Method for determining the dissolution time of metal particles in a battery

By monitoring the dissolution process of metal particles in lithium-ion batteries and using property parameters and aging parameters to determine the dissolution time, the problem of low accuracy in screening metal impurities in lithium-ion batteries has been solved, achieving higher screening accuracy and safety.

CN116774061BActive Publication Date: 2026-11-20CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202210234361.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-09
Publication Date
2026-11-20
Estimated Expiration
2042-03-09

AI Technical Summary

Technical Problem

In existing technologies, the accuracy of screening for metal impurities in lithium-ion batteries is low, making it difficult to effectively detect safety issues.

Method used

By acquiring the property parameters and aging parameters of the metal particles, the target oxidation current density is determined, and the dissolution process of the metal particles is monitored in units of time. The cumulative dissolution time is output to ensure accurate detection of problematic batteries with metal impurities during the aging stage.

Benefits of technology

It improves the accuracy of screening problematic lithium-ion batteries with metal impurities, ensuring accurate detection of batteries with incorporated metal particles during the aging stage and reducing safety hazards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116774061B_ABST
    Figure CN116774061B_ABST
Patent Text Reader

Abstract

The application discloses a method for determining the dissolution time of metal particles in a battery, which comprises the following steps: obtaining attribute parameters and aging parameters of the metal particles, and determining a corresponding target oxidation current density according to the attribute parameters and the aging parameters; determining the current radius of the metal particles at the cutoff time of the current unit time based on the target oxidation current density, and accumulating the unit time to obtain an accumulated dissolution time; determining whether the metal particles are dissolved completely according to the current radius, and outputting the accumulated dissolution time in the case that the metal particles are dissolved completely. In this way, the dissolution time of the metal particles in the battery under the aging parameters can be accurately determined, and if the metal particles are integrated into a battery to be detected, the battery can be accurately detected in the aging stage, and the screening accuracy of the problem battery integrated with metal impurities is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of batteries, specifically to a method for determining the dissolution time of metal particles in a battery and a method for detecting the battery to be tested. Background Technology

[0002] Lithium-ion batteries are now widely used in various everyday digital products, entering the lives of countless households. They are the main energy storage devices in military electronic products, aerospace electronic components, electric vehicles, and various portable electronic devices. The production process of lithium-ion battery cathode materials involves many steps, and each stage carries the risk of metal impurities being incorporated. When metal impurities are present in the cathode material, if the voltage during battery formation reaches the oxidation-reduction potential of these impurities, they will first oxidize at the cathode and then reduce at the anode. When the metal elemental content at the anode accumulates to a certain level, it can puncture the separator, causing battery self-discharge and leading to safety issues.

[0003] In existing technologies, batteries can be aged for a period of time using specific aging parameters such as aging temperature and aging voltage to detect whether metal particles dissolve and leach out, thereby identifying batteries with self-discharge problems. However, the selection of aging parameters such as aging temperature and aging voltage, as well as the determination of aging time, can affect whether problematic batteries with metal impurities can be detected, resulting in a low accuracy rate in screening for such batteries. Summary of the Invention

[0004] In view of the above problems, this application provides a method for determining the dissolution time of metal particles in a battery and a method for detecting the battery to be tested, which can alleviate the problem of low screening accuracy of batteries with metal impurities.

[0005] In a first aspect, this application provides a method for determining the dissolution time of metal particles in a battery, comprising: acquiring the property parameters and aging parameters of the metal particles, and determining the corresponding target oxidation current density based on the property parameters and aging parameters; determining the current radius of the metal particles at the end time of the current unit time based on the target oxidation current density, taking a unit time as the period, and accumulating the unit time to obtain the cumulative dissolution time; determining whether the metal particles have completely dissolved based on the current radius, and outputting the cumulative dissolution time if the metal particles have completely dissolved.

[0006] In the technical solution of this application embodiment, based on the obtained attribute parameters and aging parameters of the metal particles, the remaining radius of the metal particles is periodically monitored on a unit time basis, i.e., the dissolution process of the metal particles is periodically monitored to determine whether the metal particles have completely dissolved. When the metal particles have completely dissolved, the cumulative dissolution time consumed by the dissolution of the metal particles is output. In this way, the dissolution time of the metal particles incorporated into the battery under the given aging parameters can be accurately determined. If the battery to be tested contains the metal particles, it can be accurately detected during the aging stage, thus improving the screening accuracy of problematic batteries with incorporated metal impurities.

[0007] In some embodiments, determining the current radius of the metal particle at the cutoff time of the current unit time based on the target oxidation current density includes:

[0008] Based on the target oxidation current density, determine the current dissolution current of the metal particles per unit time;

[0009] Based on the current dissolution current, determine the current dissolution mass of the metal particles per unit time.

[0010] Based on the current dissolved mass, determine the current radius of the metal particles at the cutoff time of the current unit of time.

[0011] In the technical solution of this application embodiment, a dissolution current is generated when metal particles dissolve. The magnitude of the dissolution current can indicate how much mass of metal particles are dissolved. By monitoring the dissolution current within a unit time, the current dissolution mass of metal particles within that unit time can be determined. Based on this current dissolution mass, the current radius of the metal particles at the end of the current unit time can be determined, ensuring the accuracy of the determined current radius of the metal particles at the end of the current unit time. This, in turn, ensures the accuracy of the cumulative dissolution time consumed by the dissolution of metal particles, and more effectively alleviates the problem of low screening accuracy of batteries with metal impurities.

[0012] In some embodiments, determining the corresponding target oxidation current density based on attribute parameters and aging parameters includes:

[0013] Based on the attribute parameters and aging parameters, obtain the corresponding target oxidation current density from the preset oxidation current density table;

[0014] Accordingly, based on the target oxidation current density, the current dissolution current of the metal particles per unit time is determined, including:

[0015] Obtain the particle radius at the cutoff time of the previous unit of time, and determine the current surface area of ​​the metal particle based on the particle radius at the cutoff time of the previous unit of time.

[0016] Determine the current dissolution current of the metal particles per unit time based on the target oxidation current density and the current surface area of ​​the metal particles.

[0017] In the technical solution of this application embodiment, different metal particles and different aging parameters result in different oxidation current densities during the dissolution process. The preset oxidation current density table can store multiple attribute parameters and oxidation current densities corresponding to aging parameters in advance. Therefore, based on the obtained attribute parameters and aging parameters, the corresponding target oxidation current density can be obtained from the preset oxidation current density table. Then, combined with the current surface area of ​​the metal particles monitored in the current unit time, the current dissolution current of the metal particles in the current unit time can be accurately determined, ensuring the accuracy of the determined current dissolution current. This, in turn, ensures the accuracy of the cumulative dissolution time consumed by the metal particles, and more effectively alleviates the problem of low screening accuracy of batteries with metal impurities.

[0018] In some embodiments, determining the current dissolved mass of metal particles per unit time based on the current dissolution current includes:

[0019] Based on the current dissolution current, determine the amount of transferred charge that dissolves from the metal particles per unit time.

[0020] The current dissolved mass of metal particles per unit time is determined based on the amount of transferred charge.

[0021] In the technical solution of this application embodiment, charge transfer occurs during the dissolution process of metal particles. Therefore, the amount of transferred charge dissolved by the metal particles per unit time can be determined first based on the current dissolution current. Then, based on the amount of transferred charge, the current dissolution mass of the metal particles per unit time can be accurately determined, ensuring the accuracy of the determined current dissolution mass. This, in turn, ensures the accuracy of the cumulative dissolution time consumed by the dissolution of metal particles, and more effectively alleviates the problem of low screening accuracy of batteries with metal impurities.

[0022] In some embodiments, determining the current radius of the metal particles at the cutoff time of the current unit time, based on the current dissolved mass, includes:

[0023] Determine the current remaining mass of the metal particles based on the current dissolved mass and the remaining mass in the previous unit of time;

[0024] Based on the current remaining mass, determine the current radius of the metal particle at the cutoff time of the current unit of time.

[0025] In the technical solution of this application embodiment, the determined current dissolution mass is the mass of metal particles dissolved in the current unit time. Therefore, based on the current dissolution mass and the remaining mass in the previous unit time, the current remaining mass of the metal particles can be determined, thereby accurately determining the current radius of the metal particles at the end of the current unit time. This ensures the accuracy of the determined current radius of the metal particles at the end of the current unit time, and further ensures the accuracy of the cumulative dissolution time consumed by the dissolution of metal particles, thus more effectively alleviating the problem of low screening accuracy of batteries with metal impurities.

[0026] In some embodiments, before obtaining the corresponding target oxidation current density from a preset oxidation current density table based on attribute parameters and aging parameters, the method further includes:

[0027] Based on the test temperature group and the test voltage group, charging tests are performed on the test battery and the reference battery to determine the oxidation current density corresponding to different test temperatures and different test voltages. The test temperature group includes at least one test temperature, and the test voltage group includes at least one test voltage.

[0028] A preset oxidation current density table is constructed based on the oxidation current density corresponding to different test temperatures and test voltages.

[0029] In the technical solution of this application embodiment, test batteries and reference batteries can be pre-created. According to the test temperature group and test voltage group, the oxidation current density corresponding to different test temperatures and different test voltages is tested. The oxidation current density can be calculated based on the property parameters of the metal particles. Then, a preset oxidation current density table can be constructed based on the property parameters of the metal particles, the test temperature, and the test voltage. This makes it easy to directly obtain the corresponding target oxidation current density from the preset oxidation current density table based on the obtained property parameters and aging parameters of the metal particles. This accurately determines the current dissolution current of the metal particles per unit time, ensuring the accuracy of the determined current dissolution current. This, in turn, ensures the accuracy of the cumulative dissolution time consumed by the dissolution of the metal particles, and more effectively alleviates the problem of low screening accuracy of batteries with metal impurities.

[0030] In some embodiments, charging tests are performed on the test battery and the reference battery according to a test temperature group and a test voltage group to determine the oxidation current density corresponding to different test temperatures and different test voltages, including:

[0031] S1: Select the first test temperature from the test temperature group;

[0032] S2: At the first test temperature, the test battery and the reference battery are charged sequentially using each test voltage in the test voltage group to determine the oxidation current density corresponding to each test voltage at the first test temperature.

[0033] S3: Take any other test temperature in the test temperature group as the first test temperature, replace the test battery and the reference battery, and return to the operation steps of S2 until all test temperatures in the test temperature group have been tested, and obtain the oxidation current density corresponding to different test temperatures and different test voltages.

[0034] In the technical solution of this application embodiment, for a certain test temperature, the test battery and the reference battery can be charged and tested sequentially using each test voltage in the test voltage group to determine the oxidation current density corresponding to each test voltage at the first test temperature. Then, the above process is repeated for the next test temperature in the test temperature group until the oxidation current density corresponding to different test voltages at different test temperatures is obtained. The oxidation current density corresponding to different test voltages at different test temperatures is pre-measured, and a preset oxidation current density table is constructed. This facilitates the direct acquisition of the corresponding target oxidation current density from the preset oxidation current density table based on the obtained attribute parameters and aging parameters of the metal particles, so as to accurately determine the current dissolution current of the metal particles per unit time. This ensures the accuracy of the determined current dissolution current, thereby ensuring the accuracy of the cumulative dissolution time consumed by the dissolution of metal particles, and more effectively alleviating the problem of low screening accuracy of problematic batteries with metal impurities.

[0035] In some embodiments, the test battery and the reference battery are sequentially charged using each test voltage in the test voltage group to determine the oxidation current density corresponding to each test voltage at a first test temperature, including:

[0036] S21: Select the first test voltage from the test voltage group;

[0037] S22: After charging the test battery at a constant voltage for a preset time using the first test voltage, obtain the test current corresponding to the first test voltage, and after charging the reference battery at a constant voltage for a preset time using the first test voltage, obtain the reference current corresponding to the first test voltage.

[0038] S23: Determine the oxidation current corresponding to the first test temperature and the first test voltage based on the test current and the reference current;

[0039] S24: Obtain the property parameters of the metal particles set in the test battery, and determine the oxidation current density corresponding to the first test temperature and the first test voltage based on the property parameters and the oxidation current;

[0040] S25: Take any other test voltage in the test voltage group as the first test voltage, and return to the operation step of S22 until all test voltages in the test voltage group have been tested, and obtain the oxidation current density corresponding to each test voltage at the first test temperature.

[0041] In the technical solution of this application embodiment, for a certain test temperature, a test voltage can be selected from the test voltage group to perform a charging test on the test battery and the reference battery. Based on the test current and the reference current, the oxidation current is determined. Then, based on the property parameters of the metal particles and the oxidation current, the oxidation current density corresponding to the test voltage at the test temperature is determined. Then, at the test temperature, the above process is repeated for the next test voltage in the test voltage group until the oxidation current density corresponding to each test voltage at the test temperature is obtained. By performing the above process for each test temperature, the oxidation current density corresponding to different test voltages at different test temperatures can be measured in advance, and a preset oxidation current density table can be constructed. This makes it convenient to directly obtain the corresponding target oxidation current density from the preset oxidation current density table based on the obtained property parameters and aging parameters of the metal particles, so as to accurately determine the current dissolution current of the metal particles in the current unit time, ensuring the accuracy of the determined current dissolution current, and thus ensuring the accuracy of the cumulative dissolution time consumed by the dissolution of metal particles, and more effectively alleviating the problem of low screening accuracy of problematic batteries with metal impurities.

[0042] In some embodiments, before performing charging tests on the test battery and the reference battery according to the test temperature group and the test voltage group, and determining the oxidation current density corresponding to different test temperatures and different test voltages, the method further includes:

[0043] Experimental batteries were prepared using positive electrode materials, metal particles, and negative electrode materials.

[0044] A reference battery was prepared using positive and negative electrode materials.

[0045] In the technical solution of this application embodiment, a test battery can be prepared in advance using positive electrode material, metal particles, and negative electrode material, and a reference battery can be prepared using positive electrode material and negative electrode material. That is, the positive electrode material of the test battery incorporates metal particles, while the reference battery does not incorporate metal particles. This allows for comparison of the test current and the reference current to determine the oxidation current, providing a data basis for subsequently determining the current radius of the metal particles at the current unit time cutoff time. This ensures the accuracy of the cumulative dissolution time consumed by the metal particles and more effectively alleviates the problem of low screening accuracy of batteries with incorporated metal impurities.

[0046] In some embodiments, a test battery is prepared using a positive electrode material, metal particles, and a negative electrode material, including:

[0047] A positive electrode slurry is coated onto a current collector, and a set mass of metal particles is weighed and placed on the surface of the positive electrode slurry. The positive electrode slurry is obtained by mixing positive electrode materials according to a set ratio.

[0048] After the positive electrode slurry is dried, it is coated again to obtain the positive electrode sheet;

[0049] A test cell was prepared using a positive electrode and a pre-made negative electrode.

[0050] In the technical solution of this application embodiment, a layer of positive electrode slurry can be coated first, and a certain amount of metal particles can be placed on the positive electrode slurry. Then, a layer of positive electrode slurry is coated again to wrap the metal particles. A sandwich structure is adopted to integrate the metal particles into the positive electrode material, simulating the situation where metal particles are mixed into the positive electrode material in a real scenario. This makes the metal particles mixed in the test battery closer to the real scenario, rather than located on the surface of the positive electrode material. This ensures the accuracy of the current radius of the determined metal particles at the current unit time cutoff time, thereby ensuring the accuracy of the cumulative dissolution time consumed by the dissolution of metal particles. This more effectively alleviates the problem of low screening accuracy of batteries with metal impurities.

[0051] In some embodiments, after outputting the cumulative dissolution time, the method further includes:

[0052] The property parameters, aging parameters, and corresponding cumulative dissolution time of the metal particles are stored accordingly.

[0053] In the technical solution of this application embodiment, after determining the cumulative dissolution time consumed by the dissolution of metal particles, the attribute parameters of the metal particles, the aging parameters used, and the corresponding cumulative dissolution time can be stored accordingly. Subsequently, when aging the battery to be tested, the corresponding aging parameters and the corresponding cumulative dissolution time can be selected according to the requirements. If metal particles are incorporated into the battery to be tested, it can be ensured that they are accurately detected during the aging stage, thereby improving the screening accuracy of problematic batteries with incorporated metal impurities.

[0054] Secondly, this application provides a method for detecting a battery to be tested, comprising:

[0055] Obtain the attribute parameters, aging parameters and corresponding estimated dissolution time of the battery to be tested, wherein the estimated dissolution time is determined according to the method for determining the dissolution time of metal particles in the battery described in the first aspect above;

[0056] Aging parameters were used to estimate the dissolution time of the battery under test.

[0057] After estimating the dissolution time during aging, the voltage drop of the battery under test is determined, and the battery under test is determined to be a problem battery based on the voltage drop.

[0058] In the technical solution of this application embodiment, the attribute parameters, aging parameters and corresponding estimated dissolution time of the battery to be tested can be obtained. The estimated dissolution time is determined based on the method for determining the dissolution time of metal particles in the battery. The method can accurately determine the dissolution time of metal particles incorporated into the battery under a certain aging parameter. Therefore, the determined cumulative dissolution time can be used as the estimated dissolution time. The battery to be tested is aged using the corresponding aging parameters. If the metal particles are incorporated into the battery to be tested, it can be accurately detected during the aging stage, thus improving the screening accuracy of problematic batteries with incorporated metal impurities.

[0059] In some embodiments, after estimating the dissolution time through aging, the voltage drop of the battery under test is determined, and whether the battery under test is a problematic battery is determined based on the voltage drop, including:

[0060] After estimating the aging and dissolution time, the battery to be tested is left to stand for a first preset time, and the first voltage of the battery to be tested is obtained.

[0061] The battery to be tested is left to stand for a second preset time, and the second voltage of the battery to be tested is obtained, wherein the second preset time is longer than the first preset time.

[0062] The voltage difference between the first voltage and the second voltage is taken as the voltage drop;

[0063] If the voltage drop exceeds a preset threshold, the battery under test is identified as a problematic battery.

[0064] In the technical solution of this application embodiment, the voltage difference between the battery under test after a first preset resting time and a second preset resting time can be determined. If the voltage difference is too large, it indicates that metal particles have been incorporated into the battery under test, and the battery under test is a problematic battery. If the voltage difference is small, it indicates that no metal particles have been incorporated into the battery under test, and the battery under test is a safe battery. Thus, when the accuracy of the estimated dissolution time is high, the voltage drop of the battery under test over a period of time after aging can accurately determine whether the battery under test is a problematic battery, improving the screening accuracy of problematic batteries with incorporated metal impurities.

[0065] In some embodiments, the battery to be tested is prepared from a casing and at least one cell assembly, wherein the cell assembly is a lithium-ion cell and is prepared from a positive electrode, a negative electrode, an electrolyte, a separator, a shell, and terminals.

[0066] In the technical solution of this application embodiment, the battery to be tested can be prepared from a casing and at least one cell assembly. The cell assembly is a lithium-ion cell, which is prepared from a positive electrode, a negative electrode, an electrolyte, a separator, a casing, and terminals. The battery to be tested is tested using determined aging parameters and estimated dissolution time. If the metal particles are incorporated into the battery to be tested, it can be accurately detected during the aging stage, thus improving the screening accuracy of problematic batteries with incorporated metal impurities.

[0067] The above description is only an overview of the technical solution of this application. In order to better understand the technical means of this application and to implement it in accordance with the contents of the specification, and to make the above and other objects, features and advantages of this application more obvious and understandable, the following are specific embodiments of this application. Attached Figure Description

[0068] Various other advantages and benefits will become apparent to those skilled in the art upon reading the detailed description of the preferred embodiments below. The accompanying drawings are for illustrative purposes only and are not intended to limit the scope of this application. Furthermore, the same reference numerals denote the same parts throughout the drawings. In the drawings:

[0069] Figure 1 A flowchart illustrating a method for determining the dissolution time of metal particles in a battery, provided in some embodiments of this application;

[0070] Figure 2 This is a schematic diagram illustrating the dissolution of metal particles provided in some embodiments of this application;

[0071] Figure 3 Optical photographs of iron metal particles provided for some embodiments of this application;

[0072] Figure 4 Particle size distribution diagrams of iron metal particles provided in some embodiments of this application;

[0073] Figure 5 Schematic diagrams of the positive electrode structure provided for some embodiments of this application;

[0074] Figure 6(a) shows the cumulative dissolution time at 25°C for different voltages provided in some embodiments of this application;

[0075] Figure 6(b) shows the cumulative dissolution time at 45°C for different voltages provided in some embodiments of this application;

[0076] Figure 7 A flowchart illustrating another method for determining the dissolution time of metal particles in a battery, provided for some embodiments of this application.

[0077] Figure 8This is a flowchart illustrating a method for detecting a battery under test, provided in some embodiments of this application. Detailed Implementation

[0078] The embodiments of the technical solution of this application will now be described in detail with reference to the accompanying drawings. These embodiments are only used to more clearly illustrate the technical solution of this application and are therefore merely examples, and should not be used to limit the scope of protection of this application.

[0079] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application pertains; the terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the application; the terms “comprising” and “having”, and any variations thereof, in the specification, claims, and foregoing description of the drawings are intended to cover non-exclusive inclusion.

[0080] In the description of the embodiments of this application, technical terms such as "first" and "second" are used only to distinguish different objects and should not be construed as indicating or implying relative importance or implicitly specifying the number, specific order, or primary and secondary relationship of the indicated technical features. In the description of the embodiments of this application, "multiple" means two or more, unless otherwise explicitly defined.

[0081] In this document, the term "embodiment" means that a particular feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment of this application. The appearance of this phrase in various places throughout the specification does not necessarily refer to the same embodiment, nor is it a separate or alternative embodiment mutually exclusive with other embodiments. It will be explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments.

[0082] In the description of the embodiments in this application, the term "and / or" is merely a description of the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent three cases: A exists, A and B exist simultaneously, and B exists. In addition, the character " / " in this document generally indicates that the related objects before and after it have an "or" relationship.

[0083] In the description of the embodiments of this application, the term "multiple" refers to two or more (including two), similarly, "multiple sets" refers to two or more (including two sets), and "multiple pieces" refers to two or more (including two pieces).

[0084] In the description of the embodiments of this application, the technical terms "center," "longitudinal," "lateral," "length," "width," "thickness," "upper," "lower," "front," "rear," "left," "right," "vertical," "horizontal," "top," "bottom," "inner," "outer," "clockwise," "counterclockwise," "axial," "radial," and "circumferential" indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are only for the convenience of describing the embodiments of this application and simplifying the description, and are not intended to indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on the embodiments of this application.

[0085] In the description of the embodiments of this application, unless otherwise expressly specified and limited, technical terms such as "installation," "connection," "joining," and "fixing" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral part; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; they can refer to the internal communication of two components or the interaction between two components. For those skilled in the art, the specific meaning of the above terms in the embodiments of this application can be understood according to the specific circumstances.

[0086] Currently, lithium-ion batteries are widely used in various everyday digital products, entering thousands of households. In addition, thanks to technological innovation and policy support, larger capacity battery packs are being used to provide fuel power for isolated power equipment, such as electric vehicles, ships, cranes, and aircraft, and are also being used in power plants for energy storage projects. A battery pack contains dozens or even thousands of cells connected in series or parallel. The capacity and lifespan of the entire battery pack are closely related to the performance of each cell; the performance of a single cell significantly affects the consistency of the battery pack.

[0087] The production process of positive electrode materials for lithium-ion batteries involves many steps, and there is a risk of metal impurities being incorporated at each stage of the manufacturing process. When metal impurities are incorporated into the positive electrode material, after the voltage during the battery formation stage reaches the oxidation-reduction potential of the metal impurities, these metal impurities will first oxidize at the positive electrode and then be reduced at the negative electrode. When the metal elements at the negative electrode accumulate to a certain extent, they will puncture the separator, causing the battery to self-discharge and leading to safety issues. The self-discharge problem of a single cell caused by the dissolution of metal impurities may drag down the performance of the entire battery pack or even render it unusable.

[0088] The inventors have noted that in existing technologies, batteries are aged for a period of time using specific aging parameters such as aging temperature and aging voltage, and the presence of dissolved metal particles is detected to identify batteries with self-discharge problems. However, the selection of aging parameters such as aging temperature and aging voltage, as well as the determination of aging time, can affect the detection of batteries with metal impurities, resulting in a low accuracy rate in screening for such batteries.

[0089] To address the issue of low screening accuracy in batteries containing metallic impurities, the applicant's research revealed that the main metallic impurities in batteries are copper, iron, stainless steel, aluminum, and zinc. To detect these impurities, it is necessary to determine the dissolution time of metal particles of different sizes. The dissolution rate of different metal particles is primarily influenced by aging parameters such as aging voltage and aging temperature. By measuring the oxidation current per unit area of ​​metal particles during dissolution under different conditions and periodically monitoring the dissolution process, the cumulative dissolution time consumed by the metal particles can be determined. This can guide subsequent battery aging processes, enabling the in-factory detection of batteries with low self-discharge voltage caused by metallic impurities.

[0090] Based on the above considerations, to address the low screening accuracy of batteries with incorporated metal impurities, this application provides a method for determining the dissolution time of metal particles in a battery. The method involves aging the battery based on the obtained attribute parameters and aging parameters of the metal particles. During aging, the metal particles incorporated into the battery dissolve. The remaining radius of the metal particles is periodically monitored, i.e., the dissolution process is periodically monitored, to determine whether the metal particles have completely dissolved. When the metal particles have completely dissolved, the cumulative dissolution time is output. In this way, the dissolution time of the metal particles incorporated into the battery under the given aging parameters can be accurately determined. If the battery to be tested contains these metal particles, accurate detection during the aging stage can be guaranteed, thus improving the screening accuracy of batteries with incorporated metal impurities.

[0091] The method for determining the dissolution time of metal particles in a battery disclosed in this application can be applied to a lithium-ion battery testing system. This testing system can output the cumulative dissolution time of metal particles. Based on the determined cumulative dissolution time of metal particles, the aging process of lithium-ion batteries can be guided, enabling the detection of batteries with low self-discharge voltage caused by metal impurities in-factory.

[0092] Please refer to Figure 1 , Figure 1 A flowchart illustrating a method for determining the dissolution time of metal particles in a battery according to some embodiments of this application is shown below. Figure 1 As shown, it includes the following steps 102-106:

[0093] Step 102: Obtain the property parameters and aging parameters of the metal particles, and determine the corresponding target oxidation current density based on the property parameters and aging parameters.

[0094] Specifically, the metal particles refer to the metal particles placed in the testing battery. These metal particles can be copper, iron, stainless steel, aluminum, zinc, etc. The attribute parameters can refer to the type and radius of the metal particles, while the aging parameters can refer to the aging temperature and aging voltage.

[0095] In practical applications, the property parameters of the metal particles whose dissolution time needs to be estimated can be determined. Then, the aging parameters to be measured can be selected. The property parameters and aging parameters are used as inputs. Then, the corresponding target oxidation current density can be determined based on the obtained property parameters and aging parameters. Subsequently, the current radius of the metal particles can be determined by combining the target oxidation current density, thereby monitoring the dissolution process of the metal particles to determine whether the metal particles have completely dissolved.

[0096] Step 104: Using unit time as the period, determine the current radius of the metal particles at the cutoff time of the current unit time based on the target oxidation current density, and accumulate the unit time to obtain the cumulative dissolution time.

[0097] Specifically, a unit time refers to a set period of time, such as 1 second, 5 seconds, or 10 seconds. This unit time represents the period during which the metal particles are monitored to see if they have completely dissolved. The current radius refers to the radius remaining when the metal particles have dissolved up to the end of the current unit time. The cumulative dissolution time refers to the cumulative time that the metal particles have taken to dissolve up to the current unit time.

[0098] It should be noted that for each unit of dissolution time, the current radius of the metal particle at the cutoff time of the current unit of time can be determined, and the cumulative dissolution time can be obtained by accumulating the unit of time.

[0099] As an example, with a unit time of 10 seconds, the battery is aged based on the obtained attribute parameters and aging parameters. At the 10th second, the current radius of the metal particles is determined and accumulated over the unit time to obtain a cumulative dissolution time of 10 seconds. At the 20th second, the current radius of the metal particles is determined and accumulated over the unit time to obtain a cumulative dissolution time of 20 seconds. At the 30th second, the current radius of the metal particles is determined and accumulated over the unit time to obtain a cumulative dissolution time of 30 seconds. This process continues until the metal particles are completely dissolved, and the final cumulative dissolution time is output.

[0100] Step 106: Based on the current radius, determine whether the metal particles have completely dissolved. If the metal particles have completely dissolved, output the cumulative dissolution time.

[0101] It should be noted that metal particles are generally spherical in structure, and after a unit of time of dissolution, they remain spherical, and a certain thickness of metal particles will dissolve within that unit of time. Figure 2 For schematic diagrams of metal particle dissolution provided in some embodiments of this application, please refer to... Figure 2 The unit time is dt, and the dissolution thickness of the metal particle within this unit time is dx = (d1-d) / 2, where d1 represents the particle diameter at the cutoff time of the previous unit time, and d represents the current diameter at the cutoff time of the current unit time.

[0102] In practical applications, the current radius of a metal particle refers to the radius remaining after the particle has dissolved to the end of the current unit of time. Therefore, it is possible to determine whether the metal particle has completely dissolved based on the current radius. If the current radius is greater than a predetermined threshold, it can be determined that the metal particle has not completely dissolved, and dissolution can continue for another unit of time, accumulating the dissolution time. If the current radius is less than or equal to the predetermined threshold, it can be determined that the metal particle has completely dissolved, and the accumulated dissolution time can be output. This accumulated dissolution time is the time required for the metal particles in the battery to dissolve under this attribute parameter and aging parameter.

[0103] The predetermined threshold can be a set value, which can be 0. Furthermore, since the dissolution rate of metal particles slows significantly after they dissolve to a certain size, the predetermined threshold can also be set to a value indicating that most of the metal particles have already dissolved. In other words, the predetermined threshold can be set to an extremely small value, and it can be determined that the metal particles have completely dissolved when their current radius is less than or equal to the predetermined threshold.

[0104] As an example, with a unit time of 10 seconds, the battery is aged based on the obtained attribute parameters and aging parameters. At the 10th second, the current radius of the metal particles is determined to be 25µm. The cumulative dissolution time is calculated as 10 seconds. Since the current radius is greater than the predetermined threshold of 1µm, the metal particles continue to dissolve for another 10 seconds. At the 20th second, the current radius of the metal particles is determined to be 20µm, and the cumulative dissolution time is calculated as 20 seconds. Since the current radius is greater than the predetermined threshold of 1µm, the metal particles continue to dissolve for another 10 seconds. This process continues until the 300th second, when the current radius of the metal particles is determined to be 1µm. The cumulative dissolution time is calculated as 300 seconds. Since the current radius equals the predetermined threshold of 1µm, it can be determined that the metal particles have completely dissolved, and the final cumulative dissolution time of 300 seconds is output.

[0105] In the technical solution of this application embodiment, based on the obtained attribute parameters and aging parameters of the metal particles, the remaining radius of the metal particles is periodically monitored on a unit time basis, i.e., the dissolution process of the metal particles is periodically monitored to determine whether the metal particles have completely dissolved. When the metal particles have completely dissolved, the cumulative dissolution time consumed by the dissolution of the metal particles is output. In this way, the dissolution time of the metal particles incorporated into the battery under the given aging parameters can be accurately determined. If the battery to be tested contains the metal particles, it can be accurately detected during the aging stage, thus improving the screening accuracy of problematic batteries with incorporated metal impurities.

[0106] According to some embodiments of this application, the current dissolved mass of metal particles within a current unit time can be monitored to determine the current radius of the metal particles at the end of the current unit time, that is, the determination of the current radius of the metal particles at the end of the current unit time in step 104 above can be achieved through the following steps:

[0107] Step 1: Based on the target oxidation current density, determine the current dissolution current of the metal particles per unit time.

[0108] It should be noted that the current dissolution current is the current generated by the dissolution of metal particles per unit time.

[0109] Step 2: Determine the current dissolved mass of metal particles per unit time based on the current dissolution current.

[0110] It should be noted that the current dissolved mass refers to the mass of metal particles dissolved in the current unit of time.

[0111] Step 3: Based on the current dissolved mass, determine the current radius of the metal particles at the cutoff time of the current unit of time.

[0112] In the technical solution of this application embodiment, a dissolution current is generated when metal particles dissolve. The magnitude of the dissolution current can indicate how much mass of metal particles are dissolved. By monitoring the dissolution current within a unit time, the current dissolution mass of metal particles within that unit time can be determined. Based on this current dissolution mass, the current radius of the metal particles at the end of the current unit time can be determined, ensuring the accuracy of the determined current radius of the metal particles at the end of the current unit time. This, in turn, ensures the accuracy of the cumulative dissolution time consumed by the dissolution of metal particles, and more effectively alleviates the problem of low screening accuracy of batteries with metal impurities.

[0113] According to some embodiments of this application, the corresponding target oxidation current density can be obtained from a preset oxidation current density table, and then the current dissolution current of the metal particles can be determined based on the current surface area of ​​the metal particles and the target oxidation current density. That is, the above-mentioned step 102 and the above-mentioned step "determining the current dissolution current of the metal particles per unit time based on the target oxidation current density" can be achieved through the following steps:

[0114] Step 1: Based on the attribute parameters and aging parameters, obtain the corresponding target oxidation current density from the preset oxidation current density table.

[0115] It should be noted that attribute parameters and aging parameters refer to the relevant parameters obtained for aging the battery. The preset oxidation current density table is a set of multiple oxidation current densities measured in advance based on the test battery and the reference battery. These multiple oxidation current densities are oxidation current densities corresponding to different attribute parameters and different aging parameters.

[0116] It should be noted that different metal particles and different aging parameters result in different oxidation current densities during the dissolution process. The preset oxidation current density table can store multiple attribute parameters and oxidation current densities corresponding to aging parameters in advance. Therefore, the target oxidation current density can be obtained from the preset oxidation current density table based on the obtained attribute parameters and aging parameters.

[0117] Step 2: Obtain the particle radius at the cutoff time of the previous unit of time, and determine the current surface area of ​​the metal particle based on the particle radius at the cutoff time of the previous unit of time.

[0118] It should be noted that during the dissolution process of metal particles, the current radius at the cutoff time of the current unit time cannot be measured in real time. However, the particle radius at the cutoff time of the previous unit time has been calculated. Since unit time is often short, the dissolved thickness of the metal particle in the current unit time is smaller than that in the previous unit time, resulting in a smaller change in surface area. Therefore, the current radius at the cutoff time of the current unit time is very close to the particle radius at the cutoff time of the previous unit time. Thus, the current surface area of ​​the metal particle can be calculated based on the particle radius at the cutoff time of the previous unit time. In other words, the current surface area of ​​the metal particle in the current unit time can be estimated based on the particle radius at the cutoff time of the previous unit time.

[0119] Step 3: Determine the current dissolution current of the metal particles per unit time based on the target oxidation current density and the current surface area of ​​the metal particles.

[0120] It should be noted that the current surface area of ​​the metal particles can be the specific surface area s(m²). 2 / kg), where the specific surface area is the total area of ​​a unit mass of metal particles. The current dissolution current of the metal particles per unit time can be obtained by multiplying the target oxidation current density by this specific surface area. That is, the current dissolution current can be calculated using the following formula (1):

[0121] I = j*s (1)

[0122] Where I is the current dissolution current of the metal particles per unit time, j is the target oxidation current density, and s is the current specific surface area of ​​the metal particles (m²). 2 / kg).

[0123] In the technical solution of this application embodiment, different metal particles and different aging parameters result in different oxidation current densities during the dissolution process. The preset oxidation current density table can store multiple attribute parameters and oxidation current densities corresponding to aging parameters in advance. Therefore, based on the obtained attribute parameters and aging parameters, the corresponding target oxidation current density can be obtained from the preset oxidation current density table. Then, combined with the current surface area of ​​the metal particles monitored in the current unit time, the current dissolution current of the metal particles in the current unit time can be accurately determined, ensuring the accuracy of the determined current dissolution current. This, in turn, ensures the accuracy of the cumulative dissolution time consumed by the metal particles, and more effectively alleviates the problem of low screening accuracy of batteries with metal impurities.

[0124] According to some embodiments of this application, the current dissolved mass of metal particles can be determined based on the amount of charge transferred during the dissolution of the metal particles. That is, the above step "determining the current dissolved mass of metal particles per unit time based on the current dissolution current" can be achieved through the following steps:

[0125] Step 1: Determine the amount of transferred charge of metal particles dissolved per unit time based on the current dissolution current.

[0126] It should be noted that charge transfer occurs during the dissolution process of metal particles. Therefore, the amount of charge transferred by the dissolving metal particles per unit time can be determined based on the current dissolution current. In practical applications, the amount of charge transferred by the dissolving metal particles per unit time can be obtained by multiplying the current dissolution current by the unit time. That is, the amount of charge transferred by the dissolving metal particles per unit time can be determined by the following formula (2):

[0127] Q = idt (2)

[0128] Where Q represents the amount of charge transferred by the dissolution of metal particles per unit time, i represents the current dissolution current, and dt represents the unit time.

[0129] Step 2: Determine the current dissolved mass of metal particles per unit time based on the amount of transferred charge.

[0130] It should be noted that the amount of charge transferred per unit time can represent the amount of metal particles dissolved per unit time. Therefore, once the amount of charge transferred and dissolved by the metal particles per unit time is determined, the current dissolved mass of the metal particles per unit time can be determined based on the amount of charge transferred.

[0131] In practical applications, the current dissolved mass of metal particles per unit time can be determined using the following formula (3):

[0132] dm=QM / (nF) (3)

[0133] Where dm represents the current dissolved mass of the metal particle per unit time, Q represents the amount of charge transferred by the dissolved metal particle per unit time, M represents the relative atomic mass of the metal particle (kg / mol), n represents the number of charges transferred when the metal particle dissolves, and F is the Faraday constant 96500 C / mol.

[0134] In the technical solution of this application embodiment, charge transfer occurs during the dissolution process of metal particles. Therefore, the amount of transferred charge dissolved by the metal particles per unit time can be determined first based on the current dissolution current. Then, based on the amount of transferred charge, the current dissolution mass of the metal particles per unit time can be accurately determined, ensuring the accuracy of the determined current dissolution mass. This, in turn, ensures the accuracy of the cumulative dissolution time consumed by the dissolution of metal particles, and more effectively alleviates the problem of low screening accuracy of batteries with metal impurities.

[0135] According to some embodiments of this application, the current radius of the metal particle at the end of the current unit time can be determined by combining the current dissolved mass and the remaining mass in the previous unit time. That is, the above step "determining the current radius of the metal particle at the end of the current unit time based on the current dissolved mass" can be achieved through the following steps:

[0136] Step 1: Determine the current remaining mass of the metal particles based on the current dissolved mass and the remaining mass in the previous unit of time.

[0137] It should be noted that the current dissolved mass refers to the mass of metal particles dissolved within the current unit of time. Therefore, the current remaining mass of the metal particles can be obtained by subtracting the current dissolved mass from the remaining mass in the previous unit of time. Specifically, the current remaining mass of the metal particles refers to the mass of the metal particles remaining at the end of the current unit of time after dissolution within the current unit of time.

[0138] In practical applications, the current remaining mass of the metal particles can be determined using the following formula (4):

[0139] m = m1 - dm (4)

[0140] Where m represents the current remaining mass (kg) of the metal particles, m1 represents the remaining mass (kg) of the previous unit time, and dm represents the current dissolved mass (kg).

[0141] Step 2: Based on the current remaining mass, determine the current radius of the metal particle at the cutoff time of the current unit of time.

[0142] It should be noted that the current remaining mass of the metal particle refers to the mass remaining in the metal particle at the end of the current unit of time. Therefore, based on the current remaining mass, the current radius of the metal particle at the end of the current unit of time can be determined.

[0143] In practical applications, the current radius of a metal particle at the cutoff time of the current unit of time can be determined using the following formula (5):

[0144]

[0145] Where r represents the current radius of the metal particle at the current unit time cutoff point, m represents the current remaining mass (kg), and ρ represents the density of the metal particle (kg / m³). 3 ).

[0146] In the technical solution of this application embodiment, the determined current dissolution mass is the mass of metal particles dissolved in the current unit time. Therefore, based on the current dissolution mass and the remaining mass in the previous unit time, the current remaining mass of the metal particles can be determined, thereby accurately determining the current radius of the metal particles at the end of the current unit time. This ensures the accuracy of the determined current radius of the metal particles at the end of the current unit time, and further ensures the accuracy of the cumulative dissolution time consumed by the dissolution of metal particles, thus more effectively alleviating the problem of low screening accuracy of batteries with metal impurities.

[0147] According to some embodiments of this application, a preset oxidation current density table can also be constructed in advance based on the test battery and the reference battery. That is, before the above step "obtain the corresponding target oxidation current density from the preset oxidation current density table according to the attribute parameters and aging parameters", the following steps can also be included:

[0148] Step 1: Based on the test temperature group and the test voltage group, perform charging tests on the test battery and the reference battery to determine the oxidation current density corresponding to different test temperatures and different test voltages. The test temperature group includes at least one test temperature, and the test voltage group includes at least one test voltage.

[0149] Among them, the test battery refers to the battery with metal particles, which serves as the test group; the reference battery refers to the battery without metal particles, which serves as the reference group.

[0150] It should be noted that the test temperature group is a pre-set set including at least one test temperature, and the test voltage group is a pre-set set including at least one test voltage. In one possible implementation, the interval between every two test temperatures in the test temperature group is the same, that is, a test temperature is set at equal intervals; similarly, the interval between every two test voltages in the test voltage group is the same, that is, a test voltage is set at equal intervals. The step method is used to test the oxidation current density at different test temperatures and different test voltages.

[0151] As an example, the test temperature can be set to 10-60℃, with each 5℃ increment representing a gradient, i.e., the test temperature group is “10, 15, 20…55, 60℃”; the test voltage can be set to 3.1-4.0V, with each 0.1V increment representing a gradient, i.e., the test voltage group is “3.1, 3.2, 3.3…3.9, 4.0V”.

[0152] In practical applications, the test battery and the reference battery can be placed in a high-low temperature chamber and allowed to stand for 1 hour to allow their temperatures to equalize with the chamber temperature. The test temperatures are 10–60°C, with each 5°C increment representing a gradient. A constant voltage charge is applied for 30 seconds using an electrochemical workstation, with the test voltage ranging from 3.1–4.0V, with each 0.1V increment representing a gradient. The current value at each test voltage and temperature after 30 seconds is recorded. The same test procedure is used for both the test battery and the reference battery, and the current difference over 30 seconds is taken as the oxidation current of the metal particles.

[0153] Step 2: Construct a preset oxidation current density table based on the oxidation current density corresponding to different test temperatures and test voltages.

[0154] In the technical solution of this application embodiment, the corresponding oxidation current density can be determined under different test temperatures and different test voltages. The calculation of oxidation current density involves attribute parameters such as the density and surface area of ​​metal particles. Therefore, after determining the oxidation current density corresponding to different test temperatures and different test voltages, the attribute parameters of the metal particles used, the test temperature, and the test voltage can be stored to construct a preset oxidation current density table. This facilitates the subsequent direct acquisition of the corresponding target oxidation current density from the preset oxidation current density table based on the obtained attribute parameters and aging parameters of the metal particles. This accurately determines the current dissolution current of the metal particles per unit time, ensuring the accuracy of the determined current dissolution current. Consequently, it ensures the accuracy of the cumulative dissolution time consumed by the dissolution of metal particles, and more effectively alleviates the problem of low screening accuracy of batteries with metal impurities.

[0155] According to some embodiments of this application, for a certain test temperature, the test battery and the reference battery can be charged sequentially using each test voltage in the test voltage group. That is, the above step "to charge the test battery and the reference battery according to the test temperature group and the test voltage group, and determine the oxidation current density corresponding to different test temperatures and different test voltages" can be achieved through the following steps:

[0156] Step S1: Select the first test temperature from the test temperature group.

[0157] Step S2: At the first test temperature, the test battery and the reference battery are charged sequentially using each test voltage in the test voltage group to determine the oxidation current density corresponding to each test voltage at the first test temperature.

[0158] Step S3: Take any other test temperature in the test temperature group as the first test temperature, replace the test battery and the reference battery, and return to the operation steps of S2 until all test temperatures in the test temperature group have been tested, and obtain the oxidation current density corresponding to different test temperatures and different test voltages.

[0159] It should be noted that each test temperature can correspond to a set of test voltages. After the test voltage of a set of test voltages at a test temperature is completed, before testing the next test temperature, the test battery and reference battery can be replaced because the metal particles in the test battery have dissolved, and then the test at the next test temperature can continue.

[0160] In the technical solution of this application embodiment, for a certain test temperature, the test battery and the reference battery can be charged and tested sequentially using each test voltage in the test voltage group to determine the oxidation current density corresponding to each test voltage at the first test temperature. Then, the above process is repeated for the next test temperature in the test temperature group until the oxidation current density corresponding to different test voltages at different test temperatures is obtained. The oxidation current density corresponding to different test voltages at different test temperatures is pre-measured, and a preset oxidation current density table is constructed. This facilitates the direct acquisition of the corresponding target oxidation current density from the preset oxidation current density table based on the obtained attribute parameters and aging parameters of the metal particles, so as to accurately determine the current dissolution current of the metal particles per unit time. This ensures the accuracy of the determined current dissolution current, thereby ensuring the accuracy of the cumulative dissolution time consumed by the dissolution of metal particles, and more effectively alleviating the problem of low screening accuracy of problematic batteries with metal impurities.

[0161] According to some embodiments of this application, at the first test temperature, the test battery and the reference battery can be charged and tested sequentially using various test voltages. The above step S2 can be implemented by the following steps S21-S25:

[0162] Step S21: Select the first test voltage from the test voltage group.

[0163] Step S22: After charging the test battery at a constant voltage for a preset time using the first test voltage, obtain the test current corresponding to the first test voltage, and after charging the reference battery at a constant voltage for a preset time using the first test voltage, obtain the reference current corresponding to the first test voltage.

[0164] Specifically, the preset duration refers to the pre-set charging test time period, such as 30 seconds, 40 seconds, etc.

[0165] It should be noted that the test battery and the reference battery can be charged at a constant voltage for 30 seconds at the first test temperature and the first test voltage, respectively. The test current can be measured based on the test battery, and the reference current can be measured based on the reference battery.

[0166] Step S23: Determine the oxidation current corresponding to the first test temperature and the first test voltage based on the test current and the reference current.

[0167] It should be noted that under different test temperatures and test voltages, metal particles will undergo oxidation reaction, i.e. charge transfer, at the positive electrode. The positive electrode of the test battery contains metal particles, while the positive electrode of the reference battery does not contain metal particles. Therefore, the oxidation current generated by the dissolution of metal particles can be obtained by subtracting the reference current from the test current. The corresponding oxidation current density can then be calculated based on the oxidation current.

[0168] In practical applications, the selection of the test voltage range is mainly based on the commonly used aging voltage range of full cells. When calculating the dissolution time of metal particles, the full cell voltage can be directly input. The selection of the test temperature range is mainly based on the temperature selection of existing aging processes, but is increased to 60℃ to explore the feasibility of shortening the aging time at higher temperatures.

[0169] S24: Obtain the property parameters of the metal particles set in the test battery, and determine the oxidation current density corresponding to the first test temperature and the first test voltage based on the property parameters and the oxidation current.

[0170] It should be noted that different metal particles have different property parameters, which may refer to parameters such as the density, mass and surface area of ​​the metal particles. Based on the obtained property parameters and the calculated oxidation current, the oxidation current density corresponding to the first test temperature and the first test voltage can be determined.

[0171] In practical applications, the specific surface area S0 (m²) of metal particles can be measured using scanning electron microscopy (SEM-EDS). 2 / kg), combining the mass m (kg) and density ρ (kg / m) of the metal particles 3 The oxidation current density per unit area of ​​the metal particles is calculated using the following formula (6):

[0172]

[0173] Where j represents the oxidation current density, i represents the oxidation current, and ρ represents the density of the metal particles (kg / m³). 3 S0 represents the specific surface area (m²) of the metal particles. 2 / kg), where m represents the mass (kg) of the metal particles.

[0174] In practice, the surface area and diameter of metal particles are measured using a scanning electron microscope (SEM-EDS). Specifically, conductive adhesive is attached to the SEM-EDS sample stage, a small amount of metal particles are picked up with a toothpick and placed near the conductive adhesive, and then blown onto the conductive adhesive with compressed gas to disperse the metal particles and avoid test deviations caused by the accumulation and overlap of metal particles.

[0175] As an example, taking iron (Fe) metal particles as an example, scanning electron microscopy (SEM-EDS) was used to scan the iron metal particles. Figure 3 Optical photographs of iron metal particles provided in some embodiments of this application. Figure 4 For particle size distribution diagrams of iron metal particles provided in some embodiments of this application, please refer to... Figure 3The diameter of the Fe particles is [0.1070 mm]. Based on scanning electron microscopy (SEM-EDS) of the iron particles, the attribute parameters shown in Table 1 below can be obtained.

[0176] Table 1 Property parameters of Fe metal particles

[0177]

[0178] S25: Take any other test voltage in the test voltage group as the first test voltage, and return to the operation step of S22 until all test voltages in the test voltage group have been tested, and obtain the oxidation current density corresponding to each test voltage at the first test temperature.

[0179] It should be noted that after one test voltage is completed, before testing the next test voltage, the test battery and reference battery can be replaced, or they can remain in place and be replaced after all test voltages at the first test temperature are tested.

[0180] In the technical solution of this application embodiment, for a certain test temperature, a test voltage can be selected from the test voltage group to perform a charging test on the test battery and the reference battery. Based on the test current and the reference current, the oxidation current is determined. Then, based on the property parameters of the metal particles and the oxidation current, the oxidation current density corresponding to the test voltage at the test temperature is determined. Then, at the test temperature, the above process is repeated for the next test voltage in the test voltage group until the oxidation current density corresponding to each test voltage at the test temperature is obtained. By performing the above process for each test temperature, the oxidation current density corresponding to different test voltages at different test temperatures can be measured in advance, and a preset oxidation current density table can be constructed. This makes it convenient to directly obtain the corresponding target oxidation current density from the preset oxidation current density table based on the obtained property parameters and aging parameters of the metal particles, so as to accurately determine the current dissolution current of the metal particles in the current unit time, ensuring the accuracy of the determined current dissolution current, and thus ensuring the accuracy of the cumulative dissolution time consumed by the dissolution of metal particles, and more effectively alleviating the problem of low screening accuracy of problematic batteries with metal impurities.

[0181] According to some embodiments of this application, test batteries and reference batteries can also be prepared in advance. That is, before the above-mentioned step "conducting charging tests on test batteries and reference batteries according to test temperature groups and test voltage groups to determine the oxidation current density corresponding to different test temperatures and different test voltages", the following steps can also be included:

[0182] Step 1: Prepare experimental batteries using positive electrode materials, metal particles, and negative electrode materials;

[0183] Step 2: Prepare a reference battery using positive and negative electrode materials.

[0184] In the technical solution of this application embodiment, a test battery can be prepared in advance using positive electrode material, metal particles, and negative electrode material, and a reference battery can be prepared using positive electrode material and negative electrode material. That is, the positive electrode material of the test battery incorporates metal particles, while the reference battery does not incorporate metal particles. This allows for comparison of the test current and the reference current to determine the oxidation current, providing a data basis for subsequently determining the current radius of the metal particles at the current unit time cutoff time. This ensures the accuracy of the cumulative dissolution time consumed by the metal particles and more effectively alleviates the problem of low screening accuracy of batteries with incorporated metal impurities.

[0185] According to some embodiments of this application, test batteries can be pre-prepared based on a sandwich structure, that is, the above step "preparing test batteries using positive electrode materials, metal particles, and negative electrode materials" can be achieved through the following steps:

[0186] Step 1: Coat the positive electrode slurry onto the current collector, and weigh out a set mass of metal particles and place them on the surface of the positive electrode slurry. The positive electrode slurry is obtained by mixing positive electrode materials according to a set ratio.

[0187] Among them, the current collector refers to the structure or component that collects current. In lithium-ion batteries, it mainly refers to metal foil, such as copper foil and aluminum foil.

[0188] It should be noted that the cathode material can be a ternary material, such as lithium iron phosphate, lithium cobalt oxide, lithium manganese oxide, etc. (e.g., NCM811), with the addition of binder PVDF (polyvinylidene fluoride) and conductive carbon (SP), mixed in a certain proportion to form a cathode slurry. For example, NCM811:SP:PVDF = 96:2:2 mass ratio can be used to mix and form a cathode slurry.

[0189] In addition, metal particles include, but are not limited to, copper, iron, stainless steel, nickel, zinc, and aluminum. The set mass of implanted metal particles should not be too small, otherwise the difference in current between the reference cell and the test cell without implanted metal particles will be small, resulting in a large relative error; the set mass of implanted metal particles should not be too large either, otherwise particle aggregation and accumulation will occur, which will scratch the scraper during the second coating and result in uneven coating.

[0190] Step 2: After the positive electrode slurry dries, the positive electrode slurry is coated again to obtain the positive electrode sheet.

[0191] In practical applications, PVDF can be added to NMP (N-methylpyrrolidone) solution and stirred continuously until PVDF is completely dissolved. Then SP is added and stirred to disperse. Finally, the positive electrode active material LiNi0.8Co0.1Mn0.1O2 (hereinafter referred to as NCM811) is added and stirred to disperse evenly. The mass ratio of NCM811:SP:PVDF is 96:2:2.

[0192] Then, using Al (aluminum) as the current collector, the stirred positive electrode slurry was directly coated onto a 12µm aluminum foil using a 50µm scraper. 0.5mg of metal particles were weighed and evenly sprinkled onto the surface of the positive electrode slurry using a sieve. After drying at 100℃ under forced air conditions for 6 hours, the positive electrode slurry was coated again using a 200µm scraper. After vacuum drying at 100℃ for 12 hours, it was punched into a positive electrode sheet with a diameter of 16mm for later use.

[0193] As an example, Figure 5 For schematic diagrams of the positive electrode structure provided in some embodiments of this application, please refer to... Figure 5 The positive electrode material is coated on the Al current collector, and the metal particles are located between the two layers of positive electrode material, forming a sandwich structure.

[0194] Step 3: Prepare the test battery using the positive electrode and the pre-made negative electrode.

[0195] In practical applications, PVDF can be added to an NMP (N-methylpyrrolidone) solution and stirred continuously until the PVDF is completely dissolved. Then, graphite is added and stirred to disperse it. The mass ratio of graphite to PVDF is 98:2. The stirred negative electrode slurry is directly coated onto an 8µm Al foil using a scraper. After drying under vacuum at 100°C for 6 hours, it is punched into 18mm small round sheets for use as negative electrode sheets.

[0196] It should be noted that after preparing the positive and negative electrode sheets, a test battery can be assembled. During battery assembly, graphite is used as the negative electrode, and a coin cell is assembled inside a glove box (water and oxygen content <0.1ppm). Specifically, the negative electrode shell, negative electrode sheet, separator, positive electrode sheet, gasket, spring, and positive electrode shell are placed in sequence. During placement, 120µL of electrolyte is added dropwise, compacted, and then sealed with an aluminum-plastic film. After standing for 2 hours, a test battery is prepared, and its cycle performance is tested.

[0197] In addition, the positive electrode coating steps, negative electrode coating steps, and assembly steps of the reference battery are the same as those of the above-mentioned test battery, but there is no metal implantation step.

[0198] In the technical solution of this application embodiment, a layer of positive electrode slurry can be coated first, and a certain amount of metal particles can be placed on the positive electrode slurry. Then, a layer of positive electrode slurry is coated again to wrap the metal particles. A sandwich structure is adopted to integrate the metal particles into the positive electrode material, simulating the situation where metal particles are mixed into the positive electrode material in a real scenario. This makes the metal particles mixed in the test battery closer to the real scenario, rather than located on the surface of the positive electrode material. This ensures the accuracy of the current radius of the determined metal particles at the current unit time cutoff time, thereby ensuring the accuracy of the cumulative dissolution time consumed by the dissolution of metal particles. This more effectively alleviates the problem of low screening accuracy of batteries with metal impurities.

[0199] According to some embodiments of this application, after determining the corresponding cumulative dissolution time based on the input attribute parameters and aging parameters, the time can be stored accordingly. That is, after step 106 above, the following steps can be included:

[0200] The property parameters, aging parameters, and corresponding cumulative dissolution time of the metal particles are stored accordingly.

[0201] As an example, Figure 6(a) shows the cumulative dissolution time at 25°C for different voltages provided in some embodiments of this application, and Figure 6(b) shows the cumulative dissolution time at 45°C for different voltages provided in some embodiments of this application. Please refer to... Figure 6(a) and 6(b) The higher the voltage, the shorter the cumulative dissolution time required.

[0202] In the technical solution of this application embodiment, after determining the cumulative dissolution time consumed by the dissolution of metal particles, the attribute parameters of the metal particles, the aging parameters used, and the corresponding cumulative dissolution time can be stored accordingly. Subsequently, when aging the battery to be tested, the corresponding aging parameters and the corresponding cumulative dissolution time can be selected according to the requirements. If metal particles are incorporated into the battery to be tested, it can be ensured that they are accurately detected during the aging stage, thereby improving the screening accuracy of problematic batteries with incorporated metal impurities.

[0203] Please refer to Figure 7 , Figure 7 A flowchart illustrating another method for determining the dissolution time of metal particles in a battery, as provided in some embodiments of this application, is shown below. Figure 7 As shown, this includes the following steps 702-720:

[0204] Step 702: Input the particle type, particle radius, aging voltage and aging temperature of the metal particles. Based on the above conditions, obtain the corresponding target oxidation current density from the preset oxidation current density table.

[0205] Step 704: Obtain the particle radius at the cutoff time of the previous unit of time, and determine the current surface area of ​​the metal particle based on the particle radius at the cutoff time of the previous unit of time.

[0206] Step 706: Determine the current dissolution current of the metal particles per unit time based on the target oxidation current density and the current surface area of ​​the metal particles.

[0207] Step 708: Determine the amount of transferred charge of metal particles dissolved per unit time based on the current dissolution current.

[0208] Step 710: Determine the current dissolved mass of metal particles per unit time based on the amount of transferred charge.

[0209] Step 712: Determine the current remaining mass of the metal particles based on the current dissolved mass and the remaining mass in the previous unit of time.

[0210] Step 714: Based on the current remaining mass, determine the current radius of the metal particle at the cutoff time of the current unit of time.

[0211] Step 716: Accumulate the unit time to obtain the cumulative dissolution time.

[0212] Step 718: Determine whether the current radius is less than or equal to a predetermined threshold. If yes, proceed to step 720 below. If no, return to step 704 above.

[0213] Step 720: Output the cumulative dissolution time.

[0214] It should be noted that steps 702-720 above are models built to determine the dissolution time of metal particles in the battery. By programming, the particle type, particle radius, aging voltage and aging temperature of the metal particles are input, and the corresponding cumulative dissolution time can be output.

[0215] In practical applications, the above model essentially differentiates the metal particle dissolution process over time to obtain the cumulative dissolution time required for the metal particles to dissolve. That is, the model primarily treats the metal particles as equivalent to metal spheres; when the diameter of the spherical metal particle is d, the particle volume is... The time element dt has the following formula (7), and the cumulative dissolution time under the input conditions can be obtained based on the following formula (7):

[0216]

[0217] Where ρ represents the density of the metal particles (kg / m³) 3D is the diameter of the metal particle, n represents the charge transferred during metal dissolution, F is the Faraday constant 96500 C / mol, M represents the relative atomic mass of the metal particle (kg / mol), j represents the target oxidation current, and S represents the specific surface area of ​​the metal particle (m²). 2 / kg).

[0218] It should be noted that the preset oxidation current density table can be pre-prepared based on test and reference batteries. The test battery can use a sandwich structure to set metal particles, simulating the real state of metal particles mixed into the cathode material. The oxidation current density of metal particles at different temperatures and voltages is measured using a temperature and voltage step method to construct the preset oxidation current density table. Subsequently, a metal oxidation dissolution model can be established. Based on given property parameters and aging parameters, the corresponding target oxidation current density can be determined, thereby estimating the time required for metal particles to dissolve at different temperatures and voltages, predicting the time when risks will occur, and guiding the aging process of the battery under test in the factory, such as voltage, temperature, and time. This ensures that some metal particles can completely dissolve during the aging process, causing a short circuit, and can then be detected in the subsequent detection process, preventing undissolved metal particles from leaving the factory and causing safety hazards.

[0219] Please refer to Figure 8 , Figure 8 Flowcharts of detection methods for batteries to be tested provided in some embodiments of this application, such as Figure 8 As shown, the steps include 802-806:

[0220] Step 802: Obtain the attribute parameters, aging parameters and corresponding estimated dissolution time of the battery to be tested, wherein the estimated dissolution time is determined according to the method for determining the dissolution time of metal particles in the battery described above.

[0221] It should be noted that the attribute parameters of the battery under test can be parameters such as the type and radius of the metal particles to be tested, and the aging parameters can be aging voltage and aging temperature. In practical applications, the attribute parameters, aging parameters, and corresponding estimated dissolution time of the battery under test can be determined. This estimated dissolution time can be determined based on the method for determining the dissolution time of metal particles in the battery described above. If the metal particles are incorporated into the battery under test, they can dissolve and be detected after the estimated dissolution time.

[0222] Step 804: Use aging parameters to estimate the dissolution time of the battery under test.

[0223] Step 806: After estimating the dissolution time during aging, determine the voltage drop of the battery to be tested, and determine whether the battery to be tested is a problem battery based on the voltage drop.

[0224] In the technical solution of this application embodiment, the attribute parameters, aging parameters and corresponding estimated dissolution time of the battery to be tested can be obtained. The estimated dissolution time is determined based on the method for determining the dissolution time of metal particles in the battery. The method can accurately determine the dissolution time of metal particles incorporated into the battery under a certain aging parameter. Therefore, the determined cumulative dissolution time can be used as the estimated dissolution time. The battery to be tested is aged using the corresponding aging parameters. If the metal particles are incorporated into the battery to be tested, it can be accurately detected during the aging stage, thus improving the screening accuracy of problematic batteries with incorporated metal impurities.

[0225] According to some embodiments of this application, the battery under test can be tested based on the voltage difference after being left to stand for a period of time. That is, step 806 above can be achieved through the following steps:

[0226] Step 1: After estimating the dissolution time during aging, let the battery under test stand for a first preset time and obtain the first voltage of the battery under test.

[0227] Step 2: Let the battery under test stand for a second preset time and obtain the first voltage of the battery under test, wherein the second preset time is longer than the first preset time.

[0228] It should be noted that the first and second preset durations can be set in advance based on the needs of the actual scenario. The second preset duration should be longer than the first preset duration to determine the voltage difference between the first and second preset durations of resting the battery under test, thereby determining whether the battery under test is a problematic battery. For example, the first preset duration can be 2 days, and the second preset duration can be 5 days.

[0229] Step 3: Use the voltage difference between the first voltage and the second voltage as the voltage drop.

[0230] Step 4: If the voltage drop exceeds a preset threshold, the battery under test is determined to be a problematic battery.

[0231] In the technical solution of this application embodiment, the voltage difference between the battery under test after a first preset resting time and a second preset resting time can be determined. If the voltage difference is too large, it indicates that metal particles have been incorporated into the battery under test, and the battery is a problematic battery. If the voltage difference is small, it indicates that no metal particles have been incorporated into the battery under test, and the battery is a safe battery. Thus, when the accuracy of the estimated dissolution time is high, the voltage difference before and after aging of the battery under test can be used to accurately determine whether the battery under test is a problematic battery, improving the screening accuracy of problematic batteries with incorporated metal impurities.

[0232] According to some embodiments of this application, the battery to be tested is prepared from a casing and at least one cell assembly. The cell assembly is a lithium-ion cell, which is prepared from a positive electrode, a negative electrode, an electrolyte, a separator, a casing, and terminals. The battery to be tested is performed using determined aging parameters and an estimated dissolution time. If the metal particles are incorporated into the battery, accurate detection during the aging stage can be guaranteed, improving the screening accuracy of problematic batteries with incorporated metal impurities.

[0233] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of this application, and not to limit them. Although this application has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features therein. These modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of this application, and they should all be covered within the scope of the claims and specification of this application. In particular, as long as there is no structural conflict, the various technical features mentioned in the embodiments can be combined in any way. This application is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims.

Claims

1. A method for determining the dissolution time of metal particles in a battery, characterized in that, include: Obtain the property parameters and aging parameters of the metal particles, and determine the corresponding target oxidation current density based on the property parameters and aging parameters; Using a unit time as the period, the current radius of the metal particle at the cutoff time of the current unit time is determined based on the target oxidation current density, and the unit time is accumulated to obtain the cumulative dissolution time; Based on the current radius, determine whether the metal particles have completely dissolved. If the metal particles have completely dissolved, output the cumulative dissolution time. The step of determining the corresponding target oxidation current density based on the attribute parameters and the aging parameters includes: obtaining the corresponding target oxidation current density from a preset oxidation current density table based on the attribute parameters and the aging parameters. Before obtaining the corresponding target oxidation current density from the preset oxidation current density table based on the attribute parameters and the aging parameters, the method further includes: performing charging tests on the test battery and the reference battery according to the test temperature group and the test voltage group to determine the oxidation current density corresponding to different test temperatures and different test voltages, wherein the test temperature group includes at least one test temperature and the test voltage group includes at least one test voltage; and constructing the preset oxidation current density table based on the oxidation current densities corresponding to different test temperatures and different test voltages. Among them, the test battery refers to a battery with metal particles; the reference battery refers to a battery without metal particles. Among them, the test current can be measured based on the test battery, and the reference current can be measured based on the reference battery; The oxidation current generated by the dissolution of metal particles can be obtained by subtracting the reference current from the test current. Based on the oxidation current, the corresponding oxidation current density can be calculated.

2. The determination method as described in claim 1, characterized in that, The step of determining the current radius of the metal particle at the cutoff time of the current unit time based on the target oxidation current density includes: Based on the target oxidation current density, determine the current dissolution current of the metal particles per unit time. Based on the current dissolution current, determine the current dissolution mass of the metal particles per unit time. Based on the current dissolved mass, determine the current radius of the metal particle at the cutoff time of the current unit of time.

3. The determination method as described in claim 2, characterized in that, Determining the current dissolution current of the metal particles per unit time based on the target oxidation current density includes: Obtain the particle radius at the cutoff time of the previous unit of time for the metal particle, and determine the current surface area of ​​the metal particle based on the particle radius at the cutoff time of the previous unit of time. The current dissolution current of the metal particles per unit time is determined based on the target oxidation current density and the current surface area of ​​the metal particles.

4. The determination method as described in claim 2, characterized in that, Determining the current dissolved mass of the metal particles per unit time based on the current dissolution current includes: Based on the current dissolution current, determine the amount of transferred charge dissolved by the metal particles per unit time. The current dissolved mass of the metal particle per unit time is determined based on the amount of transferred charge.

5. The determination method as described in claim 2, characterized in that, Determining the current radius of the metal particle at the cutoff time of the current unit time based on the current dissolved mass includes: The current remaining mass of the metal particles is determined based on the current dissolved mass and the remaining mass in the previous unit time. Based on the current remaining mass, determine the current radius of the metal particle at the cutoff time of the current unit of time.

6. The determination method as described in claim 1, characterized in that, The process of performing charging tests on the test battery and the reference battery according to the test temperature group and the test voltage group to determine the oxidation current density corresponding to different test temperatures and different test voltages includes: S1: Select a first test temperature from the test temperature group; S2: At the first test temperature, the test battery and the reference battery are charged sequentially using each test voltage in the test voltage group to determine the oxidation current density corresponding to each test voltage at the first test temperature; S3: Take any other test temperature in the test temperature group as the first test temperature, replace the test battery and the reference battery, and return to the operation step of S2 until all test temperatures in the test temperature group have been tested, and obtain the oxidation current density corresponding to different test temperatures and different test voltages.

7. The determination method as described in claim 6, characterized in that, The step of sequentially charging the test battery and the reference battery using each test voltage in the test voltage group to determine the oxidation current density corresponding to each test voltage at the first test temperature includes: S21: Select a first test voltage from the test voltage group; S22: After charging the test battery at a constant voltage for a preset time using the first test voltage, obtain the test current corresponding to the first test voltage, and after charging the reference battery at a constant voltage for a preset time using the first test voltage, obtain the reference current corresponding to the first test voltage. S23: Determine the oxidation current corresponding to the first test voltage at the first test temperature based on the test current and the reference current; S24: Obtain the property parameters of the metal particles set in the test battery, and determine the oxidation current density corresponding to the first test temperature and the first test voltage based on the property parameters and the oxidation current; S25: Take any other test voltage in the test voltage group as the first test voltage, and return to execute the operation step of S22 until all test voltages in the test voltage group have been tested, and obtain the oxidation current density corresponding to each test voltage at the first test temperature.

8. The determination method as described in claim 1, characterized in that, Before determining the oxidation current density corresponding to different test temperatures and test voltages by performing charging tests on the test battery and reference battery according to the test temperature group and test voltage group, the method further includes: The experimental battery was prepared using positive electrode material, metal particles, and negative electrode material. The reference battery was prepared using positive and negative electrode materials.

9. The determination method as described in claim 8, characterized in that, The experimental battery is prepared using a positive electrode material, metal particles, and a negative electrode material, comprising: A positive electrode slurry is coated onto a current collector, and a set mass of metal particles is weighed and placed on the surface of the positive electrode slurry. The positive electrode slurry is obtained by mixing the positive electrode materials according to a set ratio. After the positive electrode slurry is dried, it is coated again to obtain a positive electrode sheet; The experimental battery was prepared using the positive electrode and the pre-made negative electrode.

10. The determining method according to any one of claims 1-7, characterized in that, After outputting the cumulative dissolution time, the method further includes: The property parameters, aging parameters, and corresponding cumulative dissolution time of the metal particles are stored accordingly.

11. A method for detecting a battery to be tested, characterized in that, include: Obtain the attribute parameters, aging parameters and corresponding estimated dissolution time of the battery to be tested, wherein the estimated dissolution time is determined according to the method for determining the dissolution time of metal particles in the battery according to any one of claims 1-10. The estimated dissolution time of the battery under test is determined by aging the battery using the aforementioned aging parameters. After aging the estimated dissolution time, the voltage drop of the battery under test is determined, and the battery under test is determined to be a problematic battery based on the voltage drop.

12. The detection method as described in claim 11, characterized in that, After the estimated dissolution time is reached during aging, the voltage drop of the battery under test is determined, and the battery under test is determined to be a problematic battery based on the voltage drop, including: After the estimated dissolution time is aged, the battery to be tested is left to stand for a first preset time, and the first voltage of the battery to be tested is obtained. The battery to be tested is left to stand for a second preset time, and the second voltage of the battery to be tested is obtained, wherein the second preset time is longer than the first preset time. The voltage difference between the first voltage and the second voltage is taken as the voltage drop; If the voltage drop exceeds a preset threshold, the battery under test is determined to be a problematic battery.

13. The detection method as described in claim 11 or 12, characterized in that, The battery to be tested is made from a casing and at least one cell assembly. The cell assembly is a lithium-ion cell and is made from a positive electrode, a negative electrode, an electrolyte, a separator, a shell, and terminals.

Citation Information

Patent Citations

  • Method and device for detecting lithium precipitation of battery

    CN112151899A

  • Positive electrode active material, positive electrode, and lithium ion secondary battery

    JP2004259518A