A method and system for hardness evaluation correction of carbon steel joint considering welding thermal cycle
By obtaining the residual plastic strain and dislocation density of carbon steel welded joints, and combining the recovery recrystallization phenomenon of welding thermal cycle, the dislocation density is corrected to evaluate the hardness value, which solves the problem of inaccurate evaluation in the prior art and achieves higher precision hardness evaluation.
Patent Information
- Application Number
- CN202310372416.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-03
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-04-03
AI Technical Summary
Existing technologies cannot accurately assess the hardness of carbon steel welded joints, especially failing to consider the welding thermal cycle process and its impact on dislocation density.
By obtaining the residual plastic strain value of the carbon steel welded joint, the dislocation density is calculated, and the dislocation density is corrected by considering the recovery recrystallization phenomenon of the welding thermal cycle, and finally the hardness value is calculated.
The accuracy of hardness assessment for carbon steel welded joints has been improved by taking into account the softening effect of welding thermal cycles and the influence of recovery recrystallization, thus enhancing the accuracy of the assessment.
Smart Images

Figure CN116776663B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of welded joint hardness assessment technology, and more specifically, to a method and system for correcting the hardness assessment of carbon steel joints taking into account welding thermal cycles. Background Technology
[0002] Carbon steel, as a commonly used metal in large steel structures such as ships, marine structures, and bridges, possesses excellent mechanical properties and cost-effectiveness. Meanwhile, fusion welding, an important welding method for joining carbon steel metals, involves the localized and rapidly moving electric arc causing the carbon steel to melt and form a molten pool; subsequent cooling and solidification result in atomic bonding between the welded components. The hardness of carbon steel welded joints, a common mechanical property parameter, is often evaluated through testing machined specimens; it can also be predicted and analyzed using the microscopic defects within the carbon steel welded joint, namely dislocation density.
[0003] Specifically, the residual plastic strain after welding carbon steel joints is the fundamental cause affecting the deformation and residual stress of the welded joint. Simultaneously, work hardening alters the dislocation density between metal atoms, which is also an important parameter for analyzing and evaluating the hardness of the welded joint. This method, based on residual plastic strain to obtain the internal dislocation density of the welded joint and thus assess its hardness, is widely used in engineering. However, residual plastic strain only reflects the final result of post-weld cooling and cannot reflect the welding thermal cycle process and its effects, especially the influence of recovery recrystallization on dislocation density, thus failing to accurately assess the hardness value of carbon steel welded joints. Summary of the Invention
[0004] This invention addresses the technical problem in the prior art that it cannot accurately assess the hardness value of carbon steel welded joints.
[0005] This invention provides a method for correcting the hardness assessment of carbon steel joints considering welding thermal cycles, comprising the following steps:
[0006] S1, obtain the residual plastic strain value of carbon steel welded joint;
[0007] S2, calculate the dislocation density at a predetermined location based on the residual plastic strain at that location;
[0008] S3, considering the recovery recrystallization phenomenon of welding thermal cycle, the dislocation density at different times is corrected;
[0009] S4, the hardness value is calculated based on the corrected dislocation density.
[0010] Preferably, the formula for calculating the dislocation density in S2 is as follows:
[0011] t=(211×ε P +1.42)×1013
[0012] Where t is the dislocation density, ε P This is plastic strain.
[0013] Preferably, the formula for calculating the hardness Y in S4 is as follows:
[0014] t=(211×ε P +1.42)×10 13
[0015] HV = 2.4 × t / 10 13 +200
[0016] Where t is the dislocation density and HV is the hardness.
[0017] Preferably, S1 specifically includes:
[0018] Thermocouple strain gauge tests or thermo-elastic-plastic finite element analysis were used to obtain the thermal cycling curve of the entire welding area, including the location, and the corresponding plastic strain values at different times. The plastic strain under thermal cycling at different times was then discretized.
[0019] Preferably, S3 specifically includes:
[0020] S31, using t i Dislocation density t at time t ia Compared to the previous moment t i-1 dislocation density change t (i-1)b The difference is used as the dislocation density t after the first correction at the current moment. ic Where i is a natural number greater than 1;
[0021] S32, calculate the time interval (t) based on the dislocation density and its first correction value. i-1 , t i The first dislocation density recovery rate r1:
[0022]
[0023] t constant The dislocation density constant under no plastic strain is 1.42 × 10⁻⁶. 13 ;
[0024] S33, calculate the first recovery recrystallization parameter c1.
[0025]
[0026] Where n is the recrystallization index of carbon steel, with a value of 0.249;
[0027] S34, based on the Arrhenius formula, calculate the second recovery recrystallization parameter c2:
[0028]
[0029] Where K0 is the recrystallization constant, 8.38 × 10⁻⁶. 8 Q is the heat of reaction, which represents the heat released or absorbed by a certain amount of substance in a reaction, with a value of 113.6 kJ / mol; R is the gas constant, with a value of 8.314; Ti is the t... i Temperature at any moment;
[0030] S35, based on the Johnson-Mehl formula, calculate the dislocation density recovery rate r2 of the second correction:
[0031] r2 = 1 - exp(-(c2)) n )
[0032] Where n is the recrystallization index of carbon steel, with a value of 0.249;
[0033] S36, considering the influence of dislocation density recovery rate, i.e., the recovery recrystallization phenomenon, the second corrected dislocation density is as follows: t icc :
[0034] t icc =t ia -r2×(t ia -t constant );
[0035] S37, Calculate t i The change in dislocation density at time t ib :
[0036] t ib =t ia -t icc
[0037] Therefore, for t i+1 The dislocation density at time step is corrected.
[0038] Preferably, after step S37, the method further includes: repeating steps S31 to S37, considering the effect of temperature on dislocation density, until the welding thermal cycle ends and the temperature returns to room temperature, to gradually obtain a second corrected dislocation density.
[0039] Preferably, at the initial time t0, t 0b =0.
[0040] The present invention also provides a carbon steel joint hardness assessment correction system considering welding thermal cycles, the system being used to implement a carbon steel joint hardness assessment correction method considering welding thermal cycles, comprising:
[0041] The residual plastic strain acquisition module is used to acquire the residual plastic strain value of carbon steel welded joints;
[0042] The dislocation density calculation module is used to calculate the dislocation density at a predetermined location based on the residual plastic strain at that location.
[0043] The dislocation density correction module is used to take into account the recovery and recrystallization phenomenon of welding thermal cycle and correct the dislocation density at different times.
[0044] The hardness calculation module is used to calculate the hardness value based on the corrected dislocation density.
[0045] The present invention also provides an electronic device, including a memory and a processor, wherein the processor is used to implement the steps of a method for correcting the hardness assessment of carbon steel joints taking into account welding thermal cycles when executing a computer management program stored in the memory.
[0046] The present invention also provides a computer-readable storage medium having a computer management program stored thereon, which, when executed by a processor, implements the steps of a method for correcting the hardness assessment of carbon steel joints taking into account welding thermal cycles.
[0047] Beneficial Effects: This invention provides a method and system for hardness assessment correction of carbon steel joints considering welding thermal cycles. The method includes: obtaining the residual plastic strain value of the carbon steel welded joint; calculating the dislocation density at a predetermined location based on the residual plastic strain; correcting the dislocation density at different times considering the recovery recrystallization phenomenon of welding thermal cycles; and calculating the hardness value based on the corrected dislocation density. This invention considers the softening effect of thermal cycles during welding and the influence of recovery recrystallization on dislocation density, correcting the shortcomings of commonly used methods that directly calculate dislocation density from plastic strain, and improving the accuracy of assessing the hardness of carbon steel welded joints based on dislocation density. Attached Figure Description
[0048] Figure 1 A flowchart of a method for evaluating and correcting the hardness of carbon steel joints considering welding thermal cycles is provided by the present invention.
[0049] Figure 2 A schematic diagram of the hardware structure of a possible electronic device provided by the present invention;
[0050] Figure 3 A schematic diagram of the hardware structure of a possible computer-readable storage medium provided by the present invention;
[0051] Figure 4 The temperature versus time graph provided for this invention;
[0052] Figure 5 The plastic strain versus time graph provided for this invention;
[0053] Figure 6 This is a comparison diagram of dislocation densities before and after correction provided by the present invention;
[0054] Figure 7 This is a comparison chart of Vickers hardness before and after the correction provided by the present invention. Detailed Implementation
[0055] The specific embodiments of the present invention will be described in further detail below with reference to the accompanying drawings and examples. The following examples are for illustrative purposes only and are not intended to limit the scope of the invention.
[0056] Figure 1 The present invention provides a method for hardness assessment and correction of carbon steel joints considering welding thermal cycles, comprising the following steps:
[0057] S1, obtain the residual plastic strain value of the carbon steel welded joint; obtain the residual plastic strain value of the carbon steel joint through experimental testing or thermo-elastic-plastic finite element analysis.
[0058] S2, based on the residual plastic strain at a predetermined location, calculate the dislocation density at that location; specifically, according to the commonly used hardness assessment method for carbon steel welded joints, calculate the dislocation density at a certain location based on the residual plastic strain at that location, using the following formula:
[0059] t=(211×ε P +1.42)×10 13
[0060] Where t is the dislocation density, ε P This is plastic strain.
[0061] S3, considering the recovery recrystallization phenomenon of welding thermal cycle, the dislocation density at different times is corrected;
[0062] S4, the hardness value is calculated based on the corrected dislocation density. The calculation formula is as follows:
[0063] HV = 2.4 × t' / 10 13 +200
[0064] HV represents hardness, and t' represents the corrected dislocation density.
[0065] In the preferred embodiment, step S1 specifically includes: obtaining the entire welding thermal cycle curve at the location and the value of plastic strain at the corresponding time through thermocouple strain gauge testing or thermo-elastic-plastic finite element analysis, and then discretizing the curve.
[0066] In a preferred embodiment, step S3 further includes: correcting the dislocation density considering the softening effect of the thermal cycling process. The specific correction process is as follows:
[0067] S31, below t i-1 -t i Let's take a time period as an example. For t... i The dislocation density at time t, considering the recovery recrystallization phenomenon of the welding thermal cycle:
[0068] t i The dislocation density t after the first correction at time t ic =t i Dislocation density t at time t ia -t i-1 The change in dislocation density at time t (i-1)b .
[0069] That is, t ic =t ia -t (i-1)b .
[0070] Among them, t ic For t i The dislocation density after the first correction at time t ia For t i Dislocation density at time t (i-1)b For t i-1 The change in dislocation density at time t0. Specifically, at the initial time t0, t... 0b =0.
[0071] S32, calculate the time interval (t) based on the dislocation density and its first correction value. i-1 , t i The first dislocation density recovery rate r1:
[0072]
[0073] t constant The dislocation density constant under no plastic strain is 1.42 × 10⁻⁶. 13 S33, calculate the first recrystallization parameter c1.
[0074]
[0075] Where n is the recrystallization index of carbon steel, with a value of 0.249.
[0076] S34, based on the Arrhenius formula, calculate the second recovery recrystallization parameter c2:
[0077]
[0078] Where K0 is the recrystallization constant, 8.38 × 10⁻⁶. 8 Q is the heat of reaction, which represents the heat released or absorbed by a certain amount of substance in a reaction, with a value of 113.6 kJ / mol; R is the gas constant, with a value of 8.314; Ti is the t... i The temperature of a moment.
[0079] S35, based on the Johnson-Mehl formula, calculate the dislocation density recovery rate r2 of the second correction:
[0080] r2 = 1 - exp(-(c2)) n )
[0081] Where n is the recrystallization index of carbon steel, with a value of 0.249.
[0082] S36, considering the influence of dislocation density recovery rate, i.e., the recovery recrystallization phenomenon, the second corrected dislocation density is as follows: t icc :
[0083] t icc =t ia -r2×(t ia -t constant )
[0084] S37, Calculate t i The change in dislocation density at time t ib :
[0085] t ib =t ia -t icc
[0086] Therefore, for t i+1 The dislocation density at time step is corrected.
[0087] The dislocation density t is adjusted to account for the effects of welding thermal cycling and the phenomenon of recovery recrystallization. icc The hardness was assessed as follows:
[0088]
[0089] Repeat steps S31 to S37 above, that is, consider the effect of temperature on dislocation density, until the welding thermal cycle ends and the temperature returns to room temperature; gradually obtain the second corrected dislocation density, evaluate the hardness change of the welded joint under thermal cycling and the final hardness value.
[0090] In a specific implementation scenario, as follows: Figure 4Taking the welding thermal cycle shown as an example, its highest temperature is 739.34 degrees Celsius, which falls within the heat-affected zone (HAZ) of the weld joint. The resulting plastic strain with temperature changes is as follows: Figure 5 As shown. The dislocation density is directly obtained based on plastic strain, and the dislocation density already considers the effects of welding thermal cycles. The calculation results are comparable to, for example... Figure 6 As shown. The Vickers hardness was evaluated by dislocation density, and its change over time is shown in the figure. Figure 7 As shown.
[0091] The calculation results show that the hardness calculated by the conventional method is 241.68, while the hardness after correction considering the welding thermal cycle effect is 209.04; at the same time, the Vickers hardness test shows that the hardness value at this point is 210.5. It can be seen that the correction method proposed in this patent takes into account the softening effect of welding thermal cycle, which is more accurate and reasonable than the conventional method of evaluating hardness only through plastic strain.
[0092] This invention also provides a carbon steel joint hardness assessment correction system considering welding thermal cycles. The system is used to implement the carbon steel joint hardness assessment correction method considering welding thermal cycles as described above, including:
[0093] The residual plastic strain acquisition module is used to acquire the residual plastic strain value of carbon steel welded joints;
[0094] The dislocation density calculation module is used to calculate the dislocation density at a predetermined location based on the residual plastic strain at that location.
[0095] The dislocation density correction module is used to take into account the recovery and recrystallization phenomenon of welding thermal cycle and correct the dislocation density at different times.
[0096] The hardness calculation module is used to calculate the hardness value based on the corrected dislocation density.
[0097] Please see Figure 2 This is a schematic diagram illustrating an embodiment of the electronic device provided in this invention. For example... Figure 2 As shown, an embodiment of the present invention provides an electronic device, including a memory 1310, a processor 1320, and a computer program 1311 stored in the memory 1310 and executable on the processor 1320. When the processor 1320 executes the computer program 1311, it performs the following steps: S1, obtaining the residual plastic strain value of the carbon steel welded joint.
[0098] S2, calculate the dislocation density at a predetermined location based on the residual plastic strain at that location;
[0099] S3, considering the recovery recrystallization phenomenon of welding thermal cycle, the dislocation density at different times is corrected;
[0100] S4, the hardness value is calculated based on the corrected dislocation density.
[0101] Please see Figure 3 This is a schematic diagram illustrating an embodiment of a computer-readable storage medium provided by the present invention. (See diagram below.) Figure 3 As shown, this embodiment provides a computer-readable storage medium 1400, on which a computer program 1411 is stored. When the computer program 1411 is executed by a processor, it performs the following steps: S1, obtaining the residual plastic strain value of the carbon steel welded joint;
[0102] S2, calculate the dislocation density at a predetermined location based on the residual plastic strain at that location;
[0103] S3, considering the recovery recrystallization phenomenon of welding thermal cycle, the dislocation density at different times is corrected;
[0104] S4, the hardness value is calculated based on the corrected dislocation density.
[0105] It should be noted that the descriptions of each embodiment in the above embodiments have different focuses. For parts that are not described in detail in a certain embodiment, please refer to the relevant descriptions in other embodiments.
[0106] Those skilled in the art will understand that embodiments of the present invention can be provided as methods, systems, or computer program products. Therefore, the present invention can take the form of a completely hardware embodiment, a completely software embodiment, or an embodiment combining software and hardware aspects. Furthermore, the present invention can take the form of a computer program product embodied on one or more computer-usable storage media (including, but not limited to, disk storage, CD-ROM, optical storage, etc.) containing computer-usable program code.
[0107] This invention is described with reference to flowchart illustrations and / or block diagrams of methods, apparatus (systems), and computer program products according to embodiments of the invention. It will be understood that each block of the flowchart illustrations and / or block diagrams, and combinations of blocks in the flowchart illustrations and / or block diagrams, can be implemented by computer program instructions. These computer program instructions can be provided to a processor of a general-purpose computer, special-purpose computer, embedded computer, or other programmable data processing apparatus to produce a machine, such that the instructions, which execute via the processor of the computer or other programmable data processing apparatus, generate instructions for implementing the flowchart illustrations. Figure 1 One or more processes and / or boxes Figure 1 A device that provides the functions specified in one or more boxes.
[0108] These computer program instructions may also be stored in a computer-readable storage medium that can direct a computer or other programmable data processing device to function in a particular manner, such that the instructions stored in the computer-readable storage medium produce an article of manufacture including instruction means, which are implemented in a process Figure 1 One or more processes and / or boxes Figure 1 The function specified in one or more boxes.
[0109] These computer program instructions may also be loaded onto a computer or other programmable data processing equipment to cause a series of operational steps to be performed on the computer or other programmable equipment to produce a computer-implemented process, thereby providing instructions that execute on the computer or other programmable equipment for implementing the process. Figure 1 One or more processes and / or boxes Figure 1 The steps of the function specified in one or more boxes.
[0110] Although preferred embodiments of the invention have been described, those skilled in the art, upon learning the basic inventive concept, can make other changes and modifications to these embodiments. Therefore, the appended claims are intended to be interpreted as including both the preferred embodiments and all changes and modifications falling within the scope of the invention.
[0111] Obviously, those skilled in the art can make various modifications and variations to this invention without departing from its spirit and scope. Therefore, if these modifications and variations fall within the scope of the claims of this invention and their equivalents, this invention also intends to include these modifications and variations.
Claims
1. A method for hardness assessment and correction of carbon steel joints considering welding thermal cycles, characterized in that, Includes the following steps: S1, obtain the residual plastic strain value of carbon steel welded joint; specifically, by thermocouple and strain gauge testing or thermo-elastic-plastic finite element analysis, obtain the thermal cycle curve of the entire weld area including the predetermined position and the value of plastic strain at the corresponding time, and discretize it to obtain the plastic strain under thermal cycle at different times. S2, based on the residual plastic strain at the predetermined location, the dislocation density at that location is calculated as follows: ; in, For dislocation density, Plastic strain; S3, considering the recovery recrystallization phenomenon of welding thermal cycle, corrects the dislocation density at different times; S3 specifically includes: S31, utilizing dislocation density at time Compared to the previous moment dislocation density change The difference is used as the dislocation density after the first correction at the current moment. Where i is a natural number greater than or equal to 1; S32, calculate the time interval based on the dislocation density and its first correction value ( The first dislocation density recovery rate r1: ; The dislocation density constant under no plastic strain is: ; S33, Calculate the first recovery recrystallization parameter c1: ; Where n is the recrystallization index of carbon steel, with a value of 0.249; S34, based on the Arrhenius formula, calculate the second recovery recrystallization parameter c2: ; in, To restore the recrystallization constant, Q is the heat of reaction, which represents the heat released or absorbed by a certain amount of substance in a reaction, with a value of 113600 J / mol; R is the gas constant, with a value of 8.314 J / (mol·K); Ti is the thermodynamic temperature at time ti, in K. S35, based on the Johnson-Mehl formula, calculate the dislocation density recovery rate r2 of the second correction: ; S36, considering the influence of dislocation density recovery rate, i.e., the recovery recrystallization phenomenon, the second corrected dislocation density is as follows: : ; S37, Calculation Change in dislocation density at time t : ; In this way The dislocation density at any given time is corrected; S4, the hardness value is calculated based on the corrected dislocation density.
2. The method for hardness assessment and correction of carbon steel joints considering welding thermal cycles according to claim 1, characterized in that, The formula for calculating hardness in S4 is as follows: ; in, HV represents the corrected dislocation density and hardness.
3. The method for hardness assessment and correction of carbon steel joints considering welding thermal cycles according to claim 1, characterized in that, The process after S37 includes: repeating steps S31 to S37, taking into account the effect of temperature on dislocation density, until the welding thermal cycle ends and the temperature returns to room temperature, and gradually obtaining the second corrected dislocation density.
4. The method for hardness assessment and correction of carbon steel joints considering welding thermal cycles according to claim 1, characterized in that, At the initial moment hour, .
5. A hardness assessment and correction system for carbon steel joints considering welding thermal cycles, characterized in that, The system is used to implement the carbon steel joint hardness assessment correction method considering welding thermal cycles as described in any one of claims 1-4, comprising: The residual plastic strain acquisition module is used to acquire the residual plastic strain value of carbon steel welded joints; The dislocation density calculation module is used to calculate the dislocation density at a predetermined location based on the residual plastic strain at that location. The dislocation density correction module is used to take into account the recovery and recrystallization phenomenon of welding thermal cycle and correct the dislocation density at different times. The hardness calculation module is used to calculate the hardness value based on the corrected dislocation density.
6. An electronic device, characterized in that, The system includes a memory and a processor, wherein the processor is used to execute computer management programs stored in the memory to implement the steps of the carbon steel joint hardness assessment correction method considering welding thermal cycles as described in any one of claims 1-4.
7. A computer-readable storage medium, characterized in that, It stores a computer management program, which, when executed by a processor, implements the steps of the carbon steel joint hardness assessment correction method considering welding thermal cycles as described in any one of claims 1-4.