Preparation method of low-cost LED chip and LED chip

By bonding epitaxial wafers onto a substrate and using laser to decompose the buffer layer, the problem of substrate thickness loss was solved, enabling the recycling of epitaxial substrates and reducing the production cost of LED chips.

CN116759495BActive Publication Date: 2026-11-20JIANGXI ZHAO CHI SEMICON CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310895165.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-20
Publication Date
2026-11-20
Estimated Expiration
2043-07-20

AI Technical Summary

Technical Problem

Existing technologies cannot effectively reduce the production cost of LED chips, mainly because the substrate thickness is ground away in the later stages of manufacturing, resulting in the loss of raw materials and making it impossible to directly use substrates with a thickness of 80-200μm.

Method used

By bonding the epitaxial wafer to a substrate of a predetermined thickness and using a laser spot to decompose the buffer layer between the epitaxial layer and the epitaxial substrate, the epitaxial substrate and the epitaxial layer are separated. The substrate after peeling can be reused, avoiding the chip thickness reduction process.

Benefits of technology

This enables the recycling of epitaxial substrates, reduces the loss of substrate raw materials, and effectively reduces the production cost of LED chips.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116759495B_ABST
    Figure CN116759495B_ABST
Patent Text Reader

Abstract

The application discloses a preparation method of a low-cost LED chip and the LED chip, and relates to the technical field of semiconductor manufacturing. The preparation method comprises the following steps: bonding an epitaxial wafer obtained through a previous process to a substrate with a preset thickness, so that an epitaxial layer of the epitaxial wafer is bonded and connected with the substrate; the substrate is transparent glass or is made of other transparent materials resistant to high temperature; controlling a laser spot to irradiate the epitaxial wafer, decomposing a buffer layer between the epitaxial layer and an epitaxial substrate, so that the epitaxial substrate is separated from the epitaxial layer and falls off; and manufacturing a chip structure on the epitaxial layer of the substrate to obtain the LED chip. In the process of manufacturing the LED chip, the peeled-off substrate can be recycled, on the one hand, the chip post-thinning and grinding process is removed, and on the other hand, the substrate can be recycled, the loss of substrate raw materials is reduced, and therefore, the production cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of semiconductor manufacturing technology, specifically to a method for preparing a low-cost LED chip and the LED chip itself. Background Technology

[0002] LED chips are light-emitting semiconductor electronic components characterized by their small size, high brightness, and low power consumption, and are widely used in lighting and other fields. LED chips are obtained by splitting LED epitaxial wafers. An LED epitaxial wafer includes a substrate and a GaN epitaxial layer grown on the substrate.

[0003] With the continued large-scale mass production of LED chips, cost has become a crucial production metric. The traditional process flow currently involves four main stages: wafer fabrication, PSS (Pressurized Substrate System), epitaxy, and chip fabrication. The final chip thickness is typically 80-200μm. Current mainstream substrates are 2-inch, 4-inch, and 6-inch. A 2-inch substrate is approximately 430μm thick, a 4-inch substrate is approximately 650μm thick, and a 6-inch substrate is approximately 1300μm thick. This results in a 400-1000μm thickness being ground away at the back end of chip fabrication, leading to material loss and increased production costs.

[0004] If the substrate thickness were directly made to 80-200μm at the source, the chip production cost could be significantly reduced. However, if an 80-200μm thick substrate is used directly, problems such as wafer breakage and epitaxial growth failures will occur from the substrate to the epitaxial layer and then to the chip. Existing technologies cannot solve these problems, thus the current solution is not feasible. This invention aims to provide a new process method that can solve this problem, thereby significantly reducing the overall manufacturing cost of LED chips. Summary of the Invention

[0005] In view of the shortcomings of the prior art, the purpose of this invention is to provide a low-cost LED chip manufacturing method and LED chip. In the process of manufacturing LED chips, the substrate stripped off can be reused repeatedly. On the one hand, this eliminates the need for the subsequent chip thinning and polishing process, and on the other hand, it allows the substrate to be recycled, reducing the loss of substrate raw materials and thus reducing production costs.

[0006] One aspect of the present invention is to provide a method for fabricating a low-cost LED chip, the method comprising: The epitaxial wafer obtained from the previous process is bonded to a substrate of a predetermined thickness, so that the epitaxial layer of the epitaxial wafer is bonded to the substrate; wherein, the substrate is transparent glass or made of other high-temperature resistant transparent materials. The laser spot is controlled to irradiate the epitaxial wafer, decomposing the buffer layer between the epitaxial layer and the epitaxial substrate, so that the epitaxial substrate is separated from the epitaxial layer and falls off; A chip structure is fabricated on the epitaxial layer of the substrate to obtain an LED chip.

[0007] According to one aspect of the above technical solution, in the method, the front-end process of the epitaxial wafer includes: An epitaxial substrate is flattened; The epitaxial substrate is etched and patterned to obtain a patterned substrate; The patterned substrate is coated using a physical vapor deposition process to obtain an AlN film layer on the surface of the patterned substrate. An epitaxial layer is fabricated on the patterned substrate using a metal-organic chemical vapor deposition process to obtain an epitaxial wafer.

[0008] According to one aspect of the above technical solution, the step of flattening an epitaxial substrate specifically includes: A predetermined epitaxial substrate is subjected to cutting, edge grinding, and polishing processes to obtain the epitaxial substrate that meets the usage requirements. The epitaxial substrate is a double-polished substrate.

[0009] According to one aspect of the above technical solution, the step of bonding the epitaxial wafer obtained through the previous process to a substrate of a predetermined thickness, so that the epitaxial layer of the epitaxial wafer is bonded to the substrate, specifically includes: A first bonding medium and a second bonding medium are respectively coated on the surface of the epitaxial layer of the epitaxial wafer and the surface of the substrate; Under high temperature and high pressure conditions, the first bonding medium and the second bonding medium between the epitaxial layer and the substrate are bonded to obtain a bonding layer, so that the epitaxial wafer is bonded to the substrate through the bonding layer.

[0010] According to one aspect of the above technical solution, the bonding temperature under the high temperature and high pressure conditions is 500℃-600℃.

[0011] According to one aspect of the above technical solution, the bonding pressure under the high temperature and high pressure conditions is 12000kg-15000kg.

[0012] According to one aspect of the above technical solution, a buffer layer is provided between the epitaxial layer and the epitaxial substrate, the buffer layer is an AlN buffer layer, and the thickness of the AlN buffer layer is 150nm-300nm.

[0013] According to one aspect of the above technical solution, the step of controlling the laser spot to irradiate the epitaxial wafer and decompose the buffer layer between the epitaxial layer and the epitaxial substrate, so as to separate and detach the epitaxial substrate from the epitaxial layer, specifically includes: The laser source is controlled to emit a laser spot, and the laser spot is controlled to move according to a preset rule so that the laser spot irradiates the epitaxial wafer; Based on the laser energy generated by the laser spot, the AlN buffer layer between the epitaxial layer and the epitaxial substrate is burned to achieve complete or partial decomposition, thereby separating and detaching the epitaxial substrate from the epitaxial layer.

[0014] According to one aspect of the above technical solution, the laser is a continuous laser or a pulsed laser, the diameter of the laser spot is 1nm-3mm, and the energy of a single pulse laser is 50mJ-60mJ.

[0015] A second aspect of the present invention is to provide a low-cost LED chip, wherein the LED chip is prepared by the preparation method described in the above technical solution.

[0016] Compared with existing technologies, the advantages of using the low-cost LED chip fabrication method and LED chip shown in this invention are as follows: By bonding the epitaxial wafer obtained in the previous process to a substrate of a predetermined thickness, the epitaxial layer of the epitaxial wafer is bonded to the substrate. Then, the epitaxial wafer is irradiated with a laser spot to decompose the buffer layer between the epitaxial layer and the epitaxial substrate, causing the epitaxial substrate to separate and detach from the epitaxial layer. The chip structure can then be fabricated on the epitaxial layer of the substrate to obtain an LED chip. Furthermore, the epitaxial substrate detached from the substrate can be reused. On the one hand, the chip thickness reduction process is eliminated, and on the other hand, the epitaxial substrate can be recycled, reducing damage to the substrate raw materials, thus effectively reducing the production cost of LED chips. Attached Figure Description

[0017] The above and / or additional aspects and advantages of the present invention will become apparent and readily understood from the description of the embodiments taken in conjunction with the following drawings, in which: Figure 1 This is a schematic flowchart illustrating a method for fabricating a low-cost LED chip according to an embodiment of the present invention. Detailed Implementation

[0018] To make the objectives, features, and advantages of the present invention more apparent and understandable, specific embodiments of the present invention will be described in detail below with reference to the accompanying drawings. Several embodiments of the present invention are shown in the drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. Rather, these embodiments are provided so that the disclosure of the present invention will be more thorough and complete.

[0019] It should be noted that when a component is said to be "fixed to" another component, it can be directly on the other component or there may be an intervening component. When a component is said to be "connected to" another component, it can be directly connected to the other component or there may be an intervening component. The terms "vertical," "horizontal," "left," "right," and similar expressions used in this document are for illustrative purposes only.

[0020] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein in the description of the invention is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.

[0021] Please see Figure 1 One aspect of the present invention is to provide a method for fabricating a low-cost LED chip, the method comprising steps S10-S30: Step S10: The epitaxial wafer obtained from the previous process is bonded to a substrate of a predetermined thickness, so that the epitaxial layer of the epitaxial wafer is bonded to the substrate; wherein, the substrate is transparent glass or made of other high-temperature resistant transparent materials. Step S20: Control the laser spot to irradiate the epitaxial wafer, decompose the buffer layer between the epitaxial layer and the epitaxial substrate, so that the epitaxial substrate is separated from the epitaxial layer and falls off. Step S30: A chip structure is fabricated on the epitaxial layer of the substrate to obtain an LED chip.

[0022] Furthermore, the front-end processes for the epitaxial wafer include: An epitaxial substrate is flattened; The epitaxial substrate is etched and patterned to obtain a patterned substrate; The patterned substrate is coated using a physical vapor deposition process to obtain an AlN film layer on the surface of the patterned substrate. An epitaxial layer is fabricated on the patterned substrate using a metal-organic chemical vapor deposition process to obtain an epitaxial wafer.

[0023] Furthermore, the step of planarizing an epitaxial substrate specifically includes: A predetermined epitaxial substrate is subjected to cutting, edge grinding, and polishing processes to obtain the epitaxial substrate that meets the usage requirements. The epitaxial substrate is a double-polished substrate.

[0024] According to one aspect of the above technical solution, the step of bonding the epitaxial wafer obtained through the previous process to a substrate of a predetermined thickness, so that the epitaxial layer of the epitaxial wafer is bonded to the substrate, specifically includes: A first bonding medium and a second bonding medium are respectively coated on the surface of the epitaxial layer of the epitaxial wafer and the surface of the substrate; Under high temperature and high pressure conditions, the first bonding medium and the second bonding medium between the epitaxial layer and the substrate are bonded to obtain a bonding layer, so that the epitaxial wafer is bonded to the substrate through the bonding layer.

[0025] Furthermore, the bonding temperature under the high temperature and high pressure conditions is 500℃-600℃.

[0026] Furthermore, the bonding pressure under the high temperature and high pressure conditions is 12000kg-15000kg.

[0027] 500℃-600℃ 12000kg-15000kg Furthermore, a buffer layer is provided between the epitaxial layer and the epitaxial substrate, the buffer layer being an AlN buffer layer with a thickness of 150nm-300nm.

[0028] Furthermore, the step of controlling the laser spot to irradiate the epitaxial wafer and decompose the buffer layer between the epitaxial layer and the epitaxial substrate, so as to separate and detach the epitaxial substrate from the epitaxial layer, specifically includes: The laser source is controlled to emit a laser spot, and the laser spot is controlled to move according to a preset rule so that the laser spot irradiates the epitaxial wafer; Based on the laser energy generated by the laser spot, the AlN buffer layer between the epitaxial layer and the epitaxial substrate is burned to achieve complete or partial decomposition, thereby separating and detaching the epitaxial substrate from the epitaxial layer.

[0029] Furthermore, the laser is a continuous laser or a pulsed laser, the diameter of the laser spot is 1nm-3mm, and the energy of a single pulse laser is 50mJ-60mJ.

[0030] A second aspect of the present invention is to provide a low-cost LED chip, wherein the LED chip is prepared by the preparation method described in the above technical solution.

[0031] Compared with existing technologies, the advantages of using the low-cost LED chip fabrication method and LED chip shown in this invention are as follows: By bonding the epitaxial wafer obtained in the previous process to a substrate of a predetermined thickness, the epitaxial layer of the epitaxial wafer is bonded to the substrate. Then, the epitaxial wafer is irradiated with a laser spot to decompose the buffer layer between the epitaxial layer and the epitaxial substrate, causing the epitaxial substrate to separate and detach from the epitaxial layer. The chip structure can then be fabricated on the epitaxial layer of the substrate to obtain an LED chip. Furthermore, the epitaxial substrate peeled off from the substrate can be reused. On the one hand, this eliminates the need for a chip thickness reduction process, and on the other hand, it allows the epitaxial substrate to be reused during the LED chip manufacturing process, effectively reducing damage to the substrate raw materials and thus lowering the overall production cost of LED chips.

[0032] Example 1 Please refer to it again. Figure 1 The first embodiment of the present invention provides a method for fabricating a low-cost LED chip. The method is used to fabricate an LED chip, which includes an epitaxial substrate and an epitaxial wafer. The fabrication method shown in this embodiment aims to achieve the recycling of the epitaxial substrate to reduce substrate loss during the LED chip fabrication process, thereby reducing the production cost of the LED chip.

[0033] In this embodiment, the preparation method includes steps S10-S30: Step S10: The epitaxial wafer obtained from the previous process is bonded to a substrate of a predetermined thickness, so that the epitaxial layer of the epitaxial wafer is bonded to the substrate; wherein the substrate is transparent glass or made of other high-temperature resistant transparent materials.

[0034] In this embodiment, the front-end process of the epitaxial wafer includes: An epitaxial substrate is flattened; The epitaxial substrate is etched and patterned to obtain a patterned substrate; The patterned substrate is coated using a physical vapor deposition process to obtain an AlN film layer on the surface of the patterned substrate. An epitaxial layer is fabricated on the patterned substrate using a metal-organic chemical vapor deposition process to obtain an epitaxial wafer.

[0035] The step of flattening an epitaxial substrate specifically includes: A predetermined epitaxial substrate is subjected to cutting, edge grinding, and polishing processes to obtain the epitaxial substrate that meets the usage requirements. More specifically, the epitaxial substrate is a double-polished substrate, which means that both sides of the substrate are polished. Polishing the two sides separately is used to control the thickness of the epitaxial substrate.

[0036] In this embodiment, the epitaxial wafer obtained by the front-end process includes an epitaxial substrate and an epitaxial layer. The epitaxial layer includes an N-type semiconductor layer, a quantum well layer and a P-type semiconductor layer. The front-end process of the epitaxial wafer includes wafer flattening and PSS processing. The wafer flattening includes cutting, grinding and polishing the epitaxial substrate, and the PSS processing is an etching patterning process.

[0037] By bonding an epitaxial wafer to a substrate of a predetermined thickness, which is actually a thin substrate, such as transparent glass, sapphire substrate or other transparent materials, a bonding medium is coated between the epitaxial layer of the epitaxial wafer and the substrate, and the bonding medium is cured under predetermined conditions, so that the epitaxial wafer and the substrate are bonded together to form a whole.

[0038] In this embodiment, the step of bonding the epitaxial wafer obtained from the previous process to a substrate of a predetermined thickness, thereby bonding the epitaxial layer of the epitaxial wafer to the substrate, specifically includes steps S11-S12: Step S11: Coat the surface of the epitaxial layer of the epitaxial wafer and the surface of the substrate with a first bonding medium and a second bonding medium, respectively.

[0039] The first bonding medium and the second bonding medium are made of the same material, such as Al2O3 bonding material. Before the bonding step is performed, the first bonding medium is coated on the surface of the epitaxial layer and the second bonding medium is coated on the surface of the substrate. The epitaxial layer of the epitaxial wafer is placed opposite the substrate so that the first bonding medium and the second bonding medium are in contact.

[0040] Step S12: Under high temperature and high pressure conditions, the first bonding medium between the epitaxial layer and the substrate is bonded to the second bonding medium to obtain a bonding layer, so that the epitaxial wafer is bonded to the substrate through the bonding layer.

[0041] Specifically, the bonding equipment is controlled to operate so that the internal bonding temperature and bonding pressure meet the high temperature and high pressure bonding conditions set in this embodiment. When the bonding temperature and bonding pressure in the bonding equipment meet the bonding conditions, the first bonding medium and the second bonding medium between the epitaxial layer and the substrate fuse with each other under the action of high temperature and high pressure to achieve the bonding connection between the first bonding medium and the second bonding medium, thereby obtaining a bonding layer to bond the epitaxial layer and the substrate to form an integral structure.

[0042] In this embodiment, the bonding temperature in the temperature conditions is 550°C, and the bonding pressure in the pressure conditions is 12000 kg.

[0043] Step S20: Control the laser spot to irradiate the epitaxial wafer, decompose the buffer layer between the epitaxial layer and the epitaxial substrate, so that the epitaxial substrate is separated from the epitaxial layer and falls off.

[0044] A buffer layer is provided between the epitaxial layer and the epitaxial substrate. The buffer layer is an AlN buffer layer with a thickness of 150nm-300nm.

[0045] In this embodiment, the laser spot is a UV laser spot with strong laser energy, typically 50mJ-60mJ. When the laser spot irradiates the epitaxial wafer, the buffer layer between the epitaxial layer and the epitaxial substrate is decomposed by the laser, causing the buffer layer between the epitaxial layer and the epitaxial substrate to be completely or partially decomposed, forming a gap between the epitaxial layer and the epitaxial substrate, thereby separating the epitaxial substrate from the epitaxial layer and detaching the epitaxial substrate.

[0046] In this embodiment, the epitaxial substrate is a patterned substrate that has been cut, edged, polished and PSS treated. The epitaxial substrate peeled off from the epitaxial wafer can be reused repeatedly. On the one hand, it eliminates the need for the chip's back-end thinning and polishing process, and on the other hand, it allows the substrate to be recycled, reducing the loss of substrate raw materials and thus reducing the production cost of LED chips.

[0047] In this embodiment, the step of controlling the laser spot to irradiate the epitaxial wafer and decompose the buffer layer between the epitaxial layer and the epitaxial substrate, so that the epitaxial substrate and the epitaxial layer are separated and detached, specifically includes steps S31-S32: Step S31: Control the laser source to irradiate a laser spot, and control the laser spot to move according to a preset rule so that the laser spot irradiates the epitaxial wafer; Step S32: Based on the laser energy generated by the laser spot, the AlN buffer layer between the epitaxial layer and the epitaxial substrate is burned to achieve complete or partial decomposition, thereby separating the epitaxial substrate from the epitaxial layer and causing it to fall off.

[0048] The laser is a continuous laser or a pulsed laser, the diameter of the laser spot is 1nm-3mm, and the energy of a single pulse laser is 50mJ-60mJ.

[0049] Step S30: A chip structure is fabricated on the epitaxial layer of the substrate to obtain an LED chip.

[0050] Specifically, a chip structure is fabricated on an epitaxial layer on a substrate, including the fabrication of a conductive layer, an electron blocking layer, and an electrode structure. The conductive layer is a transparent conductive layer, and the electrode structure includes N-type electrodes and P-type electrodes.

[0051] In summary, by bonding the epitaxial wafer to the substrate, and then using laser lift-off technology to remove the epitaxial substrate from the epitaxial wafer, the epitaxial substrate can be recycled in the later LED chip manufacturing process, thereby reducing the manufacturing cost of LED chips.

[0052] The LED chip prepared by the method shown in this embodiment includes an LED epitaxial wafer and a chip structure. The LED epitaxial wafer includes an epitaxial substrate and an epitaxial layer.

[0053] Compared with existing technologies, the advantages of using the low-cost LED chip fabrication method shown in this embodiment are as follows: By bonding the epitaxial wafer obtained in the previous process to a substrate of a predetermined thickness, the epitaxial layer of the epitaxial wafer is bonded to the substrate. Then, the epitaxial wafer is irradiated with a laser spot to decompose the buffer layer between the epitaxial layer and the epitaxial substrate, causing the epitaxial substrate to separate and detach from the epitaxial layer. The chip structure can then be fabricated on the epitaxial layer of the substrate to obtain an LED chip. Furthermore, the epitaxial substrate peeled off from the substrate can be reused. On the one hand, this eliminates the need for a chip thickness reduction process, and on the other hand, it allows the epitaxial substrate to be reused during the LED chip manufacturing process, effectively reducing damage to the substrate raw materials and thus lowering the overall production cost of LED chips.

[0054] Example 2 The third embodiment of the present invention also provides a method for fabricating a low-cost LED chip. The fabrication method shown in this embodiment is the same as that in the first embodiment, except that: In this embodiment, the bonding temperature is 600°C and the bonding pressure is 12000 kg.

[0055] Example 3 The third embodiment of the present invention also provides a method for fabricating a low-cost LED chip. The fabrication method shown in this embodiment is the same as that in the first embodiment, except that: In this embodiment, the bonding temperature is 600°C and the bonding pressure is 13000 kg.

[0056] Example 4 The fourth embodiment of the present invention also provides a method for fabricating a low-cost LED chip. The fabrication method shown in this embodiment is the same as that in the first embodiment, except that: In this embodiment, the bonding temperature is 600°C and the bonding pressure is 14000 kg.

[0057] Example 5 The fourth embodiment of the present invention also provides a method for fabricating a low-cost LED chip. The fabrication method shown in this embodiment is the same as that in the first embodiment, except that: In this embodiment, the bonding temperature is 600°C and the bonding pressure is 15000 kg.

[0058] Comparative Example 1 The first comparative example of the present invention also provides a method for fabricating a low-cost LED chip. The fabrication method shown in this comparative example is the same as that in the first embodiment, except that: In this comparative example, the bonding temperature is 500℃ and the bonding pressure is 12000kg.

[0059] Comparative Example 2 The second comparative example of the present invention also provides a method for fabricating a low-cost LED chip. The fabrication method shown in this comparative example is the same as that in the first embodiment, except that: In this comparative example, the bonding temperature was 650℃ and the bonding pressure was 12000kg.

[0060] Comparative Example 3 The third comparative example of the present invention also provides a method for fabricating a low-cost LED chip. The fabrication method shown in this comparative example is the same as that in the first embodiment, except that: In this comparative example, the bonding temperature is 600℃ and the bonding pressure is 16000kg.

[0061] Table 1 is a parameter comparison table of the first to fifth embodiments of the present invention and the first to third comparative examples in the LED chip manufacturing process.

[0062] Table 1 According to Table 1, and in conjunction with the first and second embodiments, it can be seen that when the bonding pressure between the epitaxial layer and the substrate is the same, but the bonding temperature is different, the higher the bonding temperature, the higher the performance of the LED chip in all aspects.

[0063] According to Table 1, and in conjunction with the third to fifth embodiments, when the bonding temperature of the epitaxial layer and the substrate is the same, but the bonding pressure is different, the higher the bonding pressure, the higher the performance of the LED chip in all aspects.

[0064] According to Table 1, and in conjunction with the first comparative example, the second embodiment, and the first and second comparative examples, it can be seen that when the bonding pressure between the epitaxial layer and the substrate is the same, but the bonding temperature is different, the bonding temperature being too high or too low leads to a decline in the performance of various aspects of the LED chip.

[0065] According to Table 1, combined with the second to fifth embodiments and the third comparative example, when the bonding temperature of the epitaxial layer and the substrate are the same, and the bonding pressure is too high, the performance of the LED chip in various aspects will decline.

[0066] In summary, when the epitaxial layer and the substrate are bonded as described in this invention, the LED chip achieves optimal performance in all aspects when the bonding temperature is controlled at 500℃-600℃ and the bonding pressure is controlled at 12000kg-15000kg.

[0067] In the description of this specification, references to terms such as "one embodiment," "some embodiments," "example," "specific example," or "some examples," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.

[0068] The embodiments described above are merely illustrative of several implementations of the present invention, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the present invention. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these all fall within the protection scope of the present invention. Therefore, the protection scope of this patent should be determined by the appended claims.

Claims

1. A method for fabricating a low-cost LED chip, characterized in that, The preparation method includes: The epitaxial wafer obtained from the previous process is bonded to a substrate of a predetermined thickness, so that the epitaxial layer of the epitaxial wafer is bonded to the substrate; wherein, the substrate is transparent glass or made of other high-temperature resistant transparent materials. The laser spot is controlled to irradiate the epitaxial wafer, decomposing the buffer layer between the epitaxial layer and the epitaxial substrate, so that the epitaxial substrate is separated from the epitaxial layer and falls off; A chip structure is fabricated on the epitaxial layer of the substrate to obtain an LED chip; In the method, the front-end process of the epitaxial wafer includes: An epitaxial substrate is flattened; The epitaxial substrate is etched and patterned to obtain a patterned substrate; The patterned substrate is coated using a physical vapor deposition process to obtain an AlN film layer on the surface of the patterned substrate. An epitaxial layer is fabricated on the patterned substrate using a metal-organic chemical vapor deposition process to obtain an epitaxial wafer; The step of bonding the epitaxial wafer obtained from the previous process to a substrate of a predetermined thickness, thereby bonding the epitaxial layer of the epitaxial wafer to the substrate, specifically includes: A first bonding medium and a second bonding medium are respectively coated on the surface of the epitaxial layer of the epitaxial wafer and the surface of the substrate; Under high temperature and high pressure conditions, the first bonding medium and the second bonding medium between the epitaxial layer and the substrate are bonded to obtain a bonding layer, so that the epitaxial wafer is bonded to the substrate through the bonding layer.

2. The method for preparing a low-cost LED chip according to claim 1, characterized in that, The step of planarizing an epitaxial substrate specifically includes: A predetermined epitaxial substrate is subjected to cutting, edge grinding, and polishing processes to obtain the epitaxial substrate that meets the usage requirements. The epitaxial substrate is a double-polished substrate.

3. The method for preparing a low-cost LED chip according to claim 1, characterized in that, The bonding temperature under the high temperature and high pressure conditions is 500℃-600℃.

4. The method for preparing a low-cost LED chip according to claim 1, characterized in that, The bonding pressure under the high temperature and high pressure conditions is 12000kg-15000kg.

5. The method for preparing a low-cost LED chip according to any one of claims 1-4, characterized in that, A buffer layer is provided between the epitaxial layer and the epitaxial substrate. The buffer layer is an AlN buffer layer with a thickness of 150nm-300nm.

6. The method for preparing a low-cost LED chip according to claim 5, characterized in that, The step of controlling the laser spot to irradiate the epitaxial wafer and decompose the buffer layer between the epitaxial layer and the epitaxial substrate, so as to separate and detach the epitaxial substrate from the epitaxial layer, specifically includes: The laser source is controlled to emit a laser spot, and the laser spot is controlled to move according to a preset rule so that the laser spot irradiates the epitaxial wafer; Based on the laser energy generated by the laser spot, the AlN buffer layer between the epitaxial layer and the epitaxial substrate is burned to achieve complete or partial decomposition, thereby separating and detaching the epitaxial substrate from the epitaxial layer.

7. The method for preparing a low-cost LED chip according to claim 6, characterized in that, The laser is a continuous laser or a pulsed laser, with a single pulse laser energy of 50mJ-60mJ.

8. A low-cost LED chip, characterized in that, The LED chip is prepared by the preparation method described in any one of claims 1-7.

Citation Information

Patent Citations

  • Manufacturing method of semiconductor chip

    CN104409583A

  • Supporting substrates for semiconductor light emitting device and high-performance vertical structured semiconductor light emitting devices using supporting substrates

    KR1020090125676A