Method of forming a semiconductor structure

By forming a composite structure in the semiconductor process and performing cyclic etching, the size limit problem of fin field-effect transistors is solved, dummy gate residue is reduced, and the performance and stability of the semiconductor structure are improved.

CN116779441BActive Publication Date: 2026-11-20SEMICON MFG INT (SHANGHAI) CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202210242754.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-11
Publication Date
2026-11-20
Estimated Expiration
2042-03-11

AI Technical Summary

Technical Problem

In existing semiconductor processes, after the size of fin field-effect transistors is reduced to the limit, there are problems such as fin spacing, short-channel effect, leakage current and material limitations, which make transistor manufacturing difficult and dummy gate residue affects performance.

Method used

A composite structure is formed on the substrate, and discrete fin structures are formed through cyclic processing. A mask structure is used as a mask for etching to form an intermediate trench and increase its depth, thereby reducing dummy gate residue and improving performance.

Benefits of technology

By reducing the recess of the sacrificial layer sidewall relative to the channel layer sidewall, dummy gate residue is avoided, thus improving the performance and process stability of the semiconductor structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116779441B_ABST
    Figure CN116779441B_ABST
Patent Text Reader

Abstract

A method for forming a semiconductor structure includes: providing a substrate, the substrate having a composite structure thereon; forming a plurality of mutually discrete mask structures on the composite structure; and performing a plurality of cycles of processing on the composite structure with the plurality of mask structures as masks to form a plurality of mutually discrete fin structures on the substrate, the fin structures including a plurality of alternating stacks of sacrificial layers and channel layers, each cycle of processing forming a plurality of intermediate trenches between adjacent mask structures and within the composite structure after the cycle of processing, each cycle of processing including: forming a first sidewall on sidewall surfaces of the intermediate trenches formed in a previous cycle of processing; and etching the first sidewall, and at least one of a plurality of initial sacrificial layers and a plurality of initial channel layers exposed by the etching, to increase a depth of the intermediate trenches formed in the previous cycle of processing. Thus, the performance of the semiconductor structure is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of semiconductor manufacturing, and in particular to a method for forming a semiconductor structure. Background Technology

[0002] In the current semiconductor field, the FinFET (Fin Field-Effect Transistor) is an emerging multi-gate device. Compared with planar metal-oxide-semiconductor field-effect transistors (MOSFETs), FinFETs have stronger short-channel rejection and higher operating current, and are now widely used in various semiconductor devices. However, with the further development of semiconductor technology, the transistor size has shrunk to below a few nanometers. The size of FinFETs themselves has already reached its limit. Limitations in fin spacing, short-channel effect, leakage current, and materials have made transistor manufacturing precarious, and even the physical structure cannot be completed.

[0003] Gate-all-around (GAA) devices have become a new direction for research and development in the industry. This technology is characterized by the gate completely surrounding the channel on all four sides. The source and drain no longer contact the substrate; instead, multiple source and drain electrodes, arranged laterally and perpendicularly to the gate in linear (rod-like), planar, or sheet-like shapes, are used to achieve the basic structure and function of a MOSFET. This design largely solves various problems caused by reducing the gate spacing, including capacitance effects. Furthermore, since the channel is surrounded by the gate on all four sides, the channel current flows more smoothly than with the three-sided enclosure of a FinFET.

[0004] However, as an important direction for development in the industry, gate-all-around devices still require further improvement. Summary of the Invention

[0005] The technical problem solved by this invention is to provide a method for forming a semiconductor structure to improve the performance of the semiconductor structure.

[0006] To solve the above-mentioned technical problems, the present invention provides a method for forming a semiconductor structure, comprising: providing a substrate having a composite structure, the composite structure including a plurality of initial sacrificial layers and a plurality of initial channel layers alternately stacked along the normal direction of the substrate surface; forming a plurality of mutually discrete mask structures on the composite structure; using the plurality of mask structures as masks, performing a plurality of cycle processing on the composite structure to form a plurality of mutually discrete fin structures on the substrate, the fin structures including a plurality of sacrificial layers and a plurality of channel layers alternately stacked along the normal direction of the substrate surface, wherein after each cycle processing, a plurality of intermediate trenches are formed between adjacent mask structures and within the composite structure, and the method of each cycle processing includes: forming a first sidewall on the sidewall of the intermediate trench formed in the previous cycle processing, the first sidewall being at least located on the sidewall of the mask structure and the channel layers and sacrificial layers formed after the previous cycle processing; using the plurality of mask structures as masks, etching the first sidewall and at least one of the exposed plurality of initial sacrificial layers and a plurality of initial channel layers to increase the depth of the intermediate trench formed in the previous cycle processing.

[0007] Optionally, a method of etching the first sidewall and at least one of the exposed initial sacrificial layers and initial channel layers using the plurality of mask structures as masks includes: etching one exposed initial sacrificial layer or one exposed initial channel layer using the plurality of mask structures as masks.

[0008] Optionally, the multiple cyclic processes are performed within the same reaction chamber.

[0009] Optionally, the method for forming a first sidewall on the sidewall of the intermediate trench formed in the previous cycle includes: using an in-situ atomic layer deposition process to form a first sidewall film on the top surface of the mask structure and the inner wall surface of the intermediate trench formed in the previous cycle; and using an in-situ anisotropic etching process to etch the first sidewall film until the top surface of the mask structure and the bottom surface of the intermediate trench formed in the previous cycle are exposed.

[0010] Optionally, the method for performing the in-situ atomic layer deposition process includes: introducing aminosilane into the reaction chamber; and after introducing aminosilane into the reaction chamber, introducing oxygen into the reaction chamber.

[0011] Optionally, the parameters of the in-situ atomic layer deposition process include: a temperature below 100 degrees Celsius.

[0012] Optionally, the anisotropic etching process includes plasma etching.

[0013] Optionally, the process parameters for plasma etching include a bias voltage range of 600V to 1300V.

[0014] Optionally, it also includes: forming an etching stop layer on the surface of the composite structure before forming the mask structure; and, during the initial cycle processing, while etching the first sidewall film using an anisotropic etching process, the etching stop layer is also etched until the surface of the composite structure is exposed.

[0015] Optionally, the material of the etching stop layer is the same as the material of the first sidewall membrane.

[0016] Optionally, after several cycles of processing, the method further includes: forming a second sidewall on the sidewalls of the mask structures and the fin structures; using the mask structures as a mask, etching the second sidewall and the substrate to remove the second sidewall and form a substrate, and an isolation fin located between the substrate and each fin structure; and forming an isolation structure between adjacent isolation fins.

[0017] Optionally, the method for forming the second sidewall includes: using an in-situ atomic layer deposition process to form a second sidewall film on the surfaces of several mask structures, several fin structure sidewalls, and the substrate surface; and using an in-situ anisotropic etching process to etch the second sidewall film until the surface of the substrate is exposed.

[0018] Optionally, the material of the second sidewall includes silicon oxide.

[0019] Optionally, the material of the first sidewall includes silicon oxide.

[0020] Optionally, the method of forming a plurality of mutually independent mask structures on the composite structure includes: forming a plurality of mutually independent core structures on the composite structure; forming a third sidewall on the sidewall of the core structure; after forming the third sidewall, removing the core structure and using the third sidewall as the mask structure.

[0021] Optionally, a method for forming a plurality of mutually discrete mask structures on the composite structure includes: forming a mask material layer on the composite structure; forming a plurality of mutually discrete core structures on the mask material layer; forming a third sidewall on the sidewall of the core structure; removing the core structure after forming the third sidewall; and etching the mask material layer using the third sidewall as a mask after removing the mask structure, until a plurality of the mask structures are formed.

[0022] Optionally, the method further includes: forming an etching stop layer on the surface of the composite structure before forming the mask material layer; and etching the mask material layer using the third sidewalls as masks until the mask structures are formed, including: using the third sidewalls as masks to etch the mask material layer until the etching stop layer is exposed.

[0023] Optionally, the substrate and the initial channel layer are made of silicon, and the initial sacrificial layer is made of germanium-silicon.

[0024] Compared with the prior art, the technical solution of the embodiments of the present invention has the following beneficial effects:

[0025] In the semiconductor structure formation method provided by the present invention, a composite structure on a substrate includes a plurality of initial sacrificial layers and a plurality of initial channel layers alternately stacked along the normal direction of the substrate surface; a plurality of mutually discrete mask structures are formed on the composite structure; using the plurality of mask structures as masks, the composite structure is subjected to a plurality of cyclic processing to form a plurality of mutually discrete fin structures on the substrate, the fin structures including a plurality of sacrificial layers and a plurality of channel layers alternately stacked along the normal direction of the substrate surface; after each cyclic processing, a plurality of intermediate trenches are formed between adjacent mask structures and within the composite structure; the method of each cyclic processing includes: forming a first sidewall on the sidewall of the intermediate trench formed in the previous cyclic processing; using the plurality of mask structures as masks, etching the first sidewall and at least one of the exposed plurality of initial sacrificial layers and a plurality of initial channel layers to increase the depth of the intermediate trench formed in the previous cyclic processing. Therefore, after several cycles of processing, it is possible to form several fin structures with a width close to or the same as the expected width, while reducing the degree of concavity of the sidewall of the sacrificial layer relative to the sidewall of the channel layer. This reduces or avoids dummy gate residue in subsequent gate-back processes and improves the performance of the semiconductor structure. Attached Figure Description

[0026] Figures 1 to 3 This is a cross-sectional structural diagram of each step in a method for forming a semiconductor structure;

[0027] Figures 4 to 17 This is a schematic diagram of each step in a method for forming a semiconductor structure according to an embodiment of the present invention. Detailed Implementation

[0028] As described in the background section, the performance of semiconductor devices manufactured in the prior art needs improvement. An embodiment will now be used for illustration and analysis.

[0029] Figures 1 to 3 This is a cross-sectional schematic diagram of each step in a method for forming a semiconductor structure.

[0030] Please refer to Figure 1 Provides a base of 100.

[0031] Please continue to refer to this. Figure 1 A plurality of sacrificial material layers 110 and a plurality of channel material layers 120 are deposited alternately on a substrate 100. The sacrificial material layers 110 are made of germanium-silicon, and the channel material layers 120 are made of silicon.

[0032] Please continue to refer to this. Figure 1 Several mutually independent mask structures 130 are formed on several sacrificial material layers 110 and several channel material layers 120.

[0033] Please refer to Figure 2 The plasma etching process using halogen gas is employed, with several mask structures 130 as masks, to etch several sacrificial material layers 110 and several channel material layers 120 until the surface of the substrate 100 is exposed, forming several mutually independent fin structures 140, wherein the fin structure 140 includes several sacrificial layers 111 and several channel layers 121 stacked alternately.

[0034] Please continue to refer to this. Figure 2 After forming several fin structures 140, the substrate 100 is etched using several mask structures 130 as masks to form a substrate 101 and an isolation fin 150 between the substrate 101 and the fin structures 140.

[0035] Please continue to refer to this. Figure 2 An isolation layer 160 is formed between adjacent isolation fins 150.

[0036] Please refer to Figure 3 A pseudo-gate 170 is formed on the isolation layer 160, spanning several fin structures 140.

[0037] The dummy gate 170 is used for positioning in the subsequent gate process to form the metal gate. The dummy gate 170 needs to be removed and replaced with the metal gate.

[0038] However, in the above method, since the sacrificial material layer 110 contains germanium, which is more reactive than silicon, during the formation of the fin structure 140 using a halogen gas plasma etching process, the sacrificial material layer 110 is more prone to chemical bond breaking and reaction than the channel material layer 120. This results in a faster etching rate for the sacrificial material layer 110 than for the channel material layer 120. Consequently, the sidewall of the sacrificial layer 111 in the fin structure 140 is recessed relative to the sidewall of the channel layer 121 (e.g., ...). Figure 2 (As shown in region A).

[0039] Because the sidewalls of the sacrificial layer 111 are recessed relative to the sidewalls of the channel layer 121, the dummy gate 170 is difficult to remove at the recessed area and tends to remain. This results in poor performance of the semiconductor structure.

[0040] To address the aforementioned technical problems, the present invention provides a method for forming a semiconductor structure. In this method, a composite structure on a substrate includes several initial sacrificial layers and several initial channel layers alternately stacked along the normal direction of the substrate surface. Several discrete mask structures are formed on the composite structure. Using these mask structures as masks, the composite structure undergoes several cyclic processing cycles to form several discrete fin structures on the substrate. Each fin structure includes several sacrificial layers and several channel layers alternately stacked along the normal direction of the substrate surface. After each cyclic processing cycle, several intermediate trenches are formed between adjacent mask structures and within the composite structure. Each cyclic processing cycle includes: forming a first sidewall on the sidewall of the intermediate trench formed in the previous cyclic processing cycle; using the mask structures as masks, etching the first sidewall and at least one of the exposed initial sacrificial layers and initial channel layers to increase the depth of the intermediate trench formed in the previous cyclic processing cycle. Therefore, dummy gate residue in subsequent gate-after-processing is reduced or avoided, improving the performance of the semiconductor structure.

[0041] To make the above-mentioned objectives, features and beneficial effects of the present invention more apparent and understandable, specific embodiments of the present invention will be described in detail below with reference to the accompanying drawings.

[0042] Figures 4 to 17 This is a schematic diagram of each step in a method for forming a semiconductor structure according to an embodiment of the present invention.

[0043] Please refer to Figure 4 A substrate 200 is provided, wherein a composite structure 300 is provided on the substrate 200.

[0044] The substrate 200 is made of semiconductor materials.

[0045] In this embodiment, the material of the substrate 200 includes silicon.

[0046] In other embodiments, the substrate material includes silicon carbide, silicon-germanium, a multi-element semiconductor material composed of group III-V elements, silicon-on-insulator (SOI), or germanium-on-insulator (GOI), etc. The multi-element semiconductor material composed of group III-V elements includes InP, GaAs, GaP, InAs, InSb, InGaAs, or InGaAsP, etc.

[0047] The composite structure 300 provides materials for the subsequent formation of several fin structures.

[0048] The composite structure 300 includes a plurality of initial sacrificial layers 310 and a plurality of initial channel layers 320 alternately stacked along the normal direction of the surface of the substrate 200.

[0049] The initial sacrificial layer 310 provides materials for the subsequent formation of the sacrificial layer, and the initial channel layer 320 provides materials for the subsequent formation of the channel layer.

[0050] In this embodiment, the material of the initial sacrificial layer 310 includes germanium silicon, and the material of the initial channel layer 320 includes silicon.

[0051] In this embodiment, the process for forming the initial sacrificial layer 310 includes: chemical vapor deposition, physical vapor deposition, or epitaxial growth, etc.

[0052] In this embodiment, the process for forming the initial channel layer 320 includes: chemical vapor deposition, physical vapor deposition, or epitaxial growth, etc.

[0053] Next, a plurality of independent mask structures are formed on the composite structure 300. For detailed steps on forming the plurality of mask structures, please refer to [link to documentation]. Figures 5 to 7 .

[0054] Please refer to Figure 5 A mask material layer 400 is formed on the composite structure 300.

[0055] The mask material layer 400 provides material for forming the mask structure.

[0056] In this embodiment, the mask material layer 400 is a stacked composite layer structure.

[0057] In other embodiments, the mask material layer is a single-layer structure.

[0058] In this embodiment, the mask material layer 400 is made of silicon nitride and silicon oxide.

[0059] In other embodiments, the mask structure is made of silicon oxide or silicon nitride.

[0060] In this embodiment, the process for forming the mask material layer 400 includes at least one of chemical vapor deposition, physical vapor deposition, and atomic layer deposition.

[0061] In this embodiment, before forming the mask material layer 400, an etching stop layer 410 is formed on the surface of the composite structure 300.

[0062] The etching stop layer 410 protects the surface of the composite structure 300 during the etching of the mask material layer 400 to form several mask structures, reducing damage and loss to the composite structure 300, so as to form several fin structures with better morphology and more accurate size in the subsequent process, thereby improving the performance of the semiconductor structure.

[0063] In this embodiment, the material of the etching stop layer 410 is the same as the material of the first sidewall in the subsequent cycle processing, so that the exposed etching stop layer 410 can be removed during the etching process that forms the first sidewall during the initial cycle processing, thereby simplifying the manufacturing process and improving efficiency.

[0064] In this embodiment, the material of the etch stop layer 410 includes silicon oxide.

[0065] In this embodiment, the process for forming the etch stop layer 410 includes at least one of chemical vapor deposition, physical vapor deposition, and atomic layer deposition.

[0066] In other embodiments, no etch stop layer is formed.

[0067] Please refer to Figure 6 A plurality of mutually independent core structures (not shown) are formed on the mask material layer 400; a third sidewall 420 is formed on the sidewall of the core structure; after the third sidewall 420 is formed, the core structure is removed.

[0068] Please refer to Figure 7 After removing the core structure, the mask material layer 400 is etched using several third sidewalls 420 as masks until several independent mask structures 430 are formed on the composite structure 300.

[0069] By etching the mask material layer 400 after forming several third sidewalls 420, several mutually independent mask structures 430 are formed on the composite structure 300, thereby improving the stability of pattern transfer.

[0070] The etching process of the mask material layer 400 includes at least one of dry etching and wet etching.

[0071] Preferably, the mask material layer 400 is etched using a dry etching process.

[0072] In this embodiment, the method of etching the mask material layer 400 using a plurality of third sidewalls 420 as masks until a plurality of mask structures 430 are formed includes: using a plurality of third sidewalls 420 as masks, etching the mask material layer 400 until the etching stop layer 410 is exposed.

[0073] In this embodiment, after forming a plurality of mask structures 430, a plurality of the third sidewalls 420 are removed.

[0074] In another embodiment, no mask material layer is formed. Specifically, in another embodiment, the method of forming a plurality of mutually discrete mask structures on the composite structure 300 includes: forming a plurality of mutually discrete core structures on the composite structure 300; forming a third sidewall on the sidewall surface of the core structure; after forming the third sidewall, removing the core structure and using the third sidewall as the mask structure.

[0075] Next, please refer to Figures 8 to 15 Using the aforementioned mask structures 430 as masks, the composite structure 300 is subjected to several cycles of processing to form several mutually independent fin structures 330 on the substrate 200. The fin structure 330 includes several sacrificial layers 331 and several channel layers 332 that are alternately stacked along the normal direction of the surface of the substrate 200.

[0076] In several cycles of processing, after each cycle, several intermediate trenches are formed between adjacent mask structures 430 and within the composite structure 300.

[0077] In this embodiment, the multiple cycles of processing are performed within the same reaction chamber. Therefore, the vacuum is not broken during the multiple cycles, thereby reducing the risks of contamination and oxidation during the process, improving process stability, and further enhancing the performance of the semiconductor structure.

[0078] It should be noted that, Figure 8 This is a schematic diagram of the structure after the previous loop processing. Figures 9 to 11 This is a schematic diagram of the current loop processing. Figures 12 to 14 This is a schematic diagram of the initial loop processing. Figure 15 It is a schematic diagram of the cross-sectional structure of a semiconductor structure formed after several cycles of processing.

[0079] First, a first sidewall is formed on the sidewall of the intermediate trench formed in the previous cycle. This first sidewall is located on the sidewall of the mask structure, as well as the sidewall of the trench layer and sacrificial layer formed after the previous cycle. For details on the steps of forming the first sidewall on the sidewall of the intermediate trench formed in the previous cycle, please refer to [link to documentation / reference]. Figures 9 to 10 .

[0080] Please Figure 8 Based on reference Figure 9 In-situ atomic layer deposition (ALD) is employed, with the top surface of the mask structure 430 and the intermediate trench 440 formed in the previous cycle (e.g., ...) being deposited. Figure 8 The inner wall surface (as shown) forms a first sidewall membrane 500.

[0081] In-situ atomic layer deposition can be used to form a first sidewall membrane 500 with uniform thickness and low surface roughness.

[0082] It should be noted that in the initial processing cycle, the intermediate trench formed in the previous processing cycle refers to the initial intermediate trench 440a between adjacent mask structures 430 (e.g., Figure 7 (As shown).

[0083] In this embodiment, the material of the first sidewall membrane 500 includes silicon oxide.

[0084] The method for performing the in-situ atomic layer deposition process in this embodiment includes: introducing aminosilane into the reaction chamber; and after introducing aminosilane into the reaction chamber, introducing oxygen into the reaction chamber.

[0085] Aminosilane and oxygen can react at a relatively low temperature to form silicon oxide (the material of the first sidewall film 500). Therefore, the temperature of the in-situ atomic layer deposition process can be close to the temperature of the etching process, allowing the in-situ atomic layer deposition process to be performed within the reaction chamber of the etching equipment. Thus, the in-situ atomic layer deposition process, the subsequent etching process of the first sidewall film 500, and the subsequent etching process that increases the depth of the intermediate trench 440 formed in the previous cycle can all be performed within the same reaction chamber. This enables the multiple cycles of processing to be performed within the same reaction chamber.

[0086] Specifically, the parameters of the in-situ atomic layer deposition process include: a temperature below 100 degrees Celsius.

[0087] Furthermore, by introducing aminosilane into the reaction chamber, and then introducing oxygen into the reaction chamber after the aminosilane, not only is a material for forming silicon oxide provided, enabling the formation of the first sidewall film 500, but also direct contact between oxygen and the sacrificial layer 331, channel layer 332, and exposed initial sacrificial layer 310 and initial channel layer 320 formed before this cycle is reduced. This makes the sacrificial layer 331, channel layer 332, and exposed initial sacrificial layer 310 and initial channel layer 320 less susceptible to oxidation. Consequently, the width loss of the sacrificial layer 331 and channel layer 332 is reduced, forming a fin structure 330 that is closer to or consistent with the expected width (width of mask structure 420) to better improve the performance of the semiconductor structure. Moreover, the formation of germanium oxide from the oxidation of the sacrificial layer 310 is reduced, improving the etching uniformity in the subsequent etching processes of the first sidewall film 500 and the first sidewall, and reducing the difficulty of the subsequent etching processes of the first sidewall film 500 and the first sidewall.

[0088] Please refer to Figure 10The first sidewall film 500 is etched using an in-situ anisotropic etching process until the top surface of the mask structure 430 and the bottom surface of the intermediate trench 440 formed in the previous cycle are exposed, and the first sidewall 510 is formed on the sidewall of the intermediate trench 440 formed in the previous cycle.

[0089] The first sidewall 510 is located on the sidewall of the mask structure 430, as well as the channel layer 332 and sacrificial layer 331 formed after the previous cycle.

[0090] It should be noted that, when the initial processing is used as the current processing, since the channel layer 332 and sacrificial layer 331 were not formed before the initial processing (there is no previous processing before the initial processing), the first sidewall in the initial processing is located on the sidewall of the mask structure 430. When the initial processing is used as the previous processing, if only the channel layer 332 was formed in the initial processing (the initial sacrificial layer 310 was not etched in the initial processing), the first sidewall in the current processing is located on the sidewall of the mask structure 430 and the sidewall of the already formed channel layer 332.

[0091] Since the first sidewall film 500 with uniform thickness and low surface roughness can be formed by in-situ atomic layer deposition, the in-situ anisotropic etching process can be used to etch the first sidewall film 500. On the one hand, it can form a first sidewall 510 with uniform thickness, thereby reducing the difficulty of adjusting the subsequent etching process using several mask structures 430 as masks. On the other hand, the surface roughness of the first sidewall 510 located on the sidewall of the intermediate groove 440 is small. Therefore, after subsequent etching using several mask structures 430 as masks, a sacrificial layer 331 and a channel layer 332 with better morphology can be formed, thereby further improving the performance of the semiconductor structure.

[0092] In this embodiment, the material of the first sidewall 510 includes silicon oxide.

[0093] In this embodiment, the anisotropic etching process includes plasma etching.

[0094] Preferably, the process parameters for plasma etching include a bias voltage range of 600V to 1300V to better improve the etching directionality of the plasma etching.

[0095] In this embodiment, the parameters of the anisotropic etching process further include: the reaction gas includes C X H Y F Z It should be noted that C X H Y F Z It can be a complex gas, for example, CX H Y F Z It can be a composite gas composed of gaseous CHF3, gaseous CH3F, and gaseous CH2F2.

[0096] Next, please refer to Figure 11 Using several mask structures 430 as masks, the first sidewall 510, and at least one of the exposed initial sacrificial layers 310 and initial trench layers 320 are etched to increase the intermediate trench 440 formed in the previous cycle (e.g., Figure 8 As shown, at a depth of several intermediate trenches 440' are formed between adjacent mask structures 430 and within the composite structure 300 for this cycle of processing.

[0097] In this embodiment, in the etching process of etching the first sidewall 510 and at least one of the exposed initial sacrificial layers 310 and initial trench layers 320 using several mask structures 430 as masks, the time taken to complete the etching of at least one of the exposed initial sacrificial layers 310 and initial trench layers 320 is close to or the same as the time taken to complete the etching of the first sidewall 510.

[0098] It should be noted that the required film thickness of the first sidewall 510 for the specified time period can be estimated empirically. By forming the first sidewall 510 with this film thickness, the time required to complete the etching exposure of at least one of the initial sacrificial layers 310 and initial channel layers 320 is close to or consistent with the time required to complete the etching of the first sidewall 510. In other words, by pre-adjusting the film thickness of the first sidewall 510, the time required to complete the etching exposure of at least one of the initial sacrificial layers 310 and initial channel layers 320 can be close to or consistent with the time required to complete the etching of the first sidewall 510 in each processing cycle.

[0099] Preferably, the thickness of the first sidewall 510 is 2 nanometers.

[0100] In this embodiment, the method of etching at least one of the first sidewall 510, the exposed initial sacrificial layer 310, and the exposed initial channel layer 320 using the plurality of mask structures 430 as masks includes: using the plurality of mask structures 430 as masks, etching one exposed initial sacrificial layer 310 or one exposed initial channel layer 320.

[0101] Specifically, etching one exposed initial sacrificial layer 310 or one exposed initial channel layer 320 using the mask structures 430 as masks means: when one exposed initial sacrificial layer 310 is exposed in the current cycle, the one exposed initial sacrificial layer 310 is etched using the mask structures 430 as masks; when one exposed initial channel layer 320 is exposed in the current cycle, the one exposed initial channel layer 320 is etched using the mask structures 430 as masks.

[0102] Compared to etching two or more of the initial sacrificial layers 310 and initial channel layers 320, by using the mask structures 430 as masks to etch only one exposed initial sacrificial layer 310 or one exposed initial channel layer 320, the etching process difficulty can be further reduced. Furthermore, the etching time is shortened, thereby further reducing the exposure time of the formed sacrificial layer 331 and channel layer 332 during the etching process. This not only further reduces the degree of concavity between the sidewalls of the sacrificial layer 331 and the sidewalls of the channel layer 332, but also makes the widths of the sacrificial layer 331 and the channel layer 332 closer to the expected widths, thus improving the performance of the semiconductor structure.

[0103] In this embodiment, the process of etching the first sidewall 510, and at least one of the exposed initial sacrificial layers 310 and initial channel layers 320 using the mask structures 430 as masks includes atomic layer etching or dry etching.

[0104] Preferably, atomic layer etching is used to further improve etching accuracy.

[0105] It should be noted that in this embodiment, since an etch stop layer 410 is formed, in the initial cycle of several processing cycles, please refer to... Figure 12 and Figure 13 The first sidewall film 500a is etched using an anisotropic etching process (e.g., Figure 12 As shown), forming the first sidewall 510a (as shown). Figure 13 During the process (as shown), the etch stop layer 410 is also etched until the surface of the composite structure 300 is exposed, forming the etch stop layer 410a (as shown). Figure 13 (As shown). It should be understood that, since the etching stop layer 410 is made of the same material as the first sidewall film 500a, the exposed etching stop layer 410 is easily etched by the anisotropic etching process.

[0106] It should be noted that in this embodiment, due to the etching stop layer 410 and the first sidewall 510a (such as...) Figure 13The materials shown are the same; therefore, in the initial cycle of several cycles, please refer to... Figure 14 Using several mask structures 430 as masks, the first sidewall 510a, and at least one of the exposed initial sacrificial layers 310 and initial trench layers 320 are etched to increase the intermediate trench 440a (e.g., Figure 7 During the process of etching to the depth of (as shown), the etch stop layer 410a (as shown) Figure 13 (As shown) is etched together with the first sidewall 510a to form an etch stop layer 410b with a width close to that of the mask structure 430.

[0107] Please refer to Figure 15 After several cycles of the aforementioned processing, a plurality of mutually independent fin structures 330 are formed on the substrate 200.

[0108] The fin structure 330 includes a plurality of sacrificial layers 331 and a plurality of channel layers 332 that are alternately stacked along the normal direction of the surface of the substrate 200.

[0109] Because the composite structure 300 is subjected to several cycles of processing using the aforementioned mask structures 430 as masks, several mutually independent fin structures 330 are formed on the substrate 200. Each fin structure 330 includes several sacrificial layers 331 and several channel layers 332 alternately stacked along the normal direction of the substrate 200 surface. After each cycle, several intermediate trenches are formed between adjacent mask structures 430 and within the composite structure 300. The method of each cycle includes: in the intermediate trenches formed in the previous cycle (e.g., ... Figure 8 The sidewall of the intermediate trench 440 shown forms a first sidewall (e.g. Figure 10 The first sidewall 510 is shown; using the mask structures 430 as masks, the first sidewall, and at least one of the exposed initial sacrificial layers 310 and initial channel layers 320 are etched to increase the depth of the intermediate trench formed in the previous cycle. Therefore, after several cycles, it is possible to form a plurality of fin structures 330 with a width close to or the same as the expected width (i.e., the width of the mask structure 430), while reducing the degree of concavity of the sidewall surface of the sacrificial layer 331 relative to the sidewall surface of the channel layer 332, thereby reducing or avoiding dummy gate residue in subsequent gate-after processes and improving the performance of the semiconductor structure.

[0110] Specifically, on the one hand, by etching the composite structure 300 through several cycles, the overall etching time of the composite structure 300 is broken down, shortening the etching time of the composite structure 300 in each cycle. This results in a shorter exposure time for the sacrificial layer 331 and the channel layer 332 formed during the etching of the composite structure 300 in each cycle. On the other hand, by etching the composite structure 300 in the current cycle, the intermediate trenches formed in the previous cycle (e.g., Figure 8 The sidewall of the intermediate trench 440 shown forms a first sidewall (e.g. Figure 10 The first sidewall 510 shown ensures that the sacrificial layers 331 and trench layers 332 formed prior to the current etching process on the composite structure 300 are protected by the first sidewall. Therefore, the degree of concavity of the sidewall of the sacrificial layer 331 relative to the sidewall of the trench layer 332 can be reduced.

[0111] At the same time, through the first sidewall (e.g.) Figure 10 The first sidewall 510 shown can increase the mask width during the etching process of the composite structure 300 based on the width (expected width) of the mask structure 430, and reserve sacrificial material for the etching process of the composite structure 300. Thus, as the first sidewall is removed, a channel layer 332 and a sacrificial layer 331 with a width close to or the same as the expected width can be formed after this cycle of processing.

[0112] Therefore, after several cycles of processing, while forming several fin structures 330 with a width close to or the same as expected, the degree of concavity of the sidewall of the sacrificial layer 331 relative to the sidewall of the channel layer 332 can be reduced, thereby reducing or avoiding dummy gate residue in subsequent gate-back processes and improving the performance of the semiconductor structure.

[0113] Please refer to Figure 16 After several cycles of processing, a second sidewall 600 is formed on the sidewalls of several mask structures 430 and several fin structures 330.

[0114] The second sidewall 600 can protect the fin structure 330 during the subsequent etching process to form the isolation fin, thereby further improving the performance of the semiconductor structure.

[0115] In this embodiment, the method for forming the second sidewall 600 includes: using an in-situ atomic layer deposition process to form a second sidewall film (not shown) on the surfaces of several mask structures 430, the sidewalls of several fin structures 330, and the surface of the substrate 200; and using an in-situ anisotropic etching process to etch the second sidewall film until the surface of the substrate 200 is exposed. This reduces the risks of contamination and oxidation during the formation of the second sidewall 600, improves process stability, and further enhances the performance of the semiconductor structure.

[0116] In this embodiment, the material of the second sidewall 600 includes silicon oxide. The in-situ atomic layer deposition process for forming the second sidewall 600 can refer to the in-situ atomic layer deposition process in the aforementioned cycle process, and the in-situ anisotropic etching process for etching the second sidewall film can refer to the in-situ anisotropic etching process in the aforementioned cycle process, and will not be described again here.

[0117] Please refer to Figure 17 Using the mask structure 430 as a mask, the second sidewall 600 and the substrate 200 are etched to remove the second sidewall 600 and form a substrate 201 and an isolation fin 202 located between the substrate 201 and each fin structure 330.

[0118] In this embodiment, the process of etching the second sidewall 600 and the substrate 200 using the mask structure 430 as a mask includes atomic layer etching or dry etching.

[0119] In this embodiment, after forming the substrate 201 and the isolation fins 202 located between the substrate 201 and each fin structure 330, an isolation structure (not shown) is formed between adjacent isolation fins 202.

[0120] While the present invention has been disclosed above, it is not limited thereto. Any person skilled in the art can make various modifications and alterations without departing from the spirit and scope of the invention; therefore, the scope of protection of the present invention should be determined by the scope defined in the claims.

Claims

1. A method for forming a semiconductor structure, characterized in that, include: A substrate is provided having a composite structure, the composite structure comprising a plurality of initial sacrificial layers and a plurality of initial channel layers alternately stacked along the normal direction of the substrate surface; Several mutually independent mask structures are formed on the composite structure; Using the plurality of mask structures as masks, the composite structure is subjected to a plurality of cyclic processing to form a plurality of mutually independent fin structures on the substrate. The fin structures include a plurality of sacrificial layers and a plurality of channel layers that are alternately stacked along the normal direction of the substrate surface. After each cycle processing, a plurality of intermediate trenches are formed between adjacent mask structures and within the composite structure. The method of each cycle processing includes: forming a first sidewall on the sidewall of the intermediate trench formed in the previous cycle processing. The first sidewall is located on the sidewall of the mask structure and the channel layers and sacrificial layers formed after the previous cycle processing, and exposing the bottom surface of the intermediate trench formed in the previous cycle processing; using the plurality of mask structures as masks, etching the first sidewall and at least one of the exposed plurality of initial sacrificial layers and plurality of initial channel layers to increase the depth of the intermediate trench formed in the previous cycle processing.

2. The method for forming a semiconductor structure as described in claim 1, characterized in that, A method of etching the first sidewall and at least one of the exposed initial sacrificial layers and initial channel layers using the plurality of mask structures as masks includes: etching one exposed initial sacrificial layer or one exposed initial channel layer using the plurality of mask structures as masks.

3. The method for forming a semiconductor structure as described in claim 1, characterized in that, The several cycles of processing are carried out in the same reaction chamber.

4. The method for forming a semiconductor structure as described in claim 1, characterized in that, The method for forming a first sidewall on the sidewall of the intermediate trench formed in the previous cycle includes: forming a first sidewall film on the top surface of the mask structure and the inner wall surface of the intermediate trench formed in the previous cycle using an in-situ atomic layer deposition process; and etching the first sidewall film using an in-situ anisotropic etching process until the top surface of the mask structure and the bottom surface of the intermediate trench formed in the previous cycle are exposed.

5. The method for forming a semiconductor structure as described in claim 4, characterized in that, The method for performing the in-situ atomic layer deposition process includes: introducing aminosilane into the reaction chamber; and after introducing aminosilane into the reaction chamber, introducing oxygen into the reaction chamber.

6. The method for forming a semiconductor structure as described in claim 4, characterized in that, The parameters of the in-situ atomic layer deposition process include: temperature below 100 degrees Celsius.

7. The method for forming a semiconductor structure as described in claim 4, characterized in that, The anisotropic etching process includes plasma etching.

8. The method for forming a semiconductor structure as described in claim 7, characterized in that, The process parameters for plasma etching include a bias voltage range of 600V to 1300V.

9. The method for forming a semiconductor structure as described in claim 4, characterized in that, Also includes: Before forming the mask structure, an etching stop layer is formed on the surface of the composite structure; Furthermore, during the initial cycle processing, while using anisotropic etching technology to etch the first sidewall film, the etching stop layer is also etched until the surface of the composite structure is exposed.

10. The method for forming a semiconductor structure as described in claim 9, characterized in that, The material of the etching stop layer is the same as the material of the first sidewall membrane.

11. The method for forming a semiconductor structure as described in claim 1, characterized in that, After several cycles of processing, the process further includes: forming a second sidewall on the sidewalls of several mask structures and several fin structures; using the mask structure as a mask, etching the second sidewall and the substrate to remove the second sidewall and form a substrate, and an isolation fin located between the substrate and each fin structure; and forming an isolation structure between adjacent isolation fins.

12. The method for forming a semiconductor structure as described in claim 11, characterized in that, The method for forming the second sidewall includes: using an in-situ atomic layer deposition process to form a second sidewall film on the surfaces of several mask structures, several fin structure sidewalls, and the substrate surface; and using an in-situ anisotropic etching process to etch the second sidewall film until the surface of the substrate is exposed.

13. The method for forming a semiconductor structure as described in claim 11, characterized in that, The material of the second sidewall includes silicon oxide.

14. The method for forming a semiconductor structure as described in claim 1, characterized in that, The material of the first sidewall includes silicon oxide.

15. The method for forming a semiconductor structure as described in claim 1, characterized in that, A method for forming a plurality of mutually independent mask structures on the composite structure includes: forming a plurality of mutually independent core structures on the composite structure; forming a third sidewall on the sidewall of the core structure; after forming the third sidewall, removing the core structure and using the third sidewall as the mask structure.

16. The method for forming a semiconductor structure as described in claim 1, characterized in that, A method for forming a plurality of mutually independent mask structures on the composite structure includes: forming a mask material layer on the composite structure; forming a plurality of mutually independent core structures on the mask material layer; forming a third sidewall on the sidewall of the core structure; removing the core structure after forming the third sidewall; and etching the mask material layer using the third sidewall as a mask after removing the mask structure, until the plurality of mask structures are formed.

17. The method for forming a semiconductor structure as described in claim 16, characterized in that, Also includes: Before forming the mask material layer, an etching stop layer is formed on the surface of the composite structure; Furthermore, the method of etching the mask material layer using a plurality of third sidewalls as masks until a plurality of mask structures are formed includes: using the third sidewalls as masks, etching the mask material layer until the etching stop layer is exposed.

18. The method for forming a semiconductor structure as described in claim 1, characterized in that, The substrate and the initial channel layer are made of silicon, and the initial sacrificial layer is made of germanium-silicon.

Citation Information

Patent Citations

  • Methods of fabricating semiconductor fin structures

    US20150340289A1