A V3Se4 / SnSe composite material, its preparation method and application

By introducing SnSe into V₃Se₄ to construct a heterostructure, V₃Se₄/SnSe composite material was prepared, which solved the problem of insufficient rate performance and cycle life of vanadium-based selenides in sodium-ion batteries, and achieved high specific capacity and fast charge and discharge effects.

CN116768165BActive Publication Date: 2026-11-24ZHEJIANG SCI-TECH UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310723971.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-19
Publication Date
2026-11-24
Estimated Expiration
2043-06-19

AI Technical Summary

Technical Problem

Existing vanadium-based selenides exhibit poor rate performance and cycle life in sodium-ion batteries, which cannot be significantly improved through traditional modification methods.

Method used

By introducing SnSe into V₃Se₄ to construct heterostructures, V₃Se₄/SnSe composites are prepared to improve electron mobility and reaction kinetics.

Benefits of technology

It improves the specific capacity and cycle stability of sodium-ion battery anode materials, exhibiting good rate performance and long cycle life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116768165B_ABST
    Figure CN116768165B_ABST
Patent Text Reader

Abstract

This invention provides a V3Se4 / SnSe composite material, its preparation method, and its applications, relating to the field of next-generation energy materials. The method includes: mixing vanadium chloride, tin chloride pentahydrate, glycerol, isopropanol, and hexadecyltrimethylammonium bromide to obtain a mixed solution; subjecting the mixed solution to a solvothermal reaction to obtain a reaction product; washing and drying the reaction product to obtain a V3O4 / SnO precursor; and mixing the V3O4 / SnO precursor with selenium powder and then performing a selenization reaction to obtain the V3Se4 / SnSe composite material. This invention introduces SnSe into V3Se4 to construct a heterostructure, improving the electron mobility of the anode material, thereby enhancing conductivity and reaction kinetics. The prepared V3Se4 / SnSe anode material has high specific capacity, good rate performance, and cycle stability, making it particularly suitable for manufacturing sodium-ion battery anodes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of next-generation energy materials, and in particular to a V3Se4 / SnSe composite material, its preparation method, and its application. Background Technology

[0002] To address global climate change, the development of clean energy is essential. However, common renewable and clean energy sources (such as solar, wind, tidal, biomass, and geothermal energy) are often not constant but intermittent, and are difficult to predict and control, significantly hindering their large-scale application. Therefore, storage and conversion technologies that enable cross-regional energy distribution and efficient utilization of renewable energy play a crucial role. Among these, electrochemical energy storage, due to its short construction cycle and small size, is well-suited for use in various locations and is thus considered a highly efficient energy storage technology. This necessitates the development of secondary batteries suitable for large-scale energy storage.

[0003] In electrochemical energy storage systems, lithium-ion batteries (LIBs) are currently the most widely used. Since their successful commercialization in the 1990s, they have made significant contributions to transportation electrification and the development of 3C products (computers, communications, and consumer electronics). However, lithium reserves are very limited and unevenly distributed, enough to manufacture only 1.5 billion vehicles, which greatly hinders the large-scale application of LIBs. With the increasing demand for energy storage and the growing scarcity of lithium resources, sodium-ion batteries (SIBs) are showing strong competitiveness in the energy storage field due to their abundant and widely distributed sodium reserves, the ability to reduce battery costs by 30%–40%, and higher safety. Furthermore, SIB production lines have good compatibility and are easy to scale up production.

[0004] Among SIB anodes, converted metal selenides (MSex, M = V, Mo, Fe, Co, etc.) have recently attracted widespread attention due to their inherent multi-electron transfer properties, resulting in high theoretical specific capacity and making them promising anode materials for SIBs. However, the poor rate capacity and short cycle life of MSex hinder their practical application in SIBs.

[0005] To address the aforementioned issues, researchers have undertaken a series of modifications to convertible metal selenide materials. For example, surface engineering modification can adjust the physicochemical state of the material surface, improving structural stability and conductivity, and is an effective method for enhancing the electrochemical performance of active materials. Nanostructure design can regulate the microstructural evolution of the material during charge and discharge, effectively reducing volume changes and increasing cycle capacity. While these methods increase material structural stability and conductivity to some extent, they cannot alter the intrinsic properties of the material, thus failing to significantly improve the rate performance and sodium storage capacity of the battery. Therefore, we introduced SnSe into V3Se4 to construct a heterostructure, which effectively improves its intrinsic electron migration rate and enhances reaction kinetics, thereby effectively improving its rate performance and sodium storage capacity. In the field of battery anode material preparation, Chinese patent (CN110190255B) "A nitrogen-sulfur co-doped VSe-(2) / CNF potassium ion battery anode material and its preparation method" uses pig hair, cow hair, wool, poultry feathers or human hair fibers as the main raw materials to extract keratin, and uses it as the main source of nitrogen and sulfur to dope into PAN / VO(acac)-(2) composite material. The nitrogen-sulfur co-doped VSe-(2) / CNF potassium ion battery anode material is obtained by spinning and selenization. Chinese patent (CN115663143A) "Preparation method of V-xSe-y / multi-walled carbon nanotube composite material and its application" uses a simple and quick one-step solid-state method to mix vanadium source, selenium source and multi-walled carbon nanotubes and then directly calcinate and selenize at high temperature to obtain carbon composite sodium ion battery anode material with high rate and long cycle. Based on current research, there is no evidence of using SnSe introduced into V3Se4 to construct heterostructures and use them as anode materials for sodium-ion batteries, thereby improving the poor rate performance and short cycle life of vanadium-based selenides in sodium-ion batteries. Summary of the Invention

[0006] To address the aforementioned issues, this invention provides a V3Se4 / SnSe composite material, its preparation method, and its applications. The preparation method is simple, convenient, and low-cost. The V3Se4 / SnSe composite material is low-cost and exhibits excellent performance. When used to prepare sodium-ion batteries, the V3Se4 / SnSe composite material results in high specific capacity, fast charge / discharge speed, and long cycle life.

[0007] To achieve the above objectives, the present invention provides the following technical solution:

[0008] This invention provides a method for preparing V3Se4 / SnSe composite material, comprising the following steps:

[0009] 1) Vanadium chloride, tin chloride pentahydrate, glycerol, isopropanol and hexadecyltrimethylammonium bromide are mixed to obtain a mixture;

[0010] 2) The mixture obtained in step 1) is subjected to a solvothermal reaction to obtain a reaction product. The reaction product is washed and dried to obtain the V3O4 / SnO precursor.

[0011] 3) The V3O4 / SnO precursor obtained in step 2) is mixed with selenium powder and then subjected to a selenization reaction to obtain V3Se4 / SnSe composite material.

[0012] Preferably, in step 1), the molar ratio of vanadium chloride, tin chloride pentahydrate, glycerol, isopropanol, and hexadecyltrimethylammonium bromide is 1 mmol: 1-4 mmol: 6-10 ml: 20-30 ml: 1.5-2.5 mmol.

[0013] Preferably, the mixing method in step 1) includes stirring, and the stirring time is 150-210 min.

[0014] Preferably, the conditions for the solvothermal reaction in step 2) include: a temperature of 160–200°C and a time of 6–18 h.

[0015] Preferably, the reagent used for washing in step 2) includes ethanol;

[0016] The drying conditions include a temperature of 60–80°C and a time of 12 hours.

[0017] Preferably, in step 3), the mass ratio of the V3O4 / SnO precursor to selenium powder is 1:4 to 15.

[0018] Preferably, the conditions for the selenization reaction in step 3) include: a temperature of 350–600°C and a time of 2 hours;

[0019] The selenization reaction is carried out in a nitrogen atmosphere.

[0020] The present invention also provides a V3Se4 / SnSe composite material prepared by the preparation method described in the above technical solution.

[0021] This invention also provides the application of the V3Se4 / SnSe composite material described in the above technical solution in the preparation of sodium-ion batteries.

[0022] Preferably, the components of the sodium-ion battery include the V3Se4 / SnSe composite material, Ketjen Black, and polydifluoroethylene;

[0023] The mass ratio of the V3Se4 / SnSe composite material, Ketjen black, and polydifluoroethylene is 7:2:1.

[0024] The beneficial effects of this invention are as follows:

[0025] This invention introduces SnSe into V3Se4 to construct a heterostructure, which improves the electron mobility of the anode material, thereby enhancing conductivity and reaction kinetics. The resulting V3Se4 / SnSe anode material has high specific capacity, good rate performance and cycle stability, and is particularly suitable for manufacturing anodes for sodium-ion batteries. Attached Figure Description

[0026] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the accompanying drawings used in the embodiments will be briefly described below.

[0027] Figure 1 Field emission scanning electron microscope (SEM) image of the V3O4 / SnO precursor prepared in Example 1.

[0028] Figure 2 The image shows a field emission scanning electron microscope (SEM) image of the hierarchical structure of the V3Se4 / SnSe heterojunction prepared in Example 1.

[0029] Figure 3 The V3Se4 / SnSe heterojunction hierarchical electrode material prepared in Example 1 was used as a negative electrode material for a sodium-ion battery in 4Ag -1 Long-cycle performance diagram at current density for 1800 cycles. Detailed Implementation

[0030] This invention provides a method for preparing V3Se4 / SnSe composite material, comprising the following steps:

[0031] 1) Vanadium chloride, tin chloride pentahydrate, glycerol, isopropanol and hexadecyltrimethylammonium bromide are mixed to obtain a mixture;

[0032] 2) The mixture obtained in step 1) is subjected to a solvothermal reaction to obtain a reaction product. The reaction product is washed and dried to obtain the V3O4 / SnO precursor.

[0033] 3) The V3O4 / SnO precursor obtained in step 2) is mixed with selenium powder and then subjected to a selenization reaction to obtain V3Se4 / SnSe composite material.

[0034] Vanadium chloride, tin chloride pentahydrate, glycerol, isopropanol, and hexadecyltrimethylammonium bromide were mixed to obtain a mixture.

[0035] In this invention, vanadium chloride and stannous chloride pentahydrate are preferably dispersed in a mixture of glycerol and isopropanol, and then hexadecyltrimethylammonium bromide is added. The mixing method preferably includes stirring, and the stirring time is preferably 150–210 min, more preferably 180 min. In this invention, the molar ratio of vanadium chloride, stannous chloride pentahydrate, glycerol, isopropanol, and hexadecyltrimethylammonium bromide is preferably 1 mmol:1–4 mmol:6–10 ml:20–30 ml:1.5–2.5 mmol, more preferably 1 mmol:2 mmol:8 ml:25 ml:2 mmol.

[0036] The present invention involves subjecting the obtained mixture to a solvothermal reaction to obtain a reaction product, which is then washed and dried to obtain a V3O4 / SnO precursor.

[0037] In this invention, the conditions for the solvothermal reaction preferably include: a temperature of 160–200°C and a time of 6–18 h; more preferably, a temperature of 180°C and a time of 10 h. In this invention, the washing reagent preferably includes ethanol, and it is preferred to use ethanol to wash the reaction product multiple times. In this invention, the drying conditions preferably include: a temperature of 60–80°C and a time of 12 h, with the temperature more preferably being 70°C.

[0038] In this invention, the obtained V3O4 / SnO precursor is mixed with selenium powder and then subjected to a selenization reaction to obtain V3Se4 / SnSe composite material.

[0039] In this invention, the mass ratio of the V3O4 / SnO precursor to selenium powder is preferably 1:4 to 15, more preferably 1:10. In this invention, the selenization reaction conditions preferably include: a temperature of 350 to 600°C and a time of 2 hours, with the temperature more preferably 500°C. In this invention, the selenization reaction is preferably carried out in a nitrogen atmosphere.

[0040] The present invention also provides a V3Se4 / SnSe composite material prepared by the preparation method described in the above technical solution.

[0041] This invention also provides the application of the V3Se4 / SnSe composite material described in the above technical solution in the preparation of sodium-ion batteries.

[0042] In this invention, the sodium-ion battery comprises the V3Se4 / SnSe composite material, Ketjen Black, and polydifluoroethylene. The preferred mass ratio of the V3Se4 / SnSe composite material, Ketjen Black, and polydifluoroethylene is 7:2:1. This invention does not specifically limit the source of the Ketjen Black and polydifluoroethylene; commercially available products conventionally used in the manufacture of sodium-ion batteries are acceptable.

[0043] To further illustrate the present invention, the following detailed description is provided in conjunction with embodiments, but these should not be construed as limiting the scope of protection of the present invention.

[0044] Example 1

[0045] First, 1 mmol of vanadium chloride and 1 mmol of tin chloride pentahydrate were dispersed in a mixed solution of 8 ml of glycerol and 25 ml of isopropanol. Then, 1.5 mmol of hexadecyltrimethylammonium bromide was added to the above solution and stirred for 180 min to obtain a uniform light blue solution.

[0046] The light blue solution was transferred to a 50 ml polytetrafluoroethylene-lined sealed autoclave and reacted at 180 °C for 10 h. After cooling to room temperature, the solvothermal product was washed multiple times with ethanol and then dried in a forced-air drying oven at 60 °C for 12 h to obtain the precursor V3O4 / SnO black powder.

[0047] Then, the prepared 50 mg V3O4 / SnO and 500 mg selenium powder were mixed together in a crucible and selenized at 600 °C for 2 h in a tube furnace under N2 atmosphere to obtain V3Se4 / SnSe composite material.

[0048] The prepared V3Se4 / SnSe battery anode material, Ketjen black, and polyvinyl difluoroethylene (PVDF) were mixed in an N-methyl-2-pyrrolidone (NMP) solvent at a mass ratio of 7:2:1. The mixture was stirred to obtain a uniform slurry, which was then coated onto a copper foil current collector and dried overnight in a vacuum oven at 120°C. After cooling to room temperature, the slices were removed, weighed, and equilibrated in a glove box for 12 hours before being assembled into a sodium-ion battery. The electrochemical performance of the battery was then tested.

[0049] Example 2

[0050] First, 1 mmol of vanadium chloride and 2 mmol of stannous chloride pentahydrate were dispersed in a mixed solution of 6 ml of glycerol and 20 ml of isopropanol. Then, 2.0 mmol of hexadecyltrimethylammonium bromide was added to the above solution and stirred for 150 min to obtain a uniform light blue solution.

[0051] The light blue solution was transferred to a 50 ml polytetrafluoroethylene-lined sealed autoclave and reacted at 160 °C for 18 h. After cooling to room temperature, the solvothermal product was washed several times with ethanol, and then dried in a forced-air drying oven at 70 °C for 12 h to obtain the precursor V3O4 / SnO black powder.

[0052] Then, the prepared 50 mg V3O4 / SnO and 200 mg selenium powder were mixed together in a crucible and selenized at 600 °C for 2 h in a tube furnace under N2 atmosphere to obtain V3Se4 / SnSe composite material.

[0053] The prepared V3Se4 / SnSe battery anode material, Ketjen black, and polyvinyl difluoroethylene (PVDF) were mixed in an N-methyl-2-pyrrolidone (NMP) solvent at a mass ratio of 7:2:1. The mixture was stirred to obtain a uniform slurry, which was then coated onto a copper foil current collector and dried overnight in a vacuum oven at 120°C. After cooling to room temperature, the slices were removed, weighed, and equilibrated in a glove box for 12 hours before being assembled into a sodium-ion battery. The electrochemical performance of the battery was then tested.

[0054] Example 3

[0055] First, 1 mmol of vanadium chloride and 4 mmol of stannous chloride pentahydrate were dispersed in a mixed solution of 10 ml of glycerol and 30 ml of isopropanol. Then, 2.5 mmol of hexadecyltrimethylammonium bromide was added to the above solution and stirred for 210 min to obtain a uniform light blue solution.

[0056] The light blue solution was transferred to a 50 ml polytetrafluoroethylene-lined sealed autoclave and reacted at 200 °C for 6 h. After cooling to room temperature, the solvothermal product was washed several times with ethanol and then dried in a forced-air drying oven at 80 °C for 12 h to obtain the precursor V3O4 / SnO black powder.

[0057] Then, the prepared 50 mg V3O4 / SnO and 750 mg selenium powder were mixed together in a crucible and selenized at 350 °C for 2 h in a tube furnace under N2 atmosphere to obtain V3Se4 / SnSe composite material.

[0058] The prepared V3Se4 / SnSe battery anode material, Ketjen black, and polyvinyl difluoroethylene (PVDF) were mixed in an N-methyl-2-pyrrolidone (NMP) solvent at a mass ratio of 7:2:1. The mixture was stirred to obtain a uniform slurry, which was then coated onto a copper foil current collector and dried overnight in a vacuum oven at 120°C. After cooling to room temperature, the slices were removed, weighed, and equilibrated in a glove box for 12 hours before being assembled into a sodium-ion battery. The electrochemical performance of the battery was then tested.

[0059] The three V3Se4 / SnSe battery anode materials prepared in Examples 1 (denoted as a), 2 (denoted as b), and 3 (denoted as c) were measured at 4Ag. -1 Electrochemical performance at current density. Table 1 shows the characterization results of the V3Se4 / SnSe battery anode materials prepared in Examples 1, 2, and 3. As can be seen from the data in Table 1, the V3Se4 / SnSe battery anode materials (a), (b), and (c) obtained using the preparation method described in this invention exhibit electrochemical performance at 4 A g. -1 Even after 1800 cycles at high current density, it still exhibits a capacity of 360.444 mAh g. -1 335.223mAh g-1 355.687mAh g -1 Excellent sodium storage performance.

[0060] like Figure 2 As can be seen from the field emission scanning electron microscope image of the V3Se4 / SnSe battery anode material prepared in Example 1, its morphology is a nanoplate composed of nanorods.

[0061] like Figure 3 The V3Se4 / SnSe heterojunction hierarchical composite material prepared in Example 1 was used as a negative electrode material for sodium-ion batteries in 4Ag -1 Long-cycle performance diagram after 1800 cycles at current density.

[0062] Table 1 Characterization results of V3Se4 / SnSe battery anode materials

[0063]

[0064] Although the above embodiments have provided a detailed description of the present invention, they are only some embodiments of the present invention, and not all embodiments. People can obtain other embodiments based on these embodiments without creative effort, and these embodiments all fall within the protection scope of the present invention.

Claims

1. The application of V3Se4 / SnSe composite material in the preparation of sodium-ion batteries, characterized in that, The components of the sodium-ion battery include the V3Se4 / SnSe composite material, Ketjen Black, and polydifluoroethylene; The mass ratio of the V3Se4 / SnSe composite material, Ketjen Black, and polydifluoroethylene is 7:2:

1. The preparation method of the V3Se4 / SnSe composite material includes the following steps: 1) Vanadium chloride, tin chloride pentahydrate, glycerol, isopropanol and hexadecyltrimethylammonium bromide are mixed to obtain a mixture; 2) The mixture obtained in step 1) is subjected to a solvothermal reaction to obtain a reaction product. The reaction product is washed and dried to obtain the V3O4 / SnO precursor. 3) The V3O4 / SnO precursor obtained in step 2) is mixed with selenium powder and then subjected to a selenization reaction to obtain V3Se4 / SnSe composite material; In step 1), the molar ratio of vanadium chloride, tin chloride pentahydrate, glycerol, isopropanol, and hexadecyltrimethylammonium bromide is 1 mmol: 1–4 mmol: 6–10 ml: 20–30 ml: 1.5–2.5 mmol. The conditions for the solvothermal reaction in step 2) include: a temperature of 160–200°C and a time of 6–18 h. In step 3), the mass ratio of V3O4 / SnO precursor to selenium powder is 1:4 to 15. The conditions for the selenization reaction in step 3) include: a temperature of 350–600°C and a time of 2 hours; The selenization reaction is carried out in a nitrogen atmosphere.

2. The application according to claim 1, characterized in that, The mixing method in step 1) includes stirring, and the stirring time is 150-210 min.

3. The application according to claim 1, characterized in that, The reagent used for washing in step 2) includes ethanol; The drying conditions include a temperature of 60–80°C and a time of 12 hours.

Citation Information

Patent Citations

  • A nitrogen-sulfur co-doped VSe2 / CNF potassium-ion battery anode material and its preparation method

    CN110190255B

  • Preparation method and application of VxSey / multi-walled carbon nanotube composite material

    CN115663143A

  • Bimetal selenide negative electrode material and preparation method and application thereof

    CN113921790A

  • Preparation method for and application of NANO cubic bimetal selenide material