indicates that the manganese oxides are basically reduced and dissolved back into the electrolyte.

[0121] Example 5

[0122] A method for preparing a cathodeless aqueous zinc-manganese battery, the specific steps of which are as follows:

[0123] 1. Preparation of weak acid solutions: Citric acid weak acid solution and sulfuric acid weak acid solution are the same as in Example 2;

[0124] 2. Preparation of electrolyte

[0125] Add 3g acrylamide, 5.6g zinc sulfate heptahydrate, and 1.7g manganese sulfate sequentially to 10g of the prepared citric acid weak acid solution, place on a magnetic stirrer and stir at room temperature for 5min. Then add 20μg N-N-methylenebisacrylamide and 20μL 2-hydroxy-2-methylphenylacetone sequentially, place on a stirrer and stir for 5min to obtain a citric acid weak acid electrolyte.

[0126] Add 3g acrylamide, 5.6g zinc sulfate heptahydrate, and 1.7g manganese sulfate to 10g of prepared sulfuric acid solution in sequence, place on a magnetic stirrer and stir at room temperature for 5min. Then add 20μg N-N-methylenebisacrylamide and 20μL 2-hydroxy-2-methylphenylacetone in sequence, place on a stirrer and stir for 5min to obtain a weakly acidic sulfuric acid electrolyte.

[0127] Add 3g acrylamide and 5.6g zinc sulfate heptahydrate to 10g deionized water, place on a stirrer and stir at room temperature for 5min. Then add 20μg NN methylenebisacrylamide and 20μL 2-hydroxy-2-methylphenylacetone, place on a stirrer and stir for 5min to obtain a neutral electrolyte.

[0128] Add 3g of acrylamide and 1.7g of manganese sulfate to 10g of the prepared citric acid weak acid solution, place on a magnetic stirrer and stir at room temperature for 5min. Then add 20μg of NN methylenebisacrylamide and 20μL of 2-hydroxy-2-methylphenylacetone, place on a stirrer and stir for 5min to obtain a zinc sulfate-free weak acid electrolyte.

[0129] 3. Preparation of gel electrolytes

[0130] 150 μL of citric acid electrolyte was transferred onto a 16 mm diameter polytetrafluoroethylene plate using a pipette. The plate was then photoinitiated for 5 min by a UV lamp with a wavelength of 254 nm to obtain a citric acid gel electrolyte. Subsequently, 150 μL of neutral electrolyte was added to the surface of the plate, and the plate was photoinitiated for 3 min by a UV lamp with a wavelength of 254 nm to obtain a decoupled citric acid gel electrolyte.

[0131] 150 μL of sulfuric acid electrolyte was transferred onto a 16 mm diameter polytetrafluoroethylene plate using a pipette. The plate was then photoinitiated for 5 min by a UV lamp with a wavelength of 254 nm to obtain a sulfuric acid gel electrolyte. Subsequently, 150 μL of neutral electrolyte was added to the plate and the plate was photoinitiated for 3 min by a UV lamp with a wavelength of 254 nm to obtain a decoupled sulfuric acid gel electrolyte.

[0132] 150 μL of zinc sulfate-free electrolyte was transferred onto a 16 mm diameter polytetrafluoroethylene plate using a pipette. The plate was then photoinitiated for 5 min by a UV lamp with a wavelength of 254 nm to obtain a zinc sulfate-free gel electrolyte. Subsequently, 150 μL of neutral electrolyte was added to the surface of the plate, and the plate was photoinitiated for 3 min by a UV lamp with a wavelength of 254 nm to obtain a decoupled zinc sulfate-free gel electrolyte.

[0133] 300 μL of citric acid electrolyte was transferred onto a 16 mm diameter polytetrafluoroethylene plate using a pipette, and the undecoupled gel electrolyte was obtained by photoinitiation with a 254 nm UV lamp for 8 min.

[0134] 4. Assembly of button cells without positive terminals

[0135] Using zinc sheet as the negative electrode and hydrophilic carbon paper as the positive electrode current collector, a negative electrode battery case, a spring, a gasket, and a zinc sheet are stacked sequentially. The prepared gel electrolytes, conductive carbon paper, and positive electrode battery case are then encapsulated using a hydraulic press at a pressure of 50 kg / cm². -2 A zinc-manganese button cell without a positive electrode was prepared.

[0136] 5. Active substance loading, same as in Example 4.

[0137] Supplementary Example 5: Electrochemical Performance Testing

[0138] 1. Characterization by discharge curve

[0139] The battery prepared in Example 5, containing decoupled citric acid, decoupled zinc sulfate-free, and non-decoupled citric acid gel electrolyte, was subjected to constant current discharge at a current density of 0.5 mA cm⁻², and the discharge curves were obtained, as shown in the attached figure. Figure 14 As shown, it can be seen that the full cell with decoupled zinc sulfate and the undecoupled electrolyte have two discharge platforms, while the second discharge platform of the decoupled zinc sulfate-free electrolyte is unclear. This is because the positive electrode of the battery with decoupled zinc sulfate-free gel electrolyte does not have zinc ions and cannot form basic zinc sulfate, so it only has the first discharge platform. The battery with undecoupled electrolyte is in a weakly acidic environment at the negative electrode zinc plate, which easily causes hydrogen absorption reaction and zinc dendrite phenomenon, resulting in capacity decay.

[0140] 2. Ratio Performance Test

[0141] The battery is kept at a constant voltage of 2.2V, with a current of 0.05-1.0mA / cm. -2 Charge-discharge performance was tested at current density, as shown in the attached figure. Figure 15 As shown, the battery with decoupled citric acid gel electrolyte exhibits good rate performance and capacity as the current density increases from 0.05 to 1 mA cm⁻¹. -2 The capacity of the decoupled citric acid gel electrolyte increased from 345 μAh cm⁻¹. -2 Increased to 452 μAhcm -2 In contrast, the undecoupled gel electrolyte and the undecoupled gel electrolyte without zinc sulfate showed a significant decrease in capacity and had a lower capacity.

[0142] 3. Cyclic performance test

[0143] The battery was charged at a constant voltage of 2.2V for 5 minutes and then at a current of 0.5mA / cm. -2 Constant current discharge is performed using current density, as shown in the attached figure. Figure 16 As shown, the battery can achieve over 900 cycles, demonstrating its excellent cycle life. The battery capacity gradually increases during the first 250 cycles, and then remains relatively stable after that, while the efficiency remains consistently between 95% and 100%, indicating good charge / discharge capabilities. The battery was charged at a constant voltage of 2.2V for 30 minutes and then at a 0.5mA cm⁻¹. -2 Constant current discharge is performed using current density, as shown in the attached figure. Figure 17 As shown, after 200 discharge cycles, the discharge curve remained basically unchanged, and the cycle test time exceeded 202 hours, which means that the battery has a long service life and good cycle stability.

[0144] In summary, the method of the present invention has simple preparation steps. After the battery device is prepared, the active material is deposited by constant voltage charging, which eliminates the complicated steps of preparing active material coating. The cathode-free zinc-manganese battery has excellent rate capability and long cycle performance, while the gel electrolyte has green environmental protection and excellent mechanical and physical properties.

[0145] This invention uses UV photoinitiation technology to prepare decoupled gel electrolytes. The method is simple and convenient, and compared with thermal initiation, it consumes less energy and is faster. The prepared gel electrolyte can reduce zinc dendrite formation and improve service life. At the same time, it can reduce free water content, broaden the voltage window of the battery, and endow the energy storage device with excellent cycle stability and capacity.

[0146] The various embodiments in this specification are described in a progressive manner, with each embodiment focusing on its differences from other embodiments. Similar or identical parts between embodiments can be referred to interchangeably. For the apparatus disclosed in the embodiments, since it corresponds to the method disclosed in the embodiments, the description is relatively simple; relevant parts can be referred to in the method section.

[0147] The present invention provides a detailed description of a cathode-free, weakly acidic aqueous zinc-manganese battery and its preparation method. Specific examples have been used to illustrate the principles and implementation methods of the invention. These examples are merely illustrative to aid in understanding the method and core concepts of the invention. It should be noted that those skilled in the art can make various improvements and modifications to the invention without departing from its principles, and these improvements and modifications also fall within the scope of protection of the claims.

Claims

1. A method for preparing a weakly acidic aqueous zinc-manganese battery without a positive electrode, characterized in that... The method includes the following steps: S1. Preparation of a weakly acidic solution: Dissolve an appropriate amount of acid in water and stir for 1-5 hours to prepare a weakly acidic solution with a pH of 2-3. The acid is selected from one or more of citric acid, concentrated sulfuric acid, carbonic acid, hydrochloric acid, malic acid, oxalic acid, or nitric acid; S2. Preparation of electrolyte: Acrylamide, zinc sulfate heptahydrate, and manganese sulfate are added to the weakly acidic solution prepared in S1 and mixed well. Then, NN methylenebisacrylamide and photoinitiator are added sequentially and mixed well to obtain a weakly acidic electrolyte. The weakly acidic electrolyte contains the following components by mass percentage: acrylamide 15-30%, zinc sulfate heptahydrate 25-30%, manganese sulfate 5-10%, NN methylenebisacrylamide 0.05-0.5%, photoinitiator 0.05-0.5%, and the balance is a weakly acidic solution with a pH of 3-5. Acrylamide and zinc sulfate heptahydrate are added to water sequentially and mixed well. Then, NN methylenebisacrylamide and photoinitiator are added sequentially and mixed well to obtain a neutral electrolyte. The neutral electrolyte contains the following components by mass percentage: 15-30% acrylamide, 25-30% zinc sulfate heptahydrate, 0.05-0.5% NN methylenebisacrylamide, 0.05-0.5% photoinitiator, and the balance is water. The photoinitiator is selected from one or more of 2-hydroxy-2-methylphenylacetone, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, 2-methyl-2-(4-morpholino)-1-[4-(methylthio)phenyl]-1-propanone, and 1-hydroxycyclohexylphenyl ketone. S3. Preparation of decoupling gel electrolyte: A weakly acidic electrolyte was injected into a polytetrafluoroethylene template, and a photoinitiated reaction was carried out by irradiation with a UV lamp. The resulting weakly acidic gel electrolyte was obtained after the reaction. Neutral electrolyte is stacked on the surface of a weakly acidic gel electrolyte, and a photo-initiated reaction is carried out by irradiation with a UV lamp. After the reaction, a decoupled gel electrolyte is obtained. The thickness of the weakly acidic gel electrolyte is 0.25-2 mm, and the UV lamp initiation time is 2-30 min; the thickness of the neutral gel electrolyte is 0.25-2 mm, and the UV lamp initiation time is 2-30 min; the thickness of the decoupling gel electrolyte is 0.5-4 mm. S4, Preparation of cathodeless coin cell batteries Using the decoupled gel electrolyte prepared by S3 as the electrolyte of the battery, a zinc-manganese button cell without a positive electrode was prepared by encapsulation. In the decoupled gel electrolyte, the weakly acidic gel electrolyte side is attached to the positive current collector of the battery, and the neutral gel electrolyte side is attached to the negative electrode of the battery. S5, Active Material Loading A weakly acidic aqueous zinc-manganese battery without a positive electrode was prepared by oxidizing manganese ions in the electrolyte of the battery to manganese oxide using the Blue Electric Electrochemical Workstation.

2. The preparation method according to claim 1, characterized in that: The wavelength of the UV lamp is 250-400 nm.

3. The preparation method according to claim 1, characterized in that: The positive current collector in S4 is one of conductive carbon paper, carbon cloth, or graphite paper.

4. The preparation method according to claim 1, characterized in that: The pressure used during encapsulation in S4 is 25-100 kg / cm². -2 .

5. The preparation method according to claim 1, characterized in that: The S5 constant voltage charging voltage is 1.6-2.4 V, and the constant voltage charging time is 1-120 min.

6. The preparation method according to claim 1, characterized in that: S4. The method for preparing a cathodeless coin cell is as follows: Using zinc sheet as the negative electrode and hydrophilic carbon material as the positive electrode current collector, the negative electrode battery shell, spring sheet, gasket, zinc sheet, decoupling gel electrolyte, positive electrode current collector and positive electrode battery shell are stacked in sequence and then packaged using a hydraulic press.

7. The preparation method according to claim 1, characterized in that: Conditions for loading active substances in S5: Perform chronoamperometry or constant voltage charging at 2.1-2.3 V.