An electrode sheet, a method of manufacturing the same, and a battery and a vehicle
By introducing nanorolls of one-dimensional hollow conductive material into the electrode sheet, the problems of long transport paths and difficult electrolyte wetting in lithium-ion batteries have been solved, improving the energy density and power density of the battery and simplifying the production process.
Patent Information
- Application Number
- CN202210226564.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-09
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2042-03-09
AI Technical Summary
Existing lithium-ion batteries face challenges in improving energy density and power density, especially due to safety hazards caused by incomplete electrode wetting and long transmission paths. Furthermore, the development of new electrode materials is time-consuming and inefficient.
Introducing one-dimensional hollow conductive materials with open ends, such as nanorolls formed by rolling up two-dimensional MXene materials, into the electrode sheet can construct a fast transport channel to achieve dual transport of lithium ions and electrons.
It improves the energy density and power density of batteries, solves the problem of electrolyte impregnation, simplifies the production process, and reduces costs and time.
Smart Images

Figure CN116779775B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of batteries, and in particular relates to an electrode sheet, its preparation method, and batteries and vehicles. Background Technology
[0002] Faced with the challenge of dwindling global oil resources and the urgent need to improve air pollution, the automotive industry urgently needs to reduce its dependence on oil, decrease emissions of pollutants (PM2.5, etc.) and carbon dioxide, and develop energy-saving and new energy vehicle industries. Recently, national policies have strongly supported new energy vehicles, providing ample space for the development of the lithium-ion battery industry, while also placing higher demands on the energy density, power density, and safety of lithium-ion batteries. Research on lithium-ion battery applications is developing in two directions: high-power lithium-ion batteries and high-capacity energy storage lithium-ion batteries. The electrochemical performance of lithium-ion batteries mainly depends on the structure and performance of the electrode and electrolyte materials used; the selection and quality of electrode materials directly determine the characteristics and price of lithium-ion batteries.
[0003] To improve battery energy density, current methods include two approaches. One is from a design perspective: reducing the proportion of inactive material components in the electrode to increase the energy storage capacity of the active material. For example, reducing the content of binders and conductive agents is a commonly used solution. Another approach is to increase the proportion of active material relative to the current collector (copper or aluminum foil), i.e., increasing the electrode coating thickness. However, as the electrode thickness increases, it is easy for the electrode to not be fully wetted, leading to lithium plating on the negative electrode at high rates when fully charged, reducing battery capacity, and even causing safety hazards.
[0004] Improving the rate performance of batteries essentially involves reducing the transport path of lithium ions and electrons in electrode materials. Currently, much work focuses on developing novel electrode materials, including improvements in material type, structure, and morphology. However, developing new electrode materials is time-consuming and requires compatibility with corresponding electrolytes, separators, and manufacturing processes. Furthermore, their integration into production systems necessitates small-scale and pilot-scale verification. Large-scale production and application have long cycles and low overall efficiency. Summary of the Invention
[0005] To address the aforementioned technical problems, this invention provides an electrode sheet in which a one-dimensional hollow, open-ended, one-dimensional conductive material is dispersed within the electrochemically active material. This one-dimensional conductive material acts as a "major artery" in the electrode sheet, enabling the rapid transport of lithium ions and electrons simultaneously. By utilizing existing electrochemically active materials (i.e., electrode materials) and improving the conductive network within the electrode sheet, the transport paths of lithium ions and electrons within the electrode material are reduced, while simultaneously improving electrolyte wettability, thereby increasing the energy density and power density of the battery.
[0006] The first aspect of the present invention provides an electrode sheet, comprising a current collector and an active material layer in contact with the current collector, the active material layer comprising: an electrochemically active material, a conductive agent, and a binder; wherein the conductive agent comprises: a one-dimensional conductive material having a hollow structure and openings at both ends.
[0007] In some embodiments, the aforementioned one-dimensional conductive material is a one-dimensional hollow nanoroll formed by rolling up the two-dimensional material MXene.
[0008] In some embodiments, the nanorolls are formed by rolling up a monolith of the two-dimensional material; and / or, the nanorolls are formed by rolling up a monolayer of the two-dimensional material; and / or, the one-dimensional morphology of the one-dimensional conductive material is linear.
[0009] In some embodiments, the thickness of the tube wall of the one-dimensional conductive material is between 0.3 nm and 10 nm; and / or, the length of the nanoroll is between 0.1 μm and 100 μm; and / or, the diameter of the nanoroll is between 10 nm and 200 nm; preferably, between 40 nm and 200 nm.
[0010] In some embodiments, the chemical formula of the MXene is represented as M. n+1 X n T x Where M is selected from one or more transition metal elements, X is selected from one, two, or three of carbon, nitrogen, or boron elements, n is between 1, 2, 3, or 4, and T x The functional group is preferably selected from one, two, or three of the following: Ti, V, Nb, Cr, Ta, Hf, Mo, W, Fe, Mn, Y, or Sc.
[0011] In some embodiments, the electrochemically active material is selected from: lithium-ion battery cathode materials, or lithium-based battery anode materials.
[0012] In some embodiments, the cathode material of the above-mentioned lithium-based battery is selected from lithium iron phosphate (LiFePO4), lithium cobalt oxide (LiCoO2), lithium manganese oxide (LiMn2O4), lithium nickel oxide (LiNiO2), and ternary materials (LiNi... x Co y Mn y O2, where x+y+z=1), or elemental sulfur; the above-mentioned lithium-based battery anode materials include one of silicon, silicon oxide, silicon suboxide, and graphite.
[0013] In some embodiments, the conductive agent further includes a two-dimensional conductive material or a zero-dimensional material; preferably, the two-dimensional material is selected from one or more of two-dimensional MXene materials, graphene, and graphite sheets; the zero-dimensional material is selected as carbon black.
[0014] In some embodiments, the electrochemically active material comprises 70 to 100 parts by mass percentage; the conductive agent comprises 1 to 10 parts by mass percentage; and the binder comprises 1 to 10 parts by mass percentage; wherein the mass percentage of the one-dimensional conductive material in the conductive agent is between 1 wt.% and 100 wt.%.
[0015] A second aspect of the present invention also provides a method for preparing the above-mentioned electrode sheet, characterized in that the steps include: mixing an electrochemically active material, a conductive agent and a binder, and pressing them into shape to obtain a dry electrode; or, mixing an electrochemically active material, a conductive agent and a binder and a solvent, preparing a slurry, coating it onto a current collector and drying it to obtain a wet electrode.
[0016] A third aspect of the present invention also provides a battery comprising the electrodes described above; or, the dry electrode or the wet electrode obtained by the preparation method described above.
[0017] A fourth aspect of the present invention is a means of transportation comprising the aforementioned battery.
[0018] The beneficial technical effects of this invention are as follows:
[0019] 1. The active material layer of the electrode sheet of the present invention disperses a one-dimensional hollow, open-ended, one-dimensional conductive material. This one-dimensional conductive material acts as a "major artery" in the electrode sheet, enabling the rapid transport of lithium ions and electrons simultaneously. When the electrode sheet is installed in the battery, it is immersed in the electrolyte. During the charging and discharging process of the battery, the one-dimensional conductive material itself can transfer electrons, and the open-ended, hollow structure allows the electrolyte to be immersed within it, thereby achieving rapid ion transport and improving the power density of the battery.
[0020] 2. The electrode sheet of the present invention has a dual lithium-ion and electron transport channel, which not only significantly improves the lithium-ion and electron transport efficiency, but also solves the problem of electrolyte being difficult to wet in the electrode sheet with ultra-thick active material layer, thereby improving the energy density of the battery;
[0021] 3. The preparation method of the electrode sheet of the present invention is simple. It can be made by incorporating a one-dimensional conductive material with a specific structure into the electrochemical active material. It is applicable to industrialized electrode materials, battery production equipment and processes. It has low implementation cost and short time, and can quickly realize the production and application of products. It is economical and practical. Attached Figure Description
[0022] Figure 1 This is a schematic diagram illustrating the formation of the MXene nanorolls of the present invention;
[0023] Figure 2 XRD patterns (a) of the MAX phase material and the two-dimensional MXene material in Embodiment 1 of the present invention; SEM images of the MAX phase material (b) and the etched material (c, d);
[0024] Figure 3 SEM images of samples obtained in Example 1 of this invention with positive ion pair reagent mass concentrations of 1 wt.% (a), 5 wt.% (b), 10 wt.% (c), and 20 wt.% (d) and under stirring.
[0025] Figure 4 SEM image of a sample obtained in Example 1 of this invention with a positive ion-pairing reagent concentration of 20 wt.% but without stirring;
[0026] Figure 5 TEM image (a) and tube diameter distribution statistics (b) of MXene nanorolls obtained in Example 1 of this invention;
[0027] Figure 6 These are TEM images (a and b) and HRTEM images (c and d) of MXene nanorolls at different magnifications in Example 1 of the present invention.
[0028] Figure 7 This is an elemental distribution diagram of the MXene nanorolls in Example 1 of the present invention;
[0029] Figure 8 XRD patterns (a) of the MAX phase material and the two-dimensional MXene material in Embodiment 2 of the present invention; SEM images of the MAX phase material (b) and the two-dimensional MXene material (c);
[0030] Figure 9 TEM image (a) and tube diameter distribution statistics (b) of MXene nanorolls obtained in Example 2 of this invention;
[0031] Figure 10 The images shown are TEM images (a) and HRTEM images (b and c) at different magnifications of MXene nanorolls in Example 2 of this invention, and elemental distribution images (e-j).
[0032] Figure 11 XRD patterns (a) of the MAX phase material and the two-dimensional MXene material in Embodiment 3 of the present invention; SEM images of the MAX phase material (b) and the two-dimensional MXene material (c);
[0033] Figure 12 The images are SEM images of the two-dimensional MXene material in Example 3 of the present invention at stirring times of 1 min (a), 10 min (b), and 30 min (c).
[0034] Figure 13 V2AlC and V2CT in Embodiment 4 of the present invention x XRD patterns (a), SEM images of V2AlC (b), SEM (c), TEM (d), and HRTEM (e) images of MXene nanorolls;
[0035] Figure 14 SEM images of MXene nanorolls in Example 5 of the present invention (a) and SEM images of the composite cathode material at different magnifications (b, c);
[0036] Figure 15 The figures show the cycle performance (a and c), rate performance (b), and charge-discharge curve (d) of the composite electrode containing MXene nanorolls for each lithium-sulfur battery in Example 5 of the present invention at rates of 0.2C and 0.5C.
[0037] Figure 16 The figures (a) and (b) show the AC impedance test comparison of the lithium-sulfur battery in Example 8 of this invention.
[0038] Figure 17 The graph shows the electrochemical performance test results of the symmetrical cell with graphite electrode in Example 9 of this invention.
[0039] Figure 18 The graph shows the cycle performance test results (a) of the graphite electrode in Embodiment 10 of the present invention at a current density of 0.5C and the capacity comparison graph (b) after 60 cycles.
[0040] Figure 19 This is a comparison of the cycling performance of graphite electrodes with different conductive agents added in Example 10 of the present invention.
[0041] Explanation of key figure labels:
[0042] 10 Current collector; 20 Electrode layer; 21 Electrochemical active material; 22 One-dimensional conductive material; 23 Conductive carbon black; 30 Electrolyte. Detailed Implementation
[0043] The technical solution of the present invention is illustrated below through specific embodiments. It should be understood that the one or more steps mentioned in the present invention do not preclude the existence of other methods and steps before or after the combined steps, or that other methods and steps may be inserted between these explicitly mentioned steps. It should also be understood that these examples are for illustrative purposes only and are not intended to limit the scope of the present invention. Unless otherwise stated, the numbering of each method step is only for the purpose of identifying each method step, and not for limiting the order of each method or limiting the scope of the present invention. Changes or adjustments to their relative relationships, without substantial changes to the technical content, can also be considered as within the scope of the present invention.
[0044] The raw materials and instruments used in the examples are not subject to any specific restrictions on their source; they can be purchased from the market or prepared according to conventional methods known to those skilled in the art.
[0045] The technical concept of this invention lies in providing an electrode sheet in which a one-dimensional hollow conductive material is dispersed in an electrochemically active substance. The structure of the electrode sheet and a schematic diagram of lithium-ion and electron transport are shown below. Figure 1 As shown in figure a, it includes: a current collector 10 and an electrode layer 20 coated on the current collector 10, wherein the electrode layer 20 includes: an electrochemically active material 21, a one-dimensional conductive material 22 and a binder (not shown); wherein the one-dimensional conductive material 22 has a hollow structure with open ends. Figure 1 Figure b shows the structure of an electrode sheet using conductive carbon black 23 as a conductive agent in the prior art, and a schematic diagram of lithium-ion and electron transport. When the electrode sheet is installed in the battery and immersed in the electrolyte 30, during charging and discharging, due to the conductivity of the one-dimensional conductive material 22 itself, electrons are transported along the one-dimensional tube wall, and the path is significantly shorter than that of the granular conductive carbon black 23. Because the one-dimensional conductive material 22 has a hollow structure with open ends, the electrolyte can also enter the hollow interior, realizing lithium-ion transport. For coatings with thicker active material layers, it can also improve the technical problem of difficult electrolyte wetting, thereby improving the energy density and rate performance of the battery. A comparison also shows that granular conductive carbon black has more contact points with the electrochemical active material, and its contact resistance is higher than that of the one-dimensional conductive material.
[0046] The one-dimensional conductive material of this invention is a nanoroll structure formed by rolling up the two-dimensional material MXene. Besides its one-dimensional hollow structure with open ends, this nanoroll possesses two unique structural features: a linear one-dimensional structure and structural elasticity from the rolled-up structure. These two structural characteristics, when used in electrode sheets, can produce beneficial technical effects, including: the linear one-dimensional structure further reduces the transport path of lithium ions and electrons; the rolled-up structure, due to the ability of the tube diameter to slide through the overlapping layers, exhibits structural elasticity. For electrode materials that experience significant volume changes during charging and discharging, such as tin-based, silicon-based materials, transition metal oxides, sulfides, and alloys, this can also suppress volume changes during charging and discharging, preventing material structure collapse and particle agglomeration.
[0047] In this invention, a typical two-dimensional material, MXene, is selected and nanorolls are obtained by winding. The technical features of this invention are described in detail below through the MXene nanorolls obtained by winding two-dimensional MXene material.
[0048] Example 1
[0049] This embodiment provides an MXene nanoroll with the chemical formula V2B. 0.28 C 0.57 N 0.15 T x The specific steps of the preparation method are as follows:
[0050] 1) Preparation of two-dimensional MXene materials from MAX phase materials
[0051] MAX phase material V2AlB 0.28 C 0.57 N 0.15 Etching was performed at 90°C for 48 hours using an etchant to obtain a mixture (5 mg / ml) containing the etchant. The etchant was a mixture of concentrated hydrochloric acid (30 wt.%) and NaF, with a molar ratio of NaF to HCl of 1:1. The resulting etchant was a two-dimensional MXene material, labeled as V2(B). x C y N 1-x-y )T x ;
[0052] After centrifuging and washing the mixture containing the etching material, the resulting etching material was characterized. Figure 2XRD comparison of the MAX phase material and the etched material shows that the (002) diffraction peak of the etched material shifts to a lower angle, and the characteristic peaks of other MAX phases disappear. This is because the A component (Al element) in the MAX phase material is selectively etched, resulting in a two-dimensional MXene material with increased interlayer spacing between the sheets. SEM images show that the MAX phase material exhibits a typical layered bulk morphology. Figure 2 b); while the etched material exhibits a sheet-like, stacked accordion-like morphology ( Figure 2 (c) and (d) show a significant increase in interlayer spacing, consistent with the previous XRD pattern results. Figure 2 c also shows that the etched material has a sheet diameter of about 1μm to 10μm, with most of the sheets having a diameter of about 5μm.
[0053] 2) Fabrication of MXene nanorolls from two-dimensional MXene materials
[0054] 1 g of the etching material obtained in step 1 above was added to 50 ml of a 1 wt.%–20 wt.% tetrabutylammonium hydroxide (TBAOH) aqueous solution. After magnetic stirring (1500 r / min) for 5 min, the mixture was sonicated (1500 W) for 10 min, and then centrifuged and washed multiple times to obtain the purified sample. The stirring was performed with the rotor rotating in the same direction, providing directional flow of the liquid phase. Figure 3 SEM images of samples with TBAOH added at concentrations of 1 wt.%, 5 wt.%, 10 wt.%, and 20 wt.%, respectively, are shown in ax² to d. It can be seen that when 1 wt.% TBAOH is added, the edges of the two-dimensional MXene material exhibit a curled state. Figure 3 a) Increasing the TBAOH concentration to 5 wt.% resulted in more pronounced edge curling in the two-dimensional MXene material. Figure 3 b) Further increasing the TBAOH concentration to 10 wt.%, the two-dimensional MXene material in the sample mostly exhibited a nanoroll state. Figure 3 c) When the TBAOH concentration increased to 20 wt.%, the two-dimensional MXene material in the sample was completely transformed into MXene nanorolls. Figure 3 d). Figure 3 a~d clearly demonstrate the process of MXene nanorolls gradually forming from the curling of two-dimensional MXene materials, and the one-dimensional hollow nanoroll structure formed by the curling of the edges of the same two-dimensional MXene material. Figure 4 SEM images of a sample with 20 wt.% TBAOH added but without stirring are shown. The sample exhibits a thin and flexible morphology without curling, indicating that the external force generated by directional flow is crucial for the formation of MXene nanorolls.
[0055] The above examples also demonstrate that adding an appropriate amount of positive ion-pairing reagent to the liquid phase has a significant effect on accelerating the formation of MXene nanotubes. For example, adding 20 wt.% TBAOH only requires 5 minutes of stirring and 10 minutes of sonication to obtain fully curled MXene nanotubes. In contrast, adding only 1 wt.% TBAOH, under the same conditions, can produce curling, but not the formation of nanotube structures, requiring a longer stirring time. This can be explained by the fact that a higher concentration of positive ion-pairing reagent grafts more alkyl chains onto the surface of the two-dimensional MXene material, resulting in a greater external force under the same external force, thus facilitating the rapid formation of one-dimensional hollow roll structures.
[0056] Stirring induces unidirectional flow in the liquid phase, providing a continuous and uniform external force for the rolling process, which is crucial for obtaining large quantities and uniform MXene nanorolls. Characterization results show that the two-dimensional MXene material was almost completely transformed into MXene nanorolls, as demonstrated by SEM (e.g.,...). Figure 3 d) and TEM (e.g.) Figure 6 a) As shown in the photograph, this invention enables the large-scale preparation of uniformly monodisperse MXene nanorolls, which is of great significance for subsequent applications.
[0057] In other embodiments, the positive ion pairing reagent may also be one or more of tetramethylamine hydroxide, tetraethylamine hydroxide, tetrapropylamine hydroxide, tetrabutylamine hydroxide, or tetrapentylamine hydroxide. These reagents differ from TBAOH in this embodiment in that the length of the alkyl chain is different, and it is reasonable to predict that they can produce the same technical effect.
[0058] The obtained MXene nanorolls were subjected to transmission electron microscopy (TEM) analysis, such as... Figure 5 As shown in Figure a, it can be seen that MXene nanorolls have a significant one-dimensional morphology. The length of the MXene nanorolls is between 0.5 μm and 5 μm, corresponding to the diameter of the two-dimensional MXene sheet before winding. Each MXene nanoroll is independently dispersed (monodispersed). Figure 5 b. Statistical analysis of the diameter of MXene nanotubes showed that the diameter of the nanotubes ranged from 20nm to 80nm, with the highest content of MXene nanotubes at a diameter of 40nm, accounting for more than 40%.
[0059] Figure 6 Images a and b show TEM images of MXene nanorolls at different magnifications. It is clear that the MXene nanorolls possess a hollow roll structure formed by rolling up a single sheet of two-dimensional MXene material, exhibiting a straight one-dimensional morphology, open ends, and smooth walls. Figure 6The high-resolution electron microscopy (HRTEM) images c and d show that the walls of the MXene nanorolls consist of only 2 to 3 layers of MXene, with an interlayer spacing of 1.08 nm, meaning the wall thickness is only 3 to 4 nm. This ultra-thin wall indicates that the MXene nanorolls of this invention are formed by rolling up a single layer of MXene. Figure 6 d It can also be seen that the tube walls of MXene nanorolls show the typical hexagonal lattice of MXene, indicating that MXene nanorolls have a crystalline structure.
[0060] Figure 7 The elemental distribution of MXene nanorolls as shown by TEM analysis is presented. It can be seen that the MXene nanorolls contain V, B, C, N, O, and F elements, and these elements are uniformly distributed. O and F are functional group elements on the surface of the MXene nanorolls, and their chemical formula is V₂(B₂)₃. x C y N 1-x-y )T x match.
[0061] This invention does not limit the source of the MAX phase material; the MAX phase material can be commercially available or prepared by high-temperature sintering. For example, the MAX phase material V2AlB in this embodiment... 0.28 C 0.57 N 0.15 The material is prepared by high-temperature sintering. The steps include: sintering the elemental substances or compounds of each element according to the stoichiometric ratio in the chemical formula of the MAX phase material at high temperature. In this embodiment, more specifically, vanadium powder (V), aluminum powder (Al), boron powder (B), carbon powder (C), and nitrogen carbonide (CN) are mixed in a molar ratio of 2:1:0.85:0.42:0.15 and ball-milled. The mixture is then placed in a high-temperature sintering furnace and sintered at 1500°C for 24 hours under an argon atmosphere, and then cooled to room temperature.
[0062] In some embodiments, the etchant in step 1 can also be replaced with hydrofluoric acid solution, or a solution of NaF + nitric acid, NaF + sulfuric acid, LiF + hydrochloric acid, or Li + nitric acid; or other etching methods, such as accordion-shaped MXene material obtained by vapor phase etching.
[0063] Example 2
[0064] This embodiment provides another MXene nanoroll with the chemical formula: V2C 0.5 N 0.5 T x The preparation methods include:
[0065] 1) Preparation of two-dimensional MXene materials from MAX phase materials
[0066] MAX phase material V2AlC 0.5 N 0.5 A mixture of concentrated hydrochloric acid (30 wt.%) and NaF, with a molar ratio of NaF to HCl of 1:1, was used for etching at 90°C for 48 hours. The resulting etched material was a two-dimensional MXene material, labeled as: V2(C x N 1-x )T x .
[0067] pass Figure 8 The XRD comparison of a shows that, compared with the MAX phase material, the (002) diffraction peak of the etched material shifts to a lower angle, and the characteristic peaks of other MAX phases disappear. This is because the A component (Al element) in the MAX phase material is selectively etched, and the interlayer spacing between its sheets increases. Figure 8 SEM images b and c show that the MAX phase material exhibits a typical layered bulk morphology. After etching, the etched material exhibits an accordion-like morphology of stacked sheets, with a significantly increased interlayer spacing, which is consistent with the previous XRD pattern results. The sheet diameter is approximately between 5 μm and 15 μm.
[0068] 2) Obtaining MXene nanorolls by rolling up two-dimensional MXene materials
[0069] Add 1g of the above etching material to 50ml of a 30wt.% TBAOH aqueous solution, stir magnetically for 10min, and then centrifuge and wash several times to obtain the purified sample.
[0070] TEM test results of the sample are as follows Figure 9 As shown in a, it can be seen that the sample also exhibits a significant one-dimensional morphology. The length of the MXene nanorolls is greater than 5 μm, which corresponds to the sheet diameter of the two-dimensional MXene material before winding. This indicates that the MXene nanorolls of the present invention are obtained by rolling up two-dimensional MXene sheets. Figure 9 b. Statistical analysis of the diameter of MXene nanotubes showed that the diameter of hollow rolls ranged from 20nm to 140nm, with the highest content of MXene nanotubes at a diameter of 60nm, accounting for more than 30%.
[0071] Figure 10 The TEM image of a shows that the ports of the MXene nanorolls are open. Figure 10 b and c are HRTEM images, which show the hollow roll structure of MXene nanorolls, with approximately 3 to 6 MXene layers forming the tube walls. Figure 10e-j shows the elemental distribution of MXene nanorolls. It can be seen that MXene nanorolls contain V, C, N, O, and F elements, and these elements are uniformly distributed. O and F are functional group elements on the surface of the MXene nanorolls, and their chemical formula is V2(C). x N 1-x )T x match.
[0072] The MAX phase material in this embodiment is prepared by high-temperature sintering. The steps include: obtaining the elemental or compound form of each element by high-temperature sintering according to the elemental stoichiometry in the chemical formula of the MAX phase material. In this embodiment, V2AlC 0.5 N 0.5 The preparation method includes: mixing vanadium powder (V), aluminum powder (Al), aluminum nitride (AlN), and carbon powder in a molar ratio of 2:0.5:0.5:0.5 and ball milling them, then placing them in a high-temperature sintering furnace and sintering them at a high temperature of 1500℃ for 24 hours under an argon atmosphere, and then cooling them to room temperature to obtain the final product.
[0073] Example 3
[0074] This embodiment provides an MXene nanoroll with the chemical formula Ti3CNT. x The preparation method includes the following steps:
[0075] 1) Preparation of two-dimensional MXene materials from MAX phase materials
[0076] The MAX phase material Ti3AlCN was etched at 90 °C for 48 h using a mixture of concentrated hydrochloric acid (30 wt.%) and LiF, wherein the molar ratio of LiF to HCl was 1:1, to obtain a two-dimensional MXene material, labeled Ti3CNT. x .
[0077] pass Figure 11 The XRD comparison of a shows that, compared with the MAX phase material, the (002) diffraction peak of the etched material shifts to a lower angle, and the characteristic peaks of other MAX phases disappear. Figure 11 SEM images b and c show that the MAX phase material exhibits a typical layered bulk morphology; the etched material exhibits an accordion-like morphology of stacked sheets, with a significantly increased interlayer spacing. The sheet diameter is approximately 3μm to 5μm.
[0078] 2) Obtaining MXene nanorolls by rolling up two-dimensional MXene materials
[0079] The above-mentioned etching material was added to a 10 wt.% TBAOH aqueous solution, and after magnetic stirring for 30 min, it was centrifuged and washed multiple times to obtain a purified sample. Figure 12Images a through c show SEM images of samples stirred for 1 min, 10 min, and 30 min, respectively. They reveal that the two-dimensional MXene material gradually curls, eventually forming MXene nanorolls with a diameter of approximately 200 nm to 300 nm. This demonstrates that the duration of external force application influences the formation of MXene nanorolls. Extending the stirring time can also yield MXene nanorolls even at lower concentrations of positive ion-paired reagents.
[0080] Example 4
[0081] This embodiment provides MXene nanorolls with the chemical formula: V2CT x Preparation methods include:
[0082] 1) The MAX phase material V2AlC was etched at 90°C for 48 hours using concentrated hydrochloric acid-NaF etchant to obtain the two-dimensional MXene material V2CT. x ;
[0083] 2) The above two-dimensional MXene material was added to a 20 wt.% TBAOH intercalating agent solution, and after magnetic stirring for 5 min, it was centrifuged, washed and purified several times, and then dried to obtain MXene nanorolls;
[0084] Figure 13 a gives V2AlC and V2CT x XRD patterns; Figure 13 b provides a SEM image of V2AlC, which shows that it is a blocky material; Figure 13 c and d give the MXene nanoroll (V2CT) x The SEM and TEM images show that MXene nanorolls have a monodisperse one-dimensional hollow nanoroll morphology, with tube diameters ranging from 40 nm to 70 nm and lengths ranging from 2 to 5 μm. Figure 13 The image provided by e shows that the wall thickness of the MXene nanorolls is between 2 nm and 3 nm, indicating that they have ultrathin walls.
[0085] Using a similar method, the applicant has also prepared other types of MXene nanorolls with the same structural characteristics, including: Ti2CT x Ti3C2T x Nb2CT x TiNbCT x Cr2CT x Ti3CNT x Ti2CT x Ti2C 0.5 N 0.5 T x Ti 0.5V 0.5 C 0.5 N 0.5 T x V2CT x V2C 0.75 N 0.25 T x V2B 0.28 C 0.57 N 0.15 T x 、(V 0.8 Cr 0.2 )2B 0.33 C 0.67 T x 、(V 0.8 Cr 0.2 )2CT x 、(V 0.8 Fe 0.2 )2B 0.33 C 0.67 T x 、(V 0.8 Mn 0.2 )2B 0.33 C 0.67 T x 、(V 0.8 Fe 0.2 )2B 0.28 C 0.57 N 0.15 T x 、(V 0.8 Mn 0.2 )2B 0.28 C 0.57 N 0.15 T x Therefore, the preparation method of the present invention has a certain degree of universality for two-dimensional MXene materials and can be prepared in large quantities. The types of MXene nanorolls prepared by the present invention are not limited to the examples given in the above embodiments. Other types of two-dimensional MXene materials can be wound to obtain the MXene nanoroll structure of the present invention by adjusting the experimental methods and conditions.
[0086] Since the MXene nanorolls of the present invention are formed by rolling up two-dimensional MXene materials, the length of the MXene nanorolls in the one-dimensional direction is related to the sheet diameter of the two-dimensional MXene materials. For two-dimensional MXene materials, the sheet diameter can be distributed between 0.1 μm and 100 μm. Therefore, we can reasonably predict that the length of the MXene nanorolls can also be within this range.
[0087] Examples 1-4 above detail the preparation method, morphology, and structural characteristics of the MXene nanorolls of the present invention. To illustrate the conductivity of the MXene nanorolls as a conductive agent, the etched material obtained in the above examples was centrifuged, washed, dispersed in a solvent using ultrasonication, and then freeze-dried to obtain two-dimensional MXene material powder. More specifically, the etched material was dispersed in water (2 mg / ml), ultrasonically treated for 12 hours, and then freeze-dried. The prepared MXene nanoroll dispersion was centrifuged, concentrated, and then freeze-dried to obtain MXene nanoroll powder. The conductivity of both powders was tested using the four-probe method. The test method was as follows: 50 mg of powder sample was added to the sample cell of a four-probe powder resistivity meter, leveled, and then the meter was turned on. The handle was rotated to move the upper probe of the resistivity meter downwards, and then the pressure was increased to 15 MPa. After the resistivity meter reading stabilized, the resistivity reading was read, and then the conductivity was obtained according to the conversion relationship of conductivity = 1 / resistivity. The results are shown in the table below.
[0088]
[0089] As can be seen, in the powder state, the MXene nanorolls of this invention have an order of magnitude higher conductivity than two-dimensional MXene materials. This is because, on the one hand, MXene nanorolls have a one-dimensional structure, resulting in better directional conductivity; on the other hand, MXene nanorolls are connected in a one-dimensional network manner, and their contact resistance is significantly lower than that of two-dimensional MXene materials, belonging to a sheet-like connection. The MXene nanorolls of this invention exhibit excellent conductivity. Using the same method, carbon nanotube powder was tested, and its conductivity was less than 100 S cm⁻¹. -1 The significantly lower conductivity compared to the MXene nanotubes of this invention can be explained by the fact that MXene materials have better conductivity than carbon nanotube materials. In addition, the monodisperse structure can reduce contact resistance and the linear one-dimensional structure has better directional electron conduction.
[0090] Example 5
[0091] This embodiment provides an electrode sheet and its preparation method, wherein the electrochemically active material is sulfur, and the MXene nanorolls are selected from the MXene nanorolls (V2C) prepared in Example 2. 0.5 N 0.5 T x The preparation method of the electrode sheet includes the following steps:
[0092] 1) To prepare a composite of sulfur and MXene, elemental sulfur, MXene nanotubes and solvent are thoroughly mixed to dissolve elemental sulfur in the solvent, and then dried to remove the solvent, thereby obtaining a composite in which MXene nanotubes and elemental sulfur are fully and uniformly dispersed; preferably, the implementation step also includes further heating the composite to make the elemental sulfur more fully dispersed.
[0093] In some embodiments, the mass ratio of elemental sulfur to MXene nanorolls is between (1 to 10):1; preferably, it is between (4 to 5):1.
[0094] In some embodiments, the mixture or composite of MXene nanorolls and elemental sulfur is heated to a temperature between 112°C and 450°C; preferably, between 200°C and 300°C, so that the elemental sulfur rapidly forms a liquid state and enters the hollow tube.
[0095] In some embodiments, the heating time is between 0.1 h and 50 h, preferably 5 h to 10 h.
[0096] A more specific implementation method includes the following steps:
[0097] a) Mix elemental sulfur and MXene nanorolls at a mass ratio of 4:1, add toluene solvent and stir for 24 hours to obtain a viscous slurry. Place the slurry in a vacuum oven and dry at 60°C to obtain a composite of MXene nanorolls and elemental sulfur.
[0098] b) The composite from step a is placed in a high-temperature tube furnace and heated from room temperature to 280°C at a rate of 5°C / min under a protective gas atmosphere (argon). The temperature is held for 10 hours and then naturally cooled to obtain the composite cathode material.
[0099] Figure 14 The image provided shows an SEM image of MXene nanorolls, which reveals that they exhibit a distinct one-dimensional material morphology and are monodisperse. Figure 14 b and c show SEM images of the composite cathode material obtained after combining with elemental sulfur at different magnifications. It can be seen that MXene nanorolls are uniformly mixed with elemental sulfur.
[0100] 2) Prepare the positive electrode sheet by mixing the composite obtained in step b, carbon black (Ketjen black), and binder PVDF in a mass ratio of 8:1:1, then adding solvent NMP to prepare a slurry, uniformly coating it onto aluminum foil, and then drying it in a vacuum oven at 80°C for 24 hours to obtain the positive electrode sheet.
[0101] 3) Assemble the battery by assembling the positive electrode obtained in step 1 into a 2032 coin cell. Specifically, it includes a negative electrode shell, a positive electrode, a negative electrode (lithium metal sheet), 30 μl of electrolyte (LS-009), a separator, and a positive electrode shell to obtain the lithium-sulfur battery of the present invention.
[0102] Using the same method, the composite cathode material in step 1 was replaced with elemental sulfur to obtain a control battery.
[0103] After the assembled coin cells were left to stand for 8 hours, their electrochemical performance was tested. Figure 15 As shown in Figure a, at a rate of 0.2C, the lithium-sulfur battery of the present invention maintains a capacity of 600 mAh g after 300 cycles. -1 The above, in contrast, has a battery capacity of less than 200mAh g. -1 At a magnification of 0.5C ( Figure 15 c) The lithium-sulfur battery of the present invention retains a capacity of 400 mAh g after 500 cycles. -1 The above, in contrast, has a battery capacity of less than 100mAh g. -1 It is evident that the cycle performance of the composite cathode material of the present invention is significantly better than that of the elemental sulfur cathode material. Figure 15 Figure b shows a comparison of rate performance at different rates (0.2C to 4C). It can also be seen that the rate performance of the composite cathode material of this invention is better than that of elemental sulfur. Figure 15 d shows the charge-discharge curves of the lithium-sulfur battery of the present invention under different cycle numbers. It can be seen that the discharge curve shows a voltage plateau at around 2.07V.
[0104] Example 6
[0105] This embodiment provides another electrode sheet and its preparation method, the steps of which include: mixing electrochemical active material, conductive agent and binder, and pressing to obtain a dry electrode; taking silicon powder as the electrochemical material as an example, in a specific implementation, the steps include: mixing silicon powder, MXene nanofibers and PVDF in a mass ratio of 7:1.5:1.5; then loading the mixed powder into a powder feeder, and using a dry spraying machine to spray the powder onto a copper foil. After dry spraying, the electrode sheet is kept at a constant temperature of 175℃ (because the melting point of PVDF is 155~160℃) and hot-pressed to obtain an electrode sheet with silicon and MXene nanofibers as the active material layer.
[0106] Example 7
[0107] This embodiment provides another electrode sheet and its preparation method, the steps of which include: mixing electrochemical active material, MXene nanorolls, and binder, then adding solvent to prepare a slurry, coating it into a film, and drying it. Taking silicon powder as the electrochemical material as an example, the more specific steps include: mixing silicon powder, MXene nanorolls, and polytetrafluoroethylene (PVDF) in a mass ratio of 8:1:1, then adding N-methylpyrrolidone (NMP) solvent to prepare a slurry, then coating it onto copper foil to form a film, and vacuum drying it at 80°C to obtain an electrode sheet with silicon and MXene nanorolls as the active material layer.
[0108] Example 8
[0109] This embodiment provides another positive electrode sheet for lithium-sulfur batteries and its preparation method, the steps of which include:
[0110] Sulfur powder, MXene nanoroll conductive paste, and PVDF were ground uniformly in a mass ratio of 90:5:5. Then, several drops of NMP (N-methylpyrrolidone) solvent were added to obtain a uniform electrode paste. This electrode paste was then uniformly coated onto carbon-coated aluminum foil and vacuum dried to obtain a sulfur cathode. In this embodiment, a conductive paste with MXene nanorolls at a mass fraction of 30 wt.% and 40 wt.% was selected. The preparation method included:
[0111] 1. Take a certain amount of dispersant polyvinylidene fluoride (PVDF) and add it to the organic solvent N-methylpyrrolidone (NMP). Then stir at 600 rpm for 2 to 6 hours until the solution is a homogeneous and transparent liquid.
[0112] 2. Take a certain amount of MXene nanorolls and add them to the liquid that has been stirred and dispersed uniformly. Then, stir and disperse the liquid at a speed of 450 rpm to obtain an organic conductive paste containing MXene nanorolls.
[0113] Using the same method, replacing MXene nanotubes with carbon nanotubes yielded a carbon nanotube conductive paste with the same mass content.
[0114] The obtained sulfur cathode and the control sulfur cathode were assembled into a full cell. The assembly method was as follows: a 2032 coin cell was assembled using a lithium metal sheet as the negative electrode, a polypropylene separator, and an electrolyte (model LS-009). After assembly, the cells were allowed to stand for 9 hours before electrochemical performance testing. The AC impedance testing frequency was set to 0.01Hz~10Hz. 5 Hz, potential value set to 10mV; constant current charge-discharge curve test was performed at a current density of 0.5C.
[0115] Figure 16The results of the AC impedance test are presented, showing that, at the same mass content, the battery impedance of the MXene nanoroll conductive paste is significantly lower than that of the carbon nanotube conductive paste. This can be attributed to the good conductivity and dispersibility (monodispersive characteristics) of MXene nanorolls. Specifically, the addition of 40% MXene-V2CT... x The battery with nano-roll conductive paste exhibits lower impedance, indicating that the increase in conductive components is beneficial to improving the conductivity of the electrode sheet and reducing impedance. Figure 16 b presents the cycling performance tests of full cells with MXene nanoroll conductive paste and carbon nanotube conductive paste (40 wt.%) respectively at a rate of 0.5C. It can be seen that the full cell with MXene nanoroll conductive paste of the present invention has a significantly better capacity retention than the full cell with carbon nanotube conductive paste.
[0116] The above tests demonstrate that the MXene nanoroll conductive paste of this invention exhibits significantly superior conductivity compared to carbon nanotube conductive paste in battery applications. Structurally, both MXene nanorolls and carbon nanotubes are one-dimensional materials. However, MXene nanorolls possess a linear one-dimensional structure with open ends, resulting in monodisperse aggregates that are easily dispersed and do not agglomerate. In contrast, carbon nanotubes are grown through gas-phase pyrolysis under the action of a catalyst, typically forming curved one-dimensional lines with closed ends. Their aggregates are intertwined, making them prone to agglomeration and difficult to disperse. Therefore, MXene nanorolls dispersed in electrode sheets exhibit superior conductivity. The superior electrochemical performance compared to carbon nanotubes is attributed to the dispersion and shorter transport path brought about by the linear one-dimensional structure of MXene nanorolls, as well as the fact that the hollow structure enables the simultaneous transport of lithium ions and electrons, reducing battery impedance and thus exhibiting excellent electrochemical performance. In addition, since MXene nanorolls are hollow roll structures formed by winding, the inner diameter of the hollow tubes can be adjusted by the sliding of the rolled-up layers, thus giving MXene nanorolls structural elasticity. When combined with elemental sulfur, MXene nanorolls may also act as a buffer material, limiting the volume change of elemental sulfur during charge and discharge.
[0117] Example 9
[0118] This embodiment provides a lithium-ion battery negative electrode sheet and its preparation method, more specifically an electrode sheet with graphite as the electrochemical active material, and assembling the electrode into a symmetrical battery, the steps of which include:
[0119] 1. Graphite, MXene nanotube powder, and PVDF were ground uniformly in a mass ratio of 8:1:1. Then, several drops of NMP (N-methylpyrrolidone) solvent were added to obtain a uniform electrode slurry. The electrode slurry was then coated onto a uniform copper foil and vacuum dried to obtain a graphite electrode. The MXene nanotube powder was replaced with carbon nanotubes to obtain a control electrode.
[0120] 2. Assemble the button cell in the following order: negative electrode shell - lithium sheet - PP separator - LB-092 electrolyte - graphite electrode - gasket - spring contact - positive electrode shell. After assembly, let it stand for 9 hours, then test at 1 mAcm. -2 The battery was discharged at a certain current density. After the discharge was completed, the battery was disassembled and the graphite electrode with lithium deposited on its surface (labeled as: graphite / Li electrode) was removed. The graphite electrode was replaced with a control electrode using the same method to obtain a control electrode with lithium deposited on its surface (labeled as control / Li electrode).
[0121] 3. The graphite electrode with deposited lithium obtained in step 2 above is used to assemble a coin cell in the following order: negative electrode shell - graphite / Li electrode - PP separator - graphite / Li electrode - gasket - spring sheet - positive electrode shell, to obtain a graphite / Li symmetric cell; the graphite / Li electrode is replaced with a contrast / Li electrode using the same method to obtain a contrast / Li symmetric cell.
[0122] After the battery is assembled, it should be left to stand for 9 hours before testing. The testing method is as follows: the assembled symmetrical battery is subjected to 1 mA / cm². 2 Current density, 1mAh / cm 2 Electrochemical tests were performed at the areal capacity, and the results are as follows: Figure 17 As shown, after 400 hours of cycling, the potential of the graphite / Li electrode containing MXene nanotubes stabilizes at around 45 mV, while the polarization potential of the contrast / Li electrode containing carbon nanotubes is around 100 mV.
[0123] Example 10
[0124] To illustrate the technical advantages of MXene nanorolls compared to other types of conductive agents in electrode sheets, and further to evaluate the impact of MXene nanoroll materials on electrode performance with different loadings (thicknesses), this embodiment provides a comparison of MXene nanorolls with conductive materials such as MXene nanosheets, Ketjen black, graphene, and carbon nanotubes (CNTs) used in graphite electrodes. The MXene nanorolls used are V2CT from Example 4. x MXene nanorolls.
[0125] The electrode and battery were prepared as follows: Graphite, MXene nanofibers, and PVDF were mixed in a mass ratio of 90:5:5. NMP was added to prepare a slurry, which was then coated onto copper foil with loadings of 4, 6, 8, and 10 mg / cm³ using a doctor blade of different heights. 2 The electrodes were loaded and then vacuum dried to obtain the electrodes. The electrode sheets were then assembled into a full cell using the following sequence: negative electrode shell-negative electrode-separator-electrolyte-lithium sheet-pad-spring sheet-positive electrode shell. Cyclic testing was performed at a current density of 0.5C. Using the same method, MXene nanorolls were replaced with Ketjen Black, carbon nanotubes (CNTs), and graphene to obtain a control electrode and a control cell.
[0126] like Figure 18 As shown in a and b, the loading amount is 4 mg / cm³. 2 Cycling performance tests of each electrode at a current density of 0.5C showed that the electrode containing MXene nanorolls exhibited the best cycling capacity, maintaining 312.2 mAh / g even after 60 cycles. This capacity is higher than that of current conductive agents such as Ketjen Black, CNTs, graphene, and MXene nanosheets as additives. This demonstrates that adding MXene nanorolls to the electrode can effectively improve the capacity of the electrode material.
[0127] like Figure 19 Figures a through c show the cycling performance of MXene nanorolls, Ketjen black, and carbon nanotubes (CNTs) as conductive agents under different loading levels. It can be seen that, at the same loading level (thickness), MXene nanorolls exhibit higher capacity and better cycling stability compared to Ketjen black and CNTs. Furthermore, as the loading level (thickness) increases, MXene nanorolls, due to their good conductivity and high uniformity, improve the electrochemical performance of the electrode at high loading levels, even at 10 mg / cm². 2 Even with a high loading, the electrochemical performance of MXene nanorolls remains excellent. However, the battery capacity of Ketjenblack and CNT materials significantly decreases with increasing loading. This demonstrates the promoting effect of MXene nanorolls on the application of thick electrodes.
[0128] The above technical effects have been verified through laboratory coin cell experiments. Furthermore, the loading of active materials in the electrode sheet can be further increased through process optimization, aiming for a loading of 10 mg / cm³. 2 This increases the battery's energy and volumetric density. Different electrochemical substances may have different optimal loading rates, which can be determined through a finite number of optimizations.
[0129] In the above embodiments, the electrochemically active material can also be replaced with other existing electrode materials, such as, for lithium-ion batteries, cathode materials such as: lithium iron phosphate (LiFePO4), lithium cobalt oxide (LiCoO2), lithium manganese oxide (LiMn2O4), lithium nickel oxide (LiNiO2), and ternary materials (LiNi... x Co y Mn y O2, where x+y+z=1); negative electrode materials such as silicon, silicon oxide, and silicon suboxide. Of course, the conductive agent or conductive paste of this invention can also be applied to other types of batteries, such as lead-acid batteries, sodium-ion batteries, and zinc-ion batteries.
[0130] The foregoing description of specific exemplary embodiments of the invention is for illustrative and explanatory purposes. These descriptions are not intended to limit the invention to the precise forms disclosed, and it will be apparent that many changes and variations can be made in accordance with the foregoing teachings. The exemplary embodiments were chosen and described in order to explain the specific principles of the invention and its practical application, thereby enabling those skilled in the art to implement and utilize various different exemplary embodiments of the invention, as well as various different choices and variations. The scope of the invention is intended to be defined by the claims and their equivalents.
Claims
1. An electrode sheet, comprising a current collector and an active material layer in contact with the current collector, characterized in that, The active material layer includes: an electrochemical active material, a conductive agent, and a binder; wherein the conductive agent includes: a one-dimensional conductive material that is hollow and open at both ends, wherein the one-dimensional conductive material is an MXene nanoroll formed by rolling up the two-dimensional material MXene, and the one-dimensional morphology of the one-dimensional conductive material is linear; the diameter of the nanoroll is between 10 nm and 200 nm.
2. The electrode sheet as described in claim 1, characterized in that, The nanorolls are formed by rolling up a single sheet of the two-dimensional material MXene; And / or, the nanorolls are formed by rolling up a single layer of the two-dimensional material MXene.
3. The electrode sheet as described in claim 1, characterized in that, The thickness of the tube wall of the one-dimensional conductive material is between 0.3 nm and 10 nm; And / or, the length of the nanoroll is between 0.1 μm and 100 μm; And / or, the diameter of the nanoroll is between 40 nm and 200 nm.
4. The electrode sheet as described in claim 2, characterized in that, The chemical formula of MXene is M n+1 X n T x Where M is selected from one or more transition metal elements, and X is selected from one, two, or three of carbon, nitrogen, or boron. n T is 1, 2, 3 or 4. x For functional groups.
5. The electrode sheet as described in claim 4, characterized in that, The transition metal element is selected from one, two, or three of the following: Ti, V, Nb, Cr, Ta, Hf, Mo, W, Fe, Mn, Y, or Sc.
6. The electrode sheet as described in claim 4 or 5, characterized in that, The chemical formula of the MXene is selected from one or more of the following: V2C 0.5 N 0.5 T x 、Ti3CNT x 、V2CT x 、Ti3C2T x 、Nb2CT x 、TiNbCT x 、Cr2CT x 、Ti2CT x 、Ti2C 0.5 N 0.5 T x 、Ti 0.5 V 0.5 C 0.5 N 0.5 T x 、V2C 0.75 N 0.25 T x 、V2B 0.28 C 0.57 N 0.15 T x 、(V 0.8 Cr 0.2 )2B 0.33 C 0.67 T x 、(V 0.8 Cr 0.2 )2CT x 、(V 0.8 Fe 0.2 )2B 0.33 C 0.67 T x 、(V 0.8 Mn 0.2 )2B 0.33 C 0.67 T x 、(V 0.8 Fe 0.2 )2B 0.28 C 0.57 N 0.15 T x 、(V 0.8 Mn 0.2 )2B 0.28 C 0.57 N 0.15 T x 。 7. The electrode sheet according to any one of claims 1 to 5, characterized in that, The electrochemically active material is selected from: lithium-ion battery cathode material, or lithium-based battery anode material; And / or, the conductive agent may further include a two-dimensional conductive material or a zero-dimensional material.
8. The electrode sheet as described in claim 7, characterized in that, The positive electrode material of the lithium-ion battery is selected from one of lithium iron phosphate, lithium cobalt oxide, lithium manganese oxide, lithium nickel oxide, ternary materials, and elemental sulfur; the negative electrode material of the lithium-based battery includes one of silicon, silicon oxide, silicon suboxide, and graphite. And / or, the two-dimensional conductive material is selected from one or more of the following: two-dimensional MXene material, graphene, and graphite sheets; the zero-dimensional material is selected as carbon black.
9. The electrode sheet as described in claim 1, characterized in that, According to the proportion of quality The electrochemically active substance, 70-100 parts; 1-10 parts of conductive agent; 1-10 parts adhesive; The mass percentage of the one-dimensional conductive material in the conductive agent is between 1 wt.% and 100 wt.%.
10. A method for preparing an electrode sheet as described in any one of claims 1 to 9, characterized in that, step include: A dry electrode is obtained by mixing electrochemical active materials, conductive agents and binders and pressing them into shape. Alternatively, an electrochemically active material, a conductive agent, a binder, and a solvent are mixed to form a slurry, which is then coated onto a current collector and dried to obtain a wet electrode.
11. The preparation method according to claim 10, characterized in that, The preparation steps of MXene nanorolls include: dispersing accordion-shaped etched material obtained by etching two-dimensional MXene material or MAX phase material in a liquid phase containing positive ion pairing reagent, forming liquid phase flow under the action of external force, and obtaining the MXene nanorolls.
12. The preparation method according to claim 11, characterized in that, The positive ion pairing reagent is selected from one or more of tetramethylamine hydroxide, tetraethylamine hydroxide, tetrapropylamine hydroxide, tetrabutylamine hydroxide, or tetrapentylamine hydroxide; And / or, the external force is: stirring, or, stirring and ultrasound.
13. The preparation method according to claim 12, characterized in that, The stirring is a directional rotation.
14. A battery, characterized in that, It contains an electrode sheet as described in any one of claims 1 to 9; or, the dry electrode or the wet electrode obtained by the preparation method as described in any one of claims 10 to 13.
15. A means of transportation, characterized in that, It contains the battery as described in claim 14.
16. The use of MXene nanorolls as a conductive agent in battery electrode sheets, characterized in that, The MXene nanoroll has a one-dimensional hollow rolled structure with openings at both ends, formed by rolling up the two-dimensional material MXene; the one-dimensional morphology of the one-dimensional conductive material is linear; the diameter of the nanoroll is between 10 nm and 200 nm.
Citation Information
Patent Citations
Rapid preparation method of MXene film with high volumetric specific capacitance
CN111017890A
Ti3C2Tx MXene one-dimensional hollow nanotube as well as preparation method and application thereof
CN113201807A