Method for manufacturing titanium foil
By optimizing the titanium ion concentration, temperature, and current density in a molten salt bath, the problems of low titanium foil manufacturing efficiency and difficult peeling were solved, achieving efficient titanium foil production.
Patent Information
- Application Number
- CN202280011506.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-02-25
- Filing Date
- 2022-02-22
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2042-02-22
AI Technical Summary
Existing technologies for manufacturing thin titanium foil suffer from low manufacturing efficiency and difficulty in peeling off electrodeposited titanium foil, especially when using pulsed current, where the manufacturing efficiency of titanium foil needs to be improved.
By increasing the concentration of titanium ions in the molten salt bath, controlling the electrolysis temperature and current density, and combining this with an appropriate current carrying time, the electrodeposition process conditions are optimized to ensure efficient deposition of titanium foil on the cathode and easy peeling.
This method achieves an increase in the amount of metallic titanium electrodeposited per unit time without reducing the ease of titanium foil peeling, thereby improving the manufacturing efficiency and smoothness of titanium foil.
Smart Images

Figure CN116745465B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a method for manufacturing titanium foil by electrolysis using a molten salt bath and electrodes comprising an anode and a cathode, thereby depositing metallic titanium at the cathode. Background Technology
[0002] Metallic titanium is typically manufactured using the Kroll process, which is suitable for mass production. In the production of metallic titanium, titanium oxide contained in titanium ore reacts with chlorine in the presence of a carbon source such as coke to produce titanium tetrachloride. Then, titanium tetrachloride is reduced with metallic magnesium to obtain sponge-like metallic titanium, also known as sponge titanium.
[0003] In the case of manufacturing thin foil-shaped metallic titanium using sponge titanium as the main raw material, the process typically involves melting and casting the sponge titanium to produce titanium ingots or slabs, followed by further processing such as forging and rolling. Given this process requiring melting and processing, it is difficult to say that it is possible to efficiently and cost-effectively manufacture metallic titanium in foil or other prescribed shapes.
[0004] In this context, from the perspective of reducing energy consumption and lowering costs in the manufacturing process, an alternative to the above-mentioned melting and processing was studied: using molten salt electrolysis to precipitate metallic titanium via a molten salt bath.
[0005] As a technology related to molten salt electrolysis, there are, for example, the technologies described in Patent Documents 1 to 3.
[0006] Patent document 1 describes: "A method for manufacturing high-purity titanium, characterized in that, in the method of manufacturing high-purity titanium by means of molten salt electrolysis, electrolysis is carried out in a chloride bath in which sodium ions as a bath component are 10 wt% or less", and "when electrolysis is carried out in a low electrolysis bath with a melting point of 400°C or less, the electrolysis is carried out in the range of 550 to 900°C".
[0007] In Patent Document 1, it is stated that "when using a bath with a low melting point (below 400°C) such as LiCl-KCl, electrolysis is usually carried out at 400-500°C. However, at this temperature, the electrodeposited Ti will become spongy or powdery. In this state, there is more oxygen, and the loss also increases, which deteriorates the yield." It teaches that "by setting the bath temperature to 550-900°C, preferably 600-750°C, as shown in Table 2, the electrodeposited Ti can be made into coarse crystals, specifically hexagonal plates or dendritic shapes, thereby reducing oxygen and increasing the yield."
[0008] Patent document 2 discloses "a method for manufacturing titanium, characterized in that, when purifying raw titanium by electrolysis using a molten salt electrolysis method, a voltage is applied between a container filled with raw titanium as the anode and an electrolytic container as the cathode." Specifically, it describes the following: "As a molten salt electrolysis step, firstly, starting from a state where raw titanium T and titanium rod 3 have not been loaded into the container body 1a, a mixed chloride of NaCl and KCl premixed in a molar ratio of 1:1 is added to the container body 1a. Next, the mixed chloride is heated to 650°C under reduced pressure to fully dehydrate it. Then, the furnace atmosphere is replaced with argon, and the temperature is raised to 740°C and maintained to melt the mixed chloride and form an electrolytic bath 4. Then, the raw titanium T and titanium rod 3 are immersed in the electrolytic bath." In bath 4, and with the cover 1b closed. Next, liquid TiCl4 is blown into the bottom of the raw material titanium T at an appropriate flow rate through a supply pipe (not shown) to generate titanium ions in the electrolytic bath. Then, voltages are applied to both the electrolysis circuit 11 and the impurity melting prevention circuit 21 using direct current. The voltage of the electrolysis circuit 11 is set to 100–1000 mV, and the voltage of the impurity melting prevention circuit 21 is set to 500 mV or less, preferably 10–150 mV, and more preferably 30–100 mV.
[0009] Patent document 3 discloses "a method for manufacturing metallic titanium, which involves electrolysis in a molten salt bath using an anode and a cathode to produce metallic titanium. The method includes a titanium deposition step, in which metallic titanium is deposited on a cathode using an anode containing metallic titanium as the anode, wherein the temperature of the molten salt bath is set to 250°C or higher and 600°C or lower, and the average current density of the cathode is maintained at 0.01 A / cm² for a period of 30 minutes from the start of the titanium deposition step." 2 ~0.09A / cm 2 Within the range of… In the embodiment of Patent Document 3, it is described that “a pulsed current that is repeatedly applied and stopped flows through the anode and cathode at a predetermined interval, thereby performing electrolysis, melting the anode, and depositing metallic titanium in a foil-like form on the cathode” (see Table 1).
[0010] Existing technical documents
[0011] Patent documents
[0012] Patent Document 1: Japanese Patent Application Publication No. 3-291391
[0013] Patent Document 2: Japanese Patent Application Publication No. 2000-87280
[0014] Patent Document 3: International Publication No. 2020 / 044841 Summary of the Invention
[0015] The problem that the invention aims to solve
[0016] In the method described in Patent Document 3, metallic titanium is electrodeposited thinly on the cathode, and it is also relatively easy to peel the metallic titanium off the cathode. Therefore, it is believed that a thin titanium foil can be obtained according to this method.
[0017] However, in the method described in Patent Document 3, when energizing the electrode, an intermittent current, such as a pulsed current, sometimes flows. In this case, due to the time it takes for the pulsed current to stop, the electrodeposition of metallic titanium onto the cathode requires a certain amount of time, thus leaving room for improvement in the manufacturing efficiency of the titanium foil.
[0018] The purpose of this invention is to provide a method for manufacturing titanium foil that can increase the amount of titanium electrodeposited per unit time without significantly reducing the ease of peeling the titanium electrodeposited on the cathode from the cathode.
[0019] Solution for solving the problem
[0020] It can be argued that the electrodeposition of metallic titanium onto the cathode is promoted by the high concentration of titanium ions in the molten salt bath, the increase in the temperature of the molten salt bath, and the increase in the current density when current is applied to the electrode. On the other hand, these factors may reduce the ease with which metallic titanium can be peeled off from the cathode.
[0021] The inventors conducted in-depth research and discovered a new, suitable combination of the above conditions. Therefore, even with a significantly shortened time of stopping the current to the electrode, or without stopping the current, the reduction in the ease of peeling off metallic titanium can be suppressed. Furthermore, by shortening the time of stopping the current to the electrode or by not stopping the current, an increase in the amount of metallic titanium electrodeposited per unit time can be achieved.
[0022] The method for manufacturing titanium foil of the present invention includes: an electrodeposition step, using a molten salt bath containing titanium ions and formed by molten chloride, electrolyzing using electrodes including an anode and a cathode to deposit metallic titanium on the electrolytic surface of the cathode; in the electrodeposition step, maintaining the ratio of the molar concentration of titanium ions in the molten salt bath to the total molar concentration of metal ions at 7% or more, maintaining the temperature of the molten salt bath at 510°C or below, setting the continuous interruption time of energizing the electrodes to be less than 1.0 second, and setting the current density to 0.10 A / cm². 2 Above and 1.0 A / cm 2 Hereinafter, the electrodeposition time of metallic titanium onto the electrolytic surface of the cathode will be set to 120 minutes or less.
[0023] Preferably, in the above-described method for manufacturing titanium foil, the anode contains Ti and is consumed in the electrodeposition process.
[0024] Furthermore, preferably, in the above-described method for manufacturing titanium foil, the chloride comprises titanium dichloride and / or titanium trichloride.
[0025] Preferably, in the electrodeposition process, the molar concentration of titanium ions in the molten salt bath is maintained at a ratio of more than 10% to the total molar concentration of metal ions.
[0026] Furthermore, it is preferable to maintain the temperature of the molten salt bath below 500°C during the electrodeposition process.
[0027] Furthermore, it is preferable to set the current density to 0.20 A / cm during the electrodeposition process. 2 Above and 0.50A / cm 2 the following.
[0028] Invention Effects
[0029] According to the method for manufacturing titanium foil of the present invention, the amount of titanium electrodeposited per unit time can be increased without reducing the ease with which metallic titanium electrodeposited on the cathode can be peeled off from the cathode. Attached Figure Description
[0030] Figure 1 This is a schematic cross-sectional view of an electrolytic apparatus that can be used in a method for manufacturing titanium foil according to one embodiment of the present invention.
[0031] Figure 2 It is a partial sectional perspective view of another electrolysis device, schematically showing the parts other than the electrodes.
[0032] Figure 3 It is a schematic cross-sectional view of yet another electrolysis unit.
[0033] Figure 4 It is a schematic cross-sectional view of yet another electrolysis unit.
[0034] Figure 5 This is a photograph of metallic titanium electrodeposited on the cathode of Example 1.
[0035] Figure 6 This is a photograph of metallic titanium electrodeposited on the cathode of Comparative Example 2.
[0036] Figure 7 This is a cross-sectional view representing a peel strength test. Detailed Implementation
[0037] The embodiments of the present invention will now be described in detail. It should be noted that the descriptions of each embodiment are provided using… Figures 1-4 as well as Figure 7 This is a diagram that roughly represents its composition. Therefore, Figures 1-4as well as Figure 7 The configurations, dimensions, etc. of the components shown are sometimes inaccurate.
[0038] One embodiment of the present invention provides a method for manufacturing titanium foil, comprising an electrodeposition step. The electrodeposition step utilizes a molten salt bath containing titanium ions and formed by molten chloride, and electrolysis is performed using electrodes comprising an anode and a cathode to deposit metallic titanium on the electrolytic surface of the cathode. Furthermore, in the electrodeposition step, the ratio of the molar concentration of titanium ions in the molten salt bath to the total molar concentration of metal ions is maintained at 7% or more, and the temperature of the molten salt bath is maintained at 510°C or lower. Additionally, in the electrodeposition step, the continuous interruption time of energizing the electrodes is set to less than 1.0 second, and the current density is set to 0.10 A / cm². 2 Above and 1.0 A / cm 2 The electrodeposition time of metallic titanium onto the electrolytic surface of the cathode in the electrodeposition process is set to 120 minutes or less. It should be noted that, in the description of each embodiment, the ratio of the molar concentration of titanium ions in the molten salt bath to the total molar concentration of metal ions is simply referred to as the "titanium ion ratio".
[0039] In this molten salt electrolysis, the high concentration of titanium ions in the molten salt bath, the increase in the temperature of the molten salt bath, and the increase in the current density when current is applied to the electrode promote the electrodeposition of metallic titanium onto the cathode, tending to increase the amount of metallic titanium electrodeposited per unit time. However, if all these factors are present, it is difficult to peel the metallic titanium electrodeposited on the cathode from the cathode. In particular, it is difficult to perform physical stripping such as peeling the electrodeposited metallic titanium from the electrode.
[0040] In contrast, in this embodiment, during the electrodeposition process, the concentration of titanium ions in the molten salt bath is increased to 7% or more, and the current density is increased to 0.10 A / cm². 2 Above and 1.0 A / cm 2 Below. On the other hand, the temperature of the molten salt bath is set to a relatively low temperature of 510°C or below. This increases the amount of titanium electrodeposited per unit time and facilitates the easy stripping of titanium from the cathode. In particular, physical stripping, such as peeling the electrodeposited titanium from the electrode, can be easily performed.
[0041] The reasoning is uncertain, but it can be hypothesized as follows: By increasing the proportion of titanium ions in the molten salt bath as described above, even if these titanium ions are deposited as metallic titanium on the cathode through current supply to the electrode, titanium ions near the cathode are not easily deficient. Therefore, it is believed that current deviation near the cathode is suppressed, and the deposition of dendrite-like metallic titanium caused by this current deviation is suppressed, resulting in foil-like deposition of metallic titanium on the cathode. Furthermore, no power concentration associated with dendrite formation is caused, thus suppressing the temperature rise of the cathode surface. Furthermore, the temperature of the molten salt bath is appropriately maintained at a low level, thus appropriately suppressing the temperature rise of the cathode surface. As a result, interdiffusion of metals between the cathode and the metallic titanium deposited on the cathode is suppressed. Therefore, it is hypothesized that even if the time for stopping current supply to the electrode is sufficiently shortened, such as to be less than 1.0 second, and the current is kept constant without stopping current supply, the electrodeposited metallic titanium can be easily peeled off from the cathode. However, the present invention is not limited to the theory described above.
[0042] Furthermore, in this embodiment, the continuous interruption of power supply time is set to less than 1.0 second, thus increasing the amount of titanium electrodeposited per unit time, thereby improving the manufacturing efficiency of titanium foil. Moreover, the titanium foil manufactured in this way exhibits excellent smoothness by suppressing dendrite formation.
[0043] (Molten salt bath)
[0044] The molten salt constituting the molten salt bath in the electrolytic cell is formed by melting chlorides. Preferably, the molten salt bath is formed by melting only chlorides as compounds. Specific chlorides include, for example, MgCl2, NaCl, KCl, CaCl2, LiCl, BaCl2, CsCl, etc.
[0045] The molten salt bath preferably contains one or more, or more than two, chlorides selected from the group consisting of MgCl2, NaCl, KCl, CaCl2, LiCl, BaCl2, and CsCl. It should be noted that the molten salt bath preferably contains one or more, or more than two, or more than three, chlorides selected from the group consisting of MgCl2, NaCl, KCl, CaCl2, and LiCl. Furthermore, the molten salt bath preferably contains one or more, or more than two, or more than three, chlorides selected from the group consisting of MgCl2, NaCl, KCl, and CaCl2. Specific examples of such preferred chlorides include: NaCl-KCl-MgCl2, LiCl-KCl-MgCl2, NaCl-KCl-CaCl2, LiCl-KCl-CaCl2, NaCl-LiCl-KCl-MgCl2, and NaCl-KCl-LiCl-CaCl2. By including the above-mentioned chlorides, the molten state of the molten salt bath can be well maintained even at certain low temperatures, thus easily achieving the aforementioned low temperature range of the molten salt bath in the electrodeposition process.
[0046] The combined molar concentrations of magnesium, sodium, potassium, calcium, lithium, barium, and cesium ions, relative to the total molar concentrations of all metal ions in the molten salt bath, can preferably be set to 80% or more, and more preferably 90% or more. However, considering factors such as operating temperature, the specific types and contents of chlorides can be appropriately determined. It should be noted that the molar concentrations of each metal ion are calculated using ICP-N (Inductively Coupled Phosphorescence) and atomic absorption spectrometry.
[0047] Ideally, the molten salt bath should be free of fluoride ions. In titanium foil obtained by peeling off metallic titanium deposited on the cathode during the electrodeposition process, components from the molten salt bath often remain on the surface. To remove these components, the titanium foil is sometimes washed with water after the electrodeposition process. However, if the components of the molten salt bath remaining on the surface of the titanium foil contain fluorides, harmful hydrogen fluoride or hydrofluoric acid can be generated upon contact with water. Furthermore, in cases where lithium fluoride is melted in the molten salt bath, lithium fluoride is poorly soluble in water, thus requiring a large amount of water for removal from the titanium foil by washing. To reduce such burden on operators and the environment, it is preferable to use a molten salt bath free of fluoride ions.
[0048] In addition, the molten salt bath contains titanium ions. To include titanium ions in the molten salt bath, the titanium raw material can be pre-melted in the molten salt bath before the electrodeposition process and / or, as described later, the Ti-containing anode can be melted before or during the electrodeposition process.
[0049] When titanium raw materials are pre-melted in a molten salt bath, more specifically, examples of titanium raw materials include titanium chloride and / or low-purity titanium containing impurities, such as titanium scrap or sponge titanium. Low-purity titanium containing impurities sometimes contains significant amounts of Fe and O as impurities. When titanium scrap or sponge titanium is used as a titanium raw material, it can be contacted with TiCl4 to generate low-grade titanium chlorides such as titanium dichloride (TiCl2) and / or titanium trichloride (TiCl3), which then melt to form a molten salt bath containing titanium ions. Here, after the titanium raw material is melted in the molten salt bath, metallic titanium is deposited at the cathode, thus suppressing the incorporation of impurities into the metallic titanium even if the titanium raw material contains significant impurities.
[0050] (Electrolysis apparatus)
[0051] In this invention, various electrolysis devices can be used. As one example, Figure 1 The electrolysis apparatus 1 shown includes: a sealed container-shaped electrolytic cell 2, inside which a molten salt bath Bf is disposed; electrodes 3, including an anode 3a and a cathode 3b disposed within the electrolysis apparatus 1 and immersed in the molten salt bath Bf; and a power supply 4 connected to the anode 3a and cathode 3b, energizing the anode 3a and cathode 3b. Although not shown in the figure, a portion of the electrolytic cell 2 is typically open, allowing for actions such as placing the electrodes 3 within the electrolytic cell 2 using the opening. Alternatively, the opening can be sealed to prevent atmospheric contamination from the external environment into the electrolytic cell 2 during the energization of the electrodes 3. In the anode melting process and / or electrodeposition process, the electrolytic cell 2 is sometimes maintained under reduced pressure or an inert gas atmosphere based on argon or the like.
[0052] Here, in the molten salt bath Bf immersed in the electrolytic cell 2, the anode 3a preferably contains Ti. The anode 3a can take various shapes, such as sheet, cylinder, column, plate, block, powder, granule, fibrous, or agglomerate. Specifically, sponge titanium, titanium scrap, titanium rods, and / or titanium plates can be used as the anode 3a. Furthermore, sponge titanium and / or titanium scrap can be used as the anode 3a. When sponge titanium is used as the anode 3a, the blocky sponge titanium is placed inside a cage made of Ni or the like, and an electric current is applied to the cage. Ni has a lower ionization tendency than Ti, so only the sponge titanium as the anode 3a can be melted without Ni melting out. In this case, the cage is also included as part of the anode 3a, which contains both Ti and Ni. In the anode 3a containing the cage and its contents (sponge titanium, etc.), the contents, mostly containing Ti, are consumed during the anode melting and electrodeposition processes; the cage is not consumed. Furthermore, as described above, a bulk anode can be used as the anode 3a. By using a bulk anode, the anode can be constructed without using a cage made of Ni or similar materials.
[0053] Furthermore, the material of the cathode 3b is not particularly important as long as it is a material used for titanium electrodeposition. It should be noted that the cathode 3b sometimes uses an alloy in which the electrolytic surface for titanium electrodeposition contains at least Mo, W, Ta, or Nb, or any of these. Preferably, the cathode 3b contains at least 90% by mass of Mo, and more preferably 99.9% by mass of Mo. Mo does not readily melt into Ti below 600°C; therefore, the electrolytic surface of the cathode 3b containing 90% by mass of Mo does not adhere tightly to the titanium deposited on the cathode, allowing for easy peeling off of the titanium and suppressing the incorporation of impurities such as Mo into the titanium.
[0054] When the cathode 3b has multiple layers of different materials, an electrolytic surface containing at least 90% by mass of Mo can be formed in at least the surface layer of these layers by coating the cathode surface. The electrolytic surface of the cathode 3b sometimes contains impurities other than less than 10% by mass of Mo; examples of such impurities include Ti. When the cathode 3b is repeatedly used, it may sometimes contain a certain amount of Ti. It should be noted that not only can the electrolytic surface of the cathode 3b be composed of at least 90% by mass of Mo, but the entire cathode 3b can also be composed of at least 90% by mass of Mo.
[0055] The anode (which, in the case of the cage described above, is its contents) and the cathode can respectively take the form of, for example, generally rod-shaped, strip-shaped, plate-shaped, or cylindrical, other columnar or block-shaped forms. In particular, such as... Figure 2 As illustrated in the example, the cathode 33b preferably has at least a curved surface shape for at least a portion of the electrolytic surface for titanium electrodeposition. However, the anode and cathode can also be plate-shaped. Regarding the cathode, a plate-shaped shape is sometimes preferred. Figure 2 The electrolysis apparatus 31 shown has modified the shapes of the anode 33a and cathode 33b, and otherwise has the same... Figure 1 The electrolysis apparatus 1 shown has a substantially similar configuration, namely, it includes a cylindrical cathode 33b with a cylindrical surface, and a cylindrical anode 33a arranged to surround the cathode 33b. When both the surfaces of the anode 33a and the cathode 33b are curved, it is easy to fix the distance between the electrodes even if the cathode 33b is made movable, thus enabling more uniform deposition of metallic titanium over a large area of the surface (electrolysis surface) of the cathode 33b. From this viewpoint, it is preferable that the surfaces of the anode 33a and the opposing cathode 33b have similar shapes.
[0056] Figure 3 Another electrolysis device 11 is shown. Figure 3In the electrolysis apparatus 11, within a sealed electrolytic cell 12, a cylindrical or cylindrical cathode 13b, serving as a so-called cathode drum, is immersed in a molten salt bath Bf, with a portion of its cylindrical surface disposed therein. Furthermore, in this electrolysis apparatus 11, within the molten salt bath Bf, a plate-shaped anode 13a, shaped to conform to the surface of the cylindrical cathode 13b, is positioned opposite the surface of the cathode 13b.
[0057] exist Figure 3 In the electrolysis apparatus 11, when the cylindrical or cylindrical cathode 13b is rotated about its central axis and energized by a power source (not shown), a portion of the circumferential part of the surface of the cathode 13b immersed in the molten salt bath Bf, mainly opposite the anode 13a, becomes the electrolytic surface where metallic titanium is deposited, and foil-shaped metallic titanium Ts are deposited on this electrolytic surface. The portion of the surface of the cathode 13b immersed in the molten salt bath Bf changes with the rotation of the cathode 13b, and the electrolytic surface moves accordingly along the circumferential direction of the cathode 13b. Here, by using the winding roller 15 further provided in the electrolysis apparatus 11 to wind up the metallic titanium Ts, titanium foil as long strips of metallic titanium Ts can be continuously produced by peeling it off from the surface of the cathode 13b.
[0058] Figure 4 Another electrolysis apparatus 21 shown is an electrolysis apparatus in which a strip-shaped cathode 23b, serving as a cathode strip, is wound into a ring shape between a pair of rotating rollers 26a and 26b. Furthermore, in this apparatus, a plate-shaped anode 23a, such as a flat plate, is arranged in a manner that partially faces the cathode 23b in the molten salt bath Bf. The cathode 23b is located in a closed electrolysis tank 22 such that a portion of its outer surface, wound into a ring shape, is immersed in the molten salt bath Bf. In this electrolysis apparatus 21, the portion of the surface of the cathode 23b immersed in the molten salt bath Bf that mainly faces the anode 23a becomes the electrolytic surface.
[0059] according to Figure 4 The electrolysis apparatus 21, for example, involves rotating the drive-side rotating roller 26a, causing the strip-shaped cathode 23b and its electrolytic surface to rotate around the rotating rollers 26a and 26b. Figure 4 The cathode 23 moves as indicated by the middle arrow, and the driven side rotating roller 26b follows its rotation. At this time, energizing the electrode 23 by a power source (not shown) causes metallic titanium Ts to be deposited in a foil-like form on the electrolytic surface outside the cathode 23b. The metallic titanium Ts are wound up by the winding roller 25 while being peeled off from the surface of the cathode 23b, thereby enabling the continuous production of long strips of metallic titanium foil.
[0060] It should be noted that the electrode distance between the anode and cathode is not particularly limited, but is preferably 0.5 cm or more and 10.0 cm or less at any point on their opposing surfaces. It should also be noted that the electrode distance between the anode and cathode is preferably 1.0 cm or more and 8.0 cm or less, and further preferably 1.0 cm or more and 5.0 cm or less. By setting the electrode distance to 0.5 cm or more, the occurrence of short circuits between the electrodes can be suppressed. Furthermore, by setting the electrode distance to 10.0 cm or less, unintentional voltage rises can be suppressed, saving power consumption. This electrode distance refers to the shortest distance between the surface of the anode and the surface of the cathode. It should be noted that when the anode has a cage made of Ni or the like as described above and sponge titanium or the like disposed therein, the above electrode distance is set as the shortest distance from the end of the cage to the surface of the cathode.
[0061] In the following explanation, Figure 1 The electrolysis apparatus 1 shown is used as an example for explanation, but when using... Figures 2-4 The same principle can be applied to electrolysis devices 11, 21, and 31.
[0062] (Anodic melting process)
[0063] An anodic melting process can be performed before the electrodeposition process to consume the Ti-containing anode 3a and supply titanium ions to the molten salt bath Bf. However, the anodic melting process can also be omitted.
[0064] In the anodic melting process, an appropriate current is passed between the anode 3a and the cathode 3b immersed in the molten salt bath Bf while maintaining the molten salt bath Bf at a specified temperature, in a manner substantially the same as in conventional molten salt electrolysis.
[0065] Thus, the Ti-containing anode 3a melts into the molten salt bath Bf, where titanium ions will be present. That is to say, here, the anode 3a functions as a so-called consumable electrode to supply titanium ions to the molten salt bath Bf.
[0066] The temperature of the molten salt bath Bf in the anolyte melting process can be set to 250℃~800℃, provided that it is in a molten state. Furthermore, the current density of the cathode 3b can be set to 0.01A / cm². 2 ~2.00A / cm 2 Therefore, the melting of anode 3a proceeded well.
[0067] Here, the current density of cathode 3b can be calculated using the formula: Current density (A / cm²) 2 = Current value (A) ÷ Electrolytic area (cm²) 2The calculation is performed using this formula. Here, regarding the electrolytic area, for example in the case of a cathode 3b with a cylindrical surface, it is based on the formula: Electrolytic area (cm²) 2 The current density is calculated as follows: cathode impregnation surface area = cathode diameter (cm) × π × cathode height (cm). Furthermore, the current value is the average value of the current flowing within a specified time period for which the current density is calculated. For example, if a constant current flows, its value becomes the aforementioned current value. If the current value changes according to the passage of time, for example, current measurements can be obtained within equal time intervals during the energizing period, and the current value can be calculated using "total current measurements ÷ number of measurements". The current density of cathode 3b can also be calculated similarly for the electrodeposition process described later.
[0068] It should be noted that in the anodic melting process, the cathode 3b can be replaced before the electrodeposition process after the titanium ions are supplied to the molten salt bath Bf. During the anodic melting process, metals other than Ti sometimes precipitate on the cathode 3b. Therefore, if the cathode 3b in this state is used for the electrodeposition process, the purity of the titanium obtained in the electrodeposition process may decrease. Furthermore, the titanium electrodeposited on the cathode 3b may alloy during the electrodeposition process, potentially reducing its peelability. Therefore, it is preferable to replace the cathode 3b after supplying titanium ions to the molten salt bath Bf during the anodic melting process.
[0069] (Electrodeposition process)
[0070] In the electrodeposition process, by passing an electric current from the power source 4 to the electrode 3, which contains the anode 3a and the cathode 3b, electrolysis is performed using the electrode 3, and titanium ions in the molten salt bath Bf are deposited as metallic titanium on the cathode 3b.
[0071] Electrolysis is performed such that the molar concentration of titanium ions (Mt) is maintained at 7% or higher relative to the total molar concentration of metal ions (Mm) in the molten salt bath Bf. If the proportion of titanium ions in the molten salt bath Bf is less than 7%, there will be a lack of titanium ions around the cathode 3b, which will cause a deviation in the current distribution around the cathode 3b, and dendrites may form on the metallic titanium on the cathode 3b. The formation of dendrites itself impairs the smoothness of the titanium foil obtained from the metallic titanium on the cathode 3b, and is therefore undesirable. Furthermore, it makes it difficult to peel the metallic titanium from the cathode 3b. From this perspective, the proportion of titanium ions in the molten salt bath Bf is preferably maintained at 10% or higher. There is no particular limitation on the upper limit of the above-mentioned Mt / Mm percentage, and the proportion of titanium ions can be appropriately varied within a range that can maintain the molten salt bath.
[0072] The molar concentrations of various metal ions containing titanium ions in the molten salt bath Bf were calculated as follows: After the molten salt sample collected from the molten salt bath was solidified, the composition of the sample was analyzed using ICP-luminescence analysis and atomic absorption spectrometry. Assuming the molten salt bath contains MgCl2, NaCl, KCl, CaCl2, LiCl, TiCl2, and TiCl3, the total molar concentration of the metal ions (Mm) was obtained by adding the molar concentrations of magnesium ions, sodium ions, potassium ions, calcium ions, lithium ions, and titanium ions (Mt). The proportion of titanium ions could be calculated by dividing the molar concentration of titanium ions (Mt) by the total molar concentration of the metal ions (Mm) and expressing it as a percentage.
[0073] During the electrodeposition process, as metallic titanium is electrodeposited onto the cathode 3b, titanium ions in the molten salt bath Bf are consumed. In contrast, to maintain the high concentration of titanium ions in the molten salt bath Bf as described above, an anode 3a containing Ti is preferably used in the electrodeposition process. In this case, as electrolysis progresses, the anode 3a is consumed, and the Ti contained in the anode 3a becomes titanium ions and is supplied to the molten salt bath Bf. Thus, it is easy to maintain the titanium ion concentration in the molten salt bath Bf at a predetermined ratio.
[0074] Furthermore, the temperature of the molten salt bath Bf in the electrodeposition process is set to be maintained below 510°C, preferably below 500°C, and even more preferably below 480°C. If the temperature of the molten salt bath Bf is too high, the titanium grains electrodeposited on the cathode 3b are prone to coarsening, and dendrite growth may be intensified. It should be noted that if the molten salt constituting the molten salt bath Bf can be maintained in a molten state and electrolysis using the molten salt bath Bf can be performed, the temperature of the molten salt bath Bf can be sufficiently reduced.
[0075] In addition, when current is applied to electrode 3, the current density is set to 0.10 A / cm. 2 Above and 1.0 A / cm 2 Hereinafter, it is further preferred to set it to 0.10 A / cm 2 Above and 0.50A / cm 2 Hereinafter, a further preferred value is set to 0.20 A / cm. 2 Above and 0.50A / cm 2 The following describes how, by setting such a high current density, metallic titanium is electrodeposited onto the cathode 3b in a short time. Furthermore, even with the high current density described above, in this embodiment, metallic titanium can be easily peeled off from the cathode 3b. When the current density is below 0.10 A / cm... 2When the current density is greater than 1.0 A / cm², the amount of titanium electrodeposited per unit time on the cathode 3b decreases, and the manufacturing efficiency of the titanium foil decreases. 2 At that time, metallic titanium might not be easily peeled off from cathode 3b. It should be noted that, given the variation in current during the electrolysis process of the electrodeposition step, the aforementioned current density refers to the average value from the start to the end of the electrolysis.
[0076] In the electrodeposition process of this embodiment, the time during which the current is continuously stopped from flowing through electrode 3 (i.e., the time during which no current flows continuously) is set to less than 1.0 second, thus sufficiently shortening the time during which the current is continuously stopped from flowing through electrode 3, or continuously flowing through current without stopping the current. According to the embodiment, sometimes the current is continuously flowing through electrode 3 without stopping the current. If the time during which the current is continuously stopped from flowing through electrode 3 is less than 1.0 second, the amount of titanium metal electrodeposited per unit time on cathode 3b can be significantly increased. Even when a continuous stop time is set, it is preferable, for example, to make the continuous stop time extremely short relative to the current flow time, such that the proportion of the total continuous stop time during the electrodeposition time of titanium metal electrodeposited on the electrolytic surface of the cathode is set to 20% or less. It should be noted that stopping the current flow here means stopping the forward current that causes the electrolysis of titanium metal electrodeposited on the cathode. Therefore, even if a reverse current flows during at least a portion of the time during which the current flow is stopped, no forward current flows during this period, which is equivalent to stopping the current flow.
[0077] Particularly preferred is that the current supply to electrode 3 is not stopped, and a constant current is used so that the current value or current density does not change significantly. In this case, the current density is also preferably set within the aforementioned range.
[0078] In addition to the conditions mentioned above, the electrodeposition time of metallic titanium onto the electrolytic surface of the cathode is further set to 120 minutes or less. This not only improves the manufacturing efficiency of the titanium foil but also suppresses the formation of dendrites on the metallic titanium on the cathode 3b, thus improving the smoothness of the titanium foil. In the aforementioned... Figure 3 Electrolysis device 11 Figure 4 In the electrolysis apparatus 21, the electrolysis surfaces of cathodes 13b and 23b move. In this case, the electrodeposition time of metallic titanium at the predetermined surface position that becomes the electrolysis surface of cathodes 13b and 23b can be 120 minutes or less, and the time after the electrodeposition of metallic titanium begins at other surface positions due to the movement of the electrolysis surface is not included in the electrodeposition time at the predetermined surface position. The electrodeposition time of metallic titanium to the electrolysis surface of the cathode is preferably set to 80 minutes or less, and more preferably to 60 minutes or less.
[0079] By adjusting various conditions as described above, metallic titanium electrodeposited on cathode 3b during the electrodeposition process can be easily peeled off from cathode 3b. Peeling, as referred to here, means physically removing metallic titanium from cathode 3b without the use of leaching or similar methods.
[0080] It should be noted that, for example, even when the electrolytic surface of cathode 3b is set to 78cm... 2 In the above-mentioned case, even when large-sized foil-shaped titanium metal is deposited, the titanium metal can be well peeled off from the surface of the cathode 3b. Furthermore, sometimes even when the electrolytic surface of the cathode 3b is set to 500 cm², 2 The above also ensures good peelability.
[0081] Sometimes the surface and back areas of the titanium foil obtained by peeling from cathode 3b are 78 cm². 2 The above are further divided into 500cm. 2 The above describes the process. The average thickness of the titanium foil is preferably 10 μm to 1000 μm, more preferably 50 μm to 500 μm. To calculate the average thickness of the titanium foil, an optical microscope is used to observe a cross-section along one side of the foil at 100x magnification in the thickness direction, and the thickness at 10 points is calculated. The average value of these points is taken as the average thickness of the titanium foil. It should be noted that there is a tendency for a longer electrodeposition time to result in a thicker layer of metallic titanium on the cathode 3b.
[0082] Furthermore, as described above, titanium foil is manufactured by electrolysis to deposit metallic titanium on the cathode 3b. Therefore, the oxygen and iron content that may be present in this titanium foil is lower than that of the titanium raw materials such as the anode 3a. For example, in the titanium foil manufactured according to this embodiment, the oxygen content can be reduced to below 400 ppm by mass. The oxygen content can be determined by an inert gas dissolution method.
[0083] Example
[0084] Next, the method for manufacturing the titanium foil of the present invention was experimentally implemented, and its effectiveness was confirmed, therefore, it will be described below. However, the description herein is for illustrative purposes only and is not intended to be limiting.
[0085] use Figure 2The electrolysis apparatus shown flows current through the anode and cathode, and electrolysis is performed in a molten salt bath. The bath portion of the electrolysis apparatus is sized as 500mmΦ × 800mm in depth. The molten salt bath is configured as follows: using low-grade titanium chloride (titanium dichloride and titanium trichloride) as the titanium raw material, the molar concentration of titanium ions relative to the total molar concentration of metal ions in the molten salt bath is maintained at 6% to 10% as shown in Table 1, and the remaining portion is NaCl, KCl, and MgCl2. The anode uses JIS type 2 titanium plate (6mm thick). As for the cathode, its outermost layer is a 0.2mm thick molybdenum plate formed into a cylinder with an inner diameter (diameter) of 96mm. In Example 5, the material of the outermost surface of the cathode is changed from molybdenum to tantalum. The cathode is arranged inside the cylindrical anode in the electrolysis cell of the electrolysis apparatus. Here, the height direction of the anode and cathode is made approximately parallel to the depth direction of the molten salt bath, and the central axis of the anode and the central axis of the cathode are located at the same position. Thus, the distance between the electrodes is fixed throughout the circumference of the anode and cathode.
[0086] As shown in Table 1, the conditions were varied, and electrodeposition processes were performed on Examples 1-6 and Comparative Examples 1-4 to deposit large foil-shaped pieces of metallic titanium on the surface of the cathode. During the electrodeposition process, in Examples 1-6 and Comparative Examples 1, 2, and 4, a constant current was continuously supplied to the electrode. On the other hand, in Comparative Example 3, a pulsed current was supplied, and the current density when the pulsed current was turned on was set to 0.18 A / cm². 2 Set the on-time to 1.5 seconds, the off-time current density to 0 (no power), and the average current density to 0.09 A / cm². 2 It should be noted that the "electrodeposition time" in Comparative Example 3 is the total time from the start to the end of electrodeposition, and therefore includes the disconnection time. Furthermore, the temperature of the molten salt bath was maintained at the values shown in Table 1 during the electrodeposition process.
[0087] After the electrodeposition process, the cathode with electrodeposited metallic titanium is lifted from the molten salt bath. The metallic titanium electrodeposited on the cathode in Example 1 is... Figure 5 The appearance shown is, in Comparative Example 2, Figure 6 The appearance shown.
[0088] The titanium on the cathode was then washed with water to remove the molten salt adhering to its surface. A peel strength test, described later, was then performed. The ease of peeling at this stage is shown in Table 1.
[0089] [Table 1]
[0090]
[0091] Peelability is determined by a peel strength test, rated as "0", "△", or "×". "0" indicates a peel strength below 0.2 N / mm; "△" indicates a peel strength exceeding 0.2 N / mm but below 1.0 N / mm; and "×" indicates a peel strength exceeding 1.0 N / mm. A 0 or △ rating is considered acceptable, with 0 indicating superior performance. A × rating is considered unacceptable.
[0092] Peel strength test such as Figure 7 The procedure is as shown. First, a 70mm × 10mm sample 103 is cut and collected from the cathode and the titanium electrodeposited on the cathode using a cutter or similar tool. Next, the sample 103 is placed on the worktable 111 of a 90° peel tester, and a 10mm section of titanium 101 is peeled off from one end of the sample 103 from the cathode 102, clamping the peeled portion of titanium 101 with a chuck. Then, the cathode 102 at one end of the sample 103 on the worktable 111 and the other end of the sample 103 located on the opposite side of that end are respectively fixed using a fixing clamp 112. Then, as shown... Figure 7 As indicated by the middle arrow, the chuck is raised vertically upwards at a rate of 20 mm / sec, while the worktable 111 moves horizontally at a rate of 20 mm / sec. Based on the load measured at this time, the peel strength is calculated using the formula: Peel Strength = Average Load (N) / Width of Titanium Foil (mm). Here, the average load refers to the average value of the load acting on the chuck in the vertical direction during the 20 mm displacement of the worktable 111 from 5 mm to 25 mm in the horizontal direction. Furthermore, the width of the titanium foil refers to the width along the direction orthogonal to the direction of movement of the worktable 111. Figure 7 The width of the titanium 101 (in the direction of paper depth). It should be noted that the angle between the direction of peeling off the titanium 101 and the surface of the cathode 102 is 90° as measured from the cathode surface. As the peel testing machine, an IMADA ZTS-200N digital force gauge (measurable load: 200N) and a P90-200N slide table for 90-degree peel testing are used.
[0093] Furthermore, Table 1 shows the dendrite number density, which measures the number of dendrites per unit area. Specifically, using a scanning electron microscope (SEM), the number of dendrites present on the surface of metallic titanium on the cathode was measured in five fields of view at 50x magnification. The average number of dendrites in these five fields of view was then converted to a value per 1 cm². 2 The number of dendrites is used to determine the density (rounding to the nearest decimal place). "0" indicates a dendrite density of less than 1 dendrite / cm³. 2 "△" indicates a dendrite number density of 1 dendrite / cm². 2 More than 2 and less than 2 per cm 2"×" indicates a dendrite number density of 2 dendrites / cm². 2 That's all. A rating of ○ and △ indicates passing, while ○ indicates even better. A rating of × indicates failing.
[0094] Furthermore, in Table 1, the evaluation of titanium electrodeposition amount is based on the result of converting the thickness of titanium electrodeposited on the cathode into electrodeposition time per 60 minutes. "〇" indicates a titanium thickness of 80 μm or more per 60 minutes, "△" indicates a titanium thickness of 60 μm or more but less than 80 μm per 60 minutes, and "×" indicates a titanium thickness of less than 60 μm per 60 minutes. 〇 and △ evaluations are considered acceptable, with 〇 indicating even better performance. × evaluations are considered unacceptable.
[0095] As shown in Table 1, in Examples 1-6, metallic titanium was easily peeled off from the cathode, and the titanium was electrodeposited to a sufficiently thick thickness per unit electrodeposition time. On the other hand, in Comparative Examples 1-4, it was sometimes difficult to peel metallic titanium off from the cathode, and the thickness of the titanium electrodeposited per unit electrodeposition time was thin. Furthermore, it can be said that Examples 1-6 generally suppressed the formation of dendrites on the cathode.
[0096] Therefore, according to the present invention, it is possible to increase the amount of titanium electrodeposited per unit time without significantly reducing the ease of peeling off the titanium electrodeposited on the cathode.
[0097] Explanation of reference numerals in the attached figures
[0098] 1, 11, 21, 31: Electrolysis apparatus;
[0099] 2, 12, 22, 32: Electrolytic cells;
[0100] 3, 13, 23, 33: Electrodes;
[0101] 3a, 13a, 23a, 33a: anode;
[0102] 3b, 13b, 23b, 33b: Cathode;
[0103] 4, 34: Power supply;
[0104] 15, 25: Take-up rollers;
[0105] 26a, 26b: Rotating rollers;
[0106] 101: Titanium metal;
[0107] 102: Cathode;
[0108] 103: Sample;
[0109] 111: Workbench;
[0110] 112: Fixture;
[0111] Bf: Molten salt bath;
[0112] Ts: Titanium metal.
Claims
1. A method for manufacturing titanium foil, comprising a method for manufacturing titanium foil, include: The electrodeposition process uses a molten salt bath containing titanium ions and molten chloride. Electrolysis is performed using electrodes containing an anode and a cathode, causing metallic titanium to deposit on the electrolysis surface of the cathode. The process of physically peeling metallic titanium from the cathode in foil form; In the electrodeposition process, the molar concentration of titanium ions in the molten salt bath relative to the total molar concentration of metal ions is maintained at 7% or higher, the temperature of the molten salt bath is maintained below 510°C, the continuous interruption time of energizing the electrode is set to be less than 1.0 second, and the current density is set to 0.10 A / cm². 2 Above and 1.0 A / cm 2 Hereinafter, the electrodeposition time of metallic titanium onto the electrolytic surface of the cathode will be set to 120 minutes or less. The electrolytic surface of the cathode is 78 cm. 2 The above, and The foil-shaped titanium obtained by peeling from the cathode has a surface area of 78 cm² on both the front and back sides. 2 above.
2. The method for manufacturing titanium foil according to claim 1, wherein, The anode contains Ti. The anode is consumed during the electrodeposition process.
3. The method for manufacturing titanium foil according to claim 1 or 2, wherein, The chloride comprises titanium dichloride and / or titanium trichloride.
4. The method for manufacturing titanium foil according to claim 1 or 2, wherein, In the electrodeposition process, the molar concentration of titanium ions in the molten salt bath is maintained at a ratio of more than 10% to the total molar concentration of metal ions.
5. The method for manufacturing titanium foil according to claim 1 or 2, wherein, In the electrodeposition process, the temperature of the molten salt bath is maintained below 500°C.
6. The method for manufacturing titanium foil according to claim 1 or 2, wherein, In the electrodeposition process, the current density is set to 0.20 A / cm. 2 Above and 0.50A / cm 2 the following.
7. The method for manufacturing titanium foil according to claim 1 or 2, wherein, The molten salt bath does not contain fluoride ions.
8. The method for manufacturing titanium foil according to claim 1 or 2, wherein, The surfaces of the anode and the opposite cathode have similar shapes.
9. The method for manufacturing titanium foil according to claim 1 or 2, wherein, The distance between the anode and the cathode is set to be more than 0.5 cm and less than 10.0 cm.
10. The method for manufacturing titanium foil according to claim 1 or 2, wherein, The surface and back surfaces of the titanium foil have areas of 500 cm². 2 above.
11. The method for manufacturing titanium foil according to claim 1 or 2, wherein, The average thickness of the titanium foil is in the range of 10 μm to 1000 μm.
Citation Information
Patent Citations
Production of high purity titanium
JP1991291391A
Production of titanium
JP2000087280A
Method for producing metal titanium
WO2020044841A1
Electrodeposition method
US3662047A