Metal composite electrode material, method for producing the same, battery, and vehicle

By using MXene nanorolls to composite with metals to form a hollow roll structure, the conductivity and stability problems of lithium-ion battery anode materials are solved, achieving high-efficiency electrochemical performance and stability of the battery, which is suitable for metal batteries in transportation vehicles.

CN116779833BActive Publication Date: 2026-11-24BEIHANG UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202210225222.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-09
Publication Date
2026-11-24
Estimated Expiration
2042-03-09

AI Technical Summary

Technical Problem

Existing lithium-ion battery anode materials such as MoS₂ and MXenes suffer from poor conductivity, poor cycle performance, and poor rate performance. In particular, MoS₂ is prone to agglomeration, and MXenes suffers from severe layer stacking, which limits their application in the field of lithium storage.

Method used

Using MXene nanorolls as a metal encapsulation material, a hollow roll structure is formed by combining electrochemically active metals with MXene nanorolls. The unique morphology and lithium affinity of MXene nanorolls enable the stable storage and release of metals and their uniform dispersion in the battery.

Benefits of technology

It improves the electrochemical performance of the battery, solves the problems of conductivity and stability, realizes the stable manufacturing of metal batteries in the air environment and excellent electrochemical performance, buffers electrode volume changes, and enhances the cycle performance and rate performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116779833B_ABST
    Figure CN116779833B_ABST
Patent Text Reader

Abstract

This invention discloses a metal composite electrode material, its preparation method, battery, and transportation vehicle. The metal composite electrode material comprises an electrochemically active metal and MXene nanorolls, wherein the MXene nanorolls are MXene materials with a one-dimensional hollow roll structure. The MXene nanoroll structure facilitates the adsorption and encapsulation of metals, enabling stable storage and release of metals that are unstable in air. This greatly simplifies the harsh environment problem in metal battery manufacturing, making it possible to manufacture metal batteries in an air environment. The one-dimensional morphology of the MXene nanorolls themselves exhibits monodispersity, eliminating the phenomenon of two-dimensional sheet stacking, allowing for uniform dispersion within the metal and improving the electrochemical performance of the metal battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of new materials and batteries, and in particular relates to a metal composite electrode material, its preparation method, uses, batteries, and transportation vehicles. Background Technology

[0002] Lithium-ion batteries, with their advantages of high energy density, high output power, low self-discharge, and environmental friendliness, have experienced rapid development and widespread application since their successful development in the 1990s. With the rapid development of electric vehicles and portable electronic products, higher demands are being placed on the energy density of lithium-ion batteries, necessitating the development of anode materials with higher lithium storage capacity. Currently, the main anode materials for lithium-ion batteries are carbon materials. Although their cycle performance and safety are good, their theoretical specific capacity severely limits their application areas and cannot meet the demand for high-capacity batteries. In recent years, the application of two-dimensional materials in battery lithium storage has been extensively studied, with MoS2 and MXenes being typical examples. MoS2 materials, due to their nanolayered structure and large specific surface area, can achieve a lithium storage specific capacity of 800-1000 mAh / g, far exceeding that of graphite anodes.

[0003] However, due to its tendency to aggregate and poor conductivity, its cycle performance and rate performance are poor. While MXenes sheet materials have good conductivity and abundant surface functional groups, their theoretical capacity is low, and they suffer from severe sheet stacking, which seriously limits their application in lithium storage. Therefore, developing a lithium storage material with good conductivity, high theoretical capacity, high dispersion, and low susceptibility to stacking is key to promoting the further widespread application of lithium batteries. Summary of the Invention

[0004] The object of the present invention is to provide, in a first aspect, the use of MXene nanorolls as metal encapsulation, wherein the MXene nanorolls are MXene materials having a one-dimensional hollow roll structure.

[0005] A second aspect of the present invention provides a metal composite electrode material comprising an electrochemically active metal and the aforementioned MXene nanorolls.

[0006] In some embodiments, the hollow roll is filled with the electrochemically active metal; and / or, the mass ratio of the electrochemically active metal to the MXene nanoroll is between (0.1 and 10):1.

[0007] In some embodiments, the MXene nanorolls are open at both ends; and / or, the MXene nanorolls have a linear one-dimensional morphology; and / or, the hollow roll structure is formed by rolling up a monolithic two-dimensional MXene material; and / or, the hollow roll structure is formed by rolling up a single layer of the two-dimensional MXene material.

[0008] In some embodiments, the wall thickness of the MXene nanoroll is between 0.3 nm and 50 nm; and / or, the length of the MXene nanoroll is between 0.1 μm and 100 μm; and / or, the diameter of the MXene nanoroll is between 10 nm and 200 nm.

[0009] In some embodiments, the electrochemically active metal is selected from at least one of lithium, sodium, potassium, calcium, magnesium, or zinc; and / or, the chemical formula of the MXene nanorolls is represented as M. n+1 X n T x Where M includes one, two, or more of the elements Ti, V, Nb, Cr, Ta, Hf, Mo, W, Fe, Mn, Y, or Sc; X is selected from one, two, or three of the elements carbon, nitrogen, or boron; n is 1, 2, 3, or 4; T x The functional group includes elements of the sixth and / or seventh main groups.

[0010] A third aspect of the present invention provides a method for preparing the above-mentioned metal composite electrode material, comprising the steps of: converting an electrochemically active metal into a liquid state; and mixing the liquid metal with MXene nanorolls.

[0011] In some embodiments, the above preparation method further includes the steps of: preparing MXene nanorolls into a thin film; and then contacting the thin film with a liquid metal.

[0012] A fourth aspect of the present invention provides a metal battery comprising the metal composite electrode material described above; or a metal electrode material obtained by the preparation method described above.

[0013] A fifth aspect of the present invention provides a vehicle comprising the aforementioned metal battery.

[0014] The beneficial technical effects achievable by this invention lie in the superior electrochemical performance of the MXene nanoroll-metal composite electrode. This can be attributed to the fact that the MXene nanoroll structure facilitates the adsorption and encapsulation of metals, enabling stable storage and release of metals that are unstable in air. This greatly simplifies the harsh environment challenges of metal battery manufacturing, making manufacturing in an air environment possible. Furthermore, the monodisperse one-dimensional morphology of the MXene nanorolls eliminates the phenomenon of two-dimensional sheet stacking, allowing for uniform dispersion within the metal and improving the electrochemical performance of the metal battery. Additionally, the unique roll-like structure of the MXene nanorolls, with adjustable tube diameter, provides structural elasticity, acting as a buffer against changes in electrode volume within the metal electrode. Attached Figure Description

[0015] Figure 1 XRD patterns (a) of the MAX phase material and the two-dimensional MXene material in Embodiment 1 of the present invention; SEM images of the MAX phase material (b) and the etched material (c, d);

[0016] Figure 2 SEM images of samples obtained in Example 1 of this invention with positive ion pair reagent mass concentrations of 1 wt.% (a), 5 wt.% (b), 10 wt.% (c), and 20 wt.% (d) and under stirring.

[0017] Figure 3 SEM image of a sample obtained in Example 1 of this invention with a positive ion-pairing reagent concentration of 20 wt.% but without stirring;

[0018] Figure 4 TEM image (a) and tube diameter distribution statistics (b) of MXene nanorolls obtained in Example 1 of this invention;

[0019] Figure 5 These are TEM images (a and b) and HRTEM images (c and d) of MXene nanorolls at different magnifications in Example 1 of the present invention.

[0020] Figure 6 This is an elemental distribution diagram of the MXene nanorolls in Example 1 of the present invention;

[0021] Figure 7 XRD patterns (a) of the MAX phase material and the two-dimensional MXene material in Embodiment 2 of the present invention; SEM images of the MAX phase material (b) and the two-dimensional MXene material (c);

[0022] Figure 8 TEM image (a) and tube diameter distribution statistics (b) of MXene nanorolls obtained in Example 2 of this invention;

[0023] Figure 9 The images shown are TEM images (a) and HRTEM images (b and c) at different magnifications of MXene nanorolls in Example 2 of this invention, and elemental distribution images (e-j).

[0024] Figure 10 XRD patterns (a) of the MAX phase material and the two-dimensional MXene material in Embodiment 3 of the present invention; SEM images of the MAX phase material (b) and the two-dimensional MXene material (c);

[0025] Figure 11 The images are SEM images of the two-dimensional MXene material in Example 3 of the present invention at stirring times of 1 min (a), 10 min (b), and 30 min (c).

[0026] Figure 12 V2AlC and V2CT in Embodiment 4 of the present invention x XRD patterns (a), SEM images of V2AlC (b), SEM (c), TEM (d), and HRTEM (e) images of MXene nanorolls;

[0027] Figure 13 SEM images (a) of the surface of the MXene nanofilm in Example 5 of the present invention and (b) of the stamped wafer are shown.

[0028] Figure 14 The images shown are (a) a photograph of the disc immediately after being placed into molten lithium metal in Example 5 of the present invention, (b) a photograph after 3 minutes, (c) a photograph after cooling to room temperature, and (d) a photograph after being exposed to air for one day.

[0029] Figure 15 These are SEM images (a-c) of the surface of the lithium metal composite electrode material in Example 5 of the present invention at different magnifications.

[0030] Figure 16 These are SEM images (a-c) of the cross-section of the lithium metal composite electrode material in Example 5 of the present invention at different magnifications.

[0031] Figure 17 This is an HRTEM image of the lithium metal composite electrode material in Example 5 of the present invention;

[0032] Figure 18 The results of the discharge test of the lithium metal composite electrode material in Example 5 of this invention after being placed for one day;

[0033] Figure 19 In Embodiment 5 of the present invention, 1mA cm -2 1mAh cm -2 Cyclic performance (a) and rate performance (b) of MXene nanorolls at various rates. Detailed Implementation

[0034] The technical solution of the present invention is illustrated below through specific embodiments. It should be understood that the one or more steps mentioned in the present invention do not preclude the existence of other methods and steps before or after the combined steps, or that other methods and steps may be inserted between these explicitly mentioned steps. It should also be understood that these examples are for illustrative purposes only and are not intended to limit the scope of the present invention. Unless otherwise stated, the numbering of each method step is only for the purpose of identifying each method step, and not for limiting the order of each method or limiting the scope of the present invention. Changes or adjustments to their relative relationships, without substantial changes to the technical content, can also be considered as within the scope of the present invention.

[0035] The raw materials and instruments used in the examples are not subject to any specific restrictions on their source; they can be purchased from the market or prepared according to conventional methods known to those skilled in the art.

[0036] Example 1

[0037] This embodiment provides an MXene nanoroll with the chemical formula V2B. 0.28 C 0.57 N 0.15 T x The specific steps of the preparation method are as follows:

[0038] 1) Preparation of two-dimensional MXene materials from MAX phase materials

[0039] MAX phase material V2AlB 0.28 C 0.57 N 0.15 Etching was performed at 90°C for 48 hours using an etchant to obtain a mixture (5 mg / ml) containing the etchant. The etchant was a mixture of concentrated hydrochloric acid (30 wt.%) and NaF, with a molar ratio of NaF to HCl of 1:1. The resulting etchant was a two-dimensional MXene material, labeled as V2(B). x C y N 1-x-y )T x ;

[0040] After centrifuging and washing the mixture containing the etching material, the resulting etching material was characterized. Figure 1 XRD comparison of the MAX phase material and the etched material shows that the (002) diffraction peak of the etched material shifts to a lower angle, and the characteristic peaks of other MAX phases disappear. This is because the A component (Al element) in the MAX phase material is selectively etched, resulting in a two-dimensional MXene material with increased interlayer spacing between the sheets. SEM images show that the MAX phase material exhibits a typical layered bulk morphology. Figure 1b); while the etched material exhibits a sheet-like, stacked accordion-like morphology ( Figure 1 (c) and (d) show a significant increase in interlayer spacing, consistent with the previous XRD pattern results. Figure 1 c also shows that the etched material has a sheet diameter of about 1μm to 10μm, with most of the sheets having a diameter of about 5μm.

[0041] 2) Fabrication of MXene nanorolls from two-dimensional MXene materials

[0042] Add 1 wt.% to 20 wt.% of tetrabutylammonium hydroxide (TBAOH) aqueous solution to the etching material obtained in step 1 above, stir magnetically (1500 r / min) for 5 min, then sonicate (1000 W) for 30 min, and centrifuge and wash multiple times to obtain the purified sample.

[0043] Figure 2 SEM images of samples with TBAOH added at concentrations of 1 wt.%, 5 wt.%, 10 wt.%, and 20 wt.%, respectively, are shown in ax² to d. It can be seen that when 1 wt.% TBAOH is added, the edges of the two-dimensional MXene material exhibit a curled state. Figure 2 a) Increasing the TBAOH concentration to 5 wt.% resulted in more pronounced edge curling in the two-dimensional MXene material. Figure 2 b) Further increasing the TBAOH concentration to 10 wt.%, the two-dimensional MXene material in the sample mostly exhibited a nanoroll state. Figure 2 c) When the TBAOH concentration increased to 20 wt.%, the two-dimensional MXene material in the sample was completely transformed into MXene nanorolls. Figure 2 d). Figure 2 a~d clearly demonstrate the process of MXene nanorolls gradually forming from the curling of two-dimensional MXene materials, and the one-dimensional hollow nanoroll structure formed by the curling of the edges of the same two-dimensional MXene material. Figure 3 SEM images of a sample with 20 wt.% TBAOH added but without stirring or sonication are shown. The sample exhibits a thin and flexible morphology but does not curl, indicating that external force is crucial for the formation of MXene nanorolls.

[0044] The above examples also demonstrate that adding an appropriate amount of positive ion-pairing reagent to the liquid phase significantly accelerates the formation of MXene nanotubes. For instance, adding 20 wt.% TBAOH only requires 5 minutes of stirring and 10 minutes of sonication to obtain fully curled MXene nanotubes. In contrast, adding only 1 wt.% TBAOH, while producing curling under the same conditions, does not result in nanotube structures and requires extended stirring time. This can be explained by the fact that higher concentrations of positive ion-pairing reagent graft more alkyl chains onto the surface of the two-dimensional MXene material, resulting in a greater external force under the same force, thus facilitating the rapid formation of one-dimensional hollow roll structures. In the optimized experiments, the amount of positive ion-pairing reagent added can range from 1 wt.% to 50 wt.%. The optimal amount can be obtained through a limited number of experiments, depending on the type of MXene material and the negative charge on its surface.

[0045] Stirring induces unidirectional flow in the liquid phase, providing a continuous and uniform external force for the rolling process, which is crucial for obtaining large quantities and uniform MXene nanorolls. Characterization results show that the two-dimensional MXene material was almost completely transformed into MXene nanorolls, as demonstrated by SEM (e.g.,...). Figure 2 d) and TEM (e.g.) Figure 6 a) As shown in the photograph, this invention enables the large-scale preparation of uniformly monodisperse MXene nanorolls, which is of great significance for subsequent applications.

[0046] In other embodiments, the positive ion pairing reagent may also be selected from one or more of tetraethylammonium hydroxide, tetrapropylammonium hydroxide, or tetrapentylammonium hydroxide. These reagents differ from TBAOH in this embodiment in that the length of the alkyl chain is different, and it is reasonable to predict that they can also produce the same technical effect.

[0047] The obtained MXene nanorolls were subjected to transmission electron microscopy (TEM) analysis, such as... Figure 4 As shown in Figure a, it can be seen that MXene nanorolls have a significant one-dimensional morphology. The length of the MXene nanorolls is between 0.5 μm and 5 μm, corresponding to the sheet diameter of the two-dimensional MXene material before winding. Each MXene nanoroll is independently dispersed (monodispersed). Figure 4 b. Statistical analysis of the diameter of MXene nanotubes showed that the diameter of the nanotubes ranged from 20nm to 80nm, with the highest content of MXene nanotubes at a diameter of 40nm, accounting for more than 40%.

[0048] Figure 5Images a and b show TEM images of MXene nanorolls at different magnifications. It is clear that the MXene nanorolls possess a hollow roll structure formed by rolling up a single sheet of two-dimensional MXene material, exhibiting a straight one-dimensional morphology, open ends, and smooth walls. Figure 5 The high-resolution electron microscopy (HRTEM) images c and d show that the walls of the MXene nanorolls consist of only 2 to 3 layers of MXene, with an interlayer spacing of 1.08 nm, meaning the wall thickness is only 3 to 4 nm. This ultra-thin wall indicates that the MXene nanorolls of this invention are formed by rolling up a single layer of two-dimensional MXene material. Figure 5 d It can also be seen that the tube walls of MXene nanorolls show the typical hexagonal lattice of MXene, indicating that MXene nanorolls have a crystalline structure.

[0049] Figure 6 The elemental distribution of MXene nanorolls as shown by TEM analysis is presented. It can be seen that the MXene nanorolls contain V, B, C, N, O, and F elements, and these elements are uniformly distributed. O and F are functional group elements on the surface of the MXene nanorolls, and their chemical formula is V₂(B₂)₃. x C y N 1-x-y )T x match.

[0050] This invention does not limit the source of the MAX phase material; the MAX phase material can be commercially available or prepared by high-temperature sintering. For example, the MAX phase material V2AlB in this embodiment... 0.28 C 0.57 N 0.15 The material is prepared by high-temperature sintering. The steps include: sintering the elemental substances or compounds of each element according to the stoichiometric ratio in the chemical formula of the MAX phase material at high temperature. In this embodiment, more specifically, vanadium powder (V), aluminum powder (Al), boron powder (B), carbon powder (C), and nitrogen carbonide (CN) are mixed in a molar ratio of 2:1:0.85:0.42:0.15 and ball-milled. The mixture is then placed in a high-temperature sintering furnace and sintered at 1500°C for 24 hours under an argon atmosphere, and then cooled to room temperature.

[0051] In some embodiments, the etchant in step 1 can also be replaced with hydrofluoric acid solution, or a solution of NaF + nitric acid, NaF + sulfuric acid, LiF + hydrochloric acid, or Li + nitric acid; or other etching methods, such as accordion-shaped MXene material obtained by vapor phase etching.

[0052] Example 2

[0053] This embodiment provides another MXene nanoroll with the chemical formula: V2C0.5 N 0.5 T x The preparation methods include:

[0054] 1) Preparation of two-dimensional MXene materials from MAX phase materials

[0055] MAX phase material V2AlC 0.5 N 0.5 A mixture of concentrated hydrochloric acid (30 wt.%) and NaF, with a molar ratio of NaF to HCl of 1:1, was used for etching at 40°C for 48 hours. The resulting etched material was a two-dimensional MXene material, labeled as: V2(C x N 1-x )T x .

[0056] pass Figure 7 The XRD comparison of a shows that, compared with the MAX phase material, the (002) diffraction peak of the etched material shifts to a lower angle, and the characteristic peaks of other MAX phases disappear. This is because the A component (Al element) in the MAX phase material is selectively etched, and the interlayer spacing between its sheets increases. Figure 7 SEM images b and c show that the MAX phase material exhibits a typical layered bulk morphology. After etching, the etched material exhibits an accordion-like morphology of stacked sheets, with a significantly increased interlayer spacing, which is consistent with the previous XRD pattern results. The sheet diameter is approximately between 5 μm and 15 μm.

[0057] 2) Obtaining MXene nanorolls by rolling up two-dimensional MXene materials

[0058] Add 1g of the above etching material to 50ml of a 30wt.% TBAOH aqueous solution, stir magnetically for 10min, and then centrifuge and wash several times to obtain the purified sample.

[0059] TEM test results of the sample are as follows Figure 8 As shown in a, it can be seen that the sample also exhibits a significant one-dimensional morphology. The length of the MXene nanorolls is greater than 5 μm, which corresponds to the sheet diameter of the two-dimensional MXene material before winding. This indicates that the MXene nanorolls of the present invention are obtained by rolling up two-dimensional MXene sheets. Figure 8 b. Statistical analysis of the diameter of MXene nanotubes showed that the diameter of hollow rolls ranged from 20nm to 140nm, with the highest content of MXene nanotubes at a diameter of 60nm, accounting for more than 30%.

[0060] Figure 9 The TEM image of a shows that the ports of the MXene nanorolls are open. Figure 9b and c are HRTEM images, which show the hollow roll structure of MXene nanorolls, with approximately 3 to 6 MXene layers forming the tube walls. Figure 9 e-j shows the elemental distribution of MXene nanorolls. It can be seen that MXene nanorolls contain V, C, N, O, and F elements, and these elements are uniformly distributed. O and F are functional group elements on the surface of the MXene nanorolls, and their chemical formula is V2(C). x N 1-x )T x match.

[0061] The MAX phase material in this embodiment is prepared by high-temperature sintering. The steps include: obtaining the elemental or compound form of each element by high-temperature sintering according to the stoichiometric ratio of the elements in the chemical formula of the MAX phase material. In this embodiment, V2AlC 0.5 N 0.5 The preparation method includes: mixing vanadium powder (V), aluminum powder (Al), aluminum nitride (AlN), and carbon powder in a molar ratio of 2:0.5:0.5:0.5 and ball milling them, then placing them in a high-temperature sintering furnace and sintering them at a high temperature of 1500℃ for 24 hours under an argon atmosphere, and then cooling them to room temperature to obtain the final product.

[0062] Example 3

[0063] This embodiment provides an MXene nanoroll with the chemical formula Ti3CNT. x The preparation method includes the following steps:

[0064] 1) Preparation of two-dimensional MXene materials from MAX phase materials

[0065] The MAX phase material Ti3AlCN was etched at 40 °C for 48 h using a mixture of concentrated hydrochloric acid (30 wt.%) and LiF, wherein the molar ratio of LiF to HCl was 1:1, to obtain a two-dimensional MXene material, labeled Ti3CNT. x .

[0066] pass Figure 11 The XRD comparison of a shows that, compared with the MAX phase material, the (002) diffraction peak of the etched material shifts to a lower angle, and the characteristic peaks of other MAX phases disappear. Figure 11 SEM images b and c show that the MAX phase material exhibits a typical layered bulk morphology; the etched material exhibits an accordion-like morphology of stacked sheets, with a significantly increased interlayer spacing. The sheet diameter is approximately 3μm to 5μm.

[0067] 2) Obtaining MXene nanorolls by rolling up two-dimensional MXene materials

[0068] The above-mentioned etching material was added to a 10 wt.% TBAOH aqueous solution, and after magnetic stirring for 30 min, it was centrifuged and washed multiple times to obtain a purified sample. Figure 11 Images a through c show SEM images of samples stirred for 1 min, 10 min, and 30 min, respectively. They reveal that the two-dimensional MXene material gradually curls, eventually forming MXene nanorolls with a diameter of approximately 200 nm to 300 nm. This demonstrates that the duration of external force application influences the formation of MXene nanorolls. Extending the stirring time can also yield MXene nanorolls even at lower concentrations of positive ion-paired reagents.

[0069] Example 4

[0070] This embodiment provides another MXene nanoroll for use as a conductive component in conductive pastes, with the chemical formula: V2CT. x Preparation methods include:

[0071] 1) The MAX phase material V2AlC was etched at 90°C for 48 hours using concentrated hydrochloric acid-NaF etchant to obtain the two-dimensional MXene material V2CT. x ;

[0072] 2) The above two-dimensional MXene material was added to a 20 wt.% TBAOH intercalating agent solution, and after magnetic stirring for 5 min, it was centrifuged, washed and purified several times, and then dried to obtain MXene nanorolls;

[0073] Figure 12 a gives V2AlC and V2CT x XRD patterns; Figure 12 b provides a SEM image of V2AlC, which shows that it is a blocky material; Figure 12 c and d give the MXene nanoroll (V2CT) x The SEM and TEM images show that MXene nanorolls have a monodisperse one-dimensional hollow nanoroll morphology, with tube diameters ranging from 40 nm to 70 nm and lengths ranging from 2 to 5 μm. Figure 12 The image provided by e shows that the wall thickness of the MXene nanorolls is between 2 nm and 3 nm, indicating that they have ultrathin walls.

[0074] Using a similar method, the applicant has also prepared other types of MXene nanorolls with the same structural characteristics, including: Ti2CT x Ti3C2T x Nb2CT x TiNbCT x Cr2CT xTi3CNT x Ti2CT x Ti2C 0.5 N 0.5 T x Ti 0.5 V 0.5 C 0.5 N 0.5 T x V2CT x V2C 0.75 N 0.25 T x V2B 0.28 C 0.57 N 0.15 T x 、(V 0.8 Cr 0.2 )2B 0.33 C 0.67 T x 、(V 0.8 Cr 0.2 )2CT x 、(V 0.8 Fe 0.2 )2B 0.33 C 0.67 T x 、(V 0.8 Mn 0.2 )2B 0.33 C 0.67 T x 、(V 0.8 Fe 0.2 )2B 0.28 C 0.57 N 0.15 T x 、(V 0.8 Mn 0.2 )2B 0.28 C 0.57 N 0.15 T x Therefore, the preparation method of the present invention has a certain degree of universality for two-dimensional MXene materials. The types of MXene nanorolls prepared by the present invention are not limited to the examples given in the above embodiments. Other types of two-dimensional MXene materials can be wound to obtain the MXene nanoroll structure of the present invention by adjusting the experimental methods and conditions.

[0075] Since the MXene nanorolls of the present invention are formed by rolling up two-dimensional MXene materials, the length of the MXene nanorolls in the one-dimensional direction is related to the sheet diameter of the two-dimensional MXene materials. For two-dimensional MXene materials, the sheet diameter can be distributed between 0.1 μm and 100 μm. Therefore, we can reasonably predict that the length of the MXene nanorolls can also be within this range.

[0076] Examples 1-4 above detail the preparation method, morphology, and structural characteristics of the MXene nanorolls of the present invention. To illustrate the conductivity of the MXene nanorolls as a conductive agent, the etched material obtained in the above examples was centrifuged, washed, dispersed in a solvent using ultrasonication, and then freeze-dried to obtain two-dimensional MXene material powder. More specifically, the etched material was dispersed in water (2 mg / ml), ultrasonically treated for 12 hours, and then freeze-dried. The prepared MXene nanoroll dispersion was centrifuged, concentrated, and then freeze-dried to obtain MXene nanoroll powder. The conductivity of both powders was tested using the four-probe method. The test method was as follows: 50 mg of powder sample was added to the sample cell of a four-probe powder resistivity meter, leveled, and then the meter was turned on. The handle was rotated to move the upper probe of the resistivity meter downwards, and then the pressure was increased to 15 MPa. After the resistivity meter reading stabilized, the resistivity reading was read, and then the conductivity was obtained according to the conversion relationship of conductivity = 1 / resistivity. The results are shown in the table below.

[0077]

[0078] As can be seen, in the powder state, the MXene nanorolls of this invention have an order of magnitude higher conductivity than two-dimensional MXene materials. This is because, on the one hand, MXene nanorolls have a one-dimensional structure, resulting in better directional conductivity; on the other hand, MXene nanorolls are connected in a one-dimensional network manner, and their contact resistance is significantly lower than that of two-dimensional MXene materials, belonging to a sheet-like connection. The MXene nanorolls of this invention exhibit excellent conductivity as a conductive agent. Using the same method, carbon nanotube powder was tested, and its conductivity was less than 100 S cm⁻¹. -1 The conductivity of MXene nanotubes is significantly lower than that of the present invention. This can be explained by the fact that the conductivity of MXene materials is better than that of carbon nanotube materials. In addition, the monodisperse structure can reduce contact resistance and the linear one-dimensional structure has better electronic orientation conduction.

[0079] Example 5

[0080] This embodiment provides a lithium metal composite electrode material and its preparation method, including the following steps: melting an electrochemically active metal and then mixing or contacting it with MXene nanorolls. In this embodiment, lithium metal is used. The technical concept of this invention lies in, on the one hand, utilizing the inherent properties of MXene material, which contains metallic elements and has an affinity for liquid metals; on the other hand, the unique hollow roll structure of MXene nanorolls has a suitable diameter, enabling capillary adsorption to adsorb liquid metal into the hollow roll, forming a metal-coated structure. A more specific implementation includes the following steps:

[0081] 1) The MXene nanorolls (V2B) prepared in Example 1 above 0.28 C 0.57 N 0.15 T x Prepared to a mass concentration of 5 mg / ml -1 The dispersion was filtered under vacuum to form a thin film on the filter membrane. The film was then vacuum dried at 60°C for 24 hours to obtain an MXene nanofiber membrane. Figure 13 The image shows a SEM image of the MXene nanoroll film surface. It can be seen that the MXene nanorolls are a one-dimensional material and are in a monodisperse state.

[0082] 2) The MXene nanofilm is stamped into a disc with a diameter of 1.5 cm (e.g., Figure 13 b);

[0083] 3) In a glove box under an argon atmosphere, metallic lithium is heated to 250°C and melted into a liquid state;

[0084] 4) Place the disc obtained in step 2 into molten lithium metal, such as... Figure 14 As shown in Figure a, molten lithium metal appears as a bright silver liquid. The disc is initially black, but after contact with the liquid lithium metal, it is slowly soaked in. After about 3 minutes, the back surface of the black disc changes from black to silver. Figure 14 b) indicates that MXene nanorolls are lithiophilic and can successfully adsorb metallic lithium.

[0085] 5) After removing the disc and cooling it to room temperature, the resulting photograph of the disc is as follows. Figure 14 As shown in Figure c, the lithium metal composite electrode material of the present invention was obtained. By comparing the weights of the MXene nanorolls before and after adsorption, the mass ratio of MXene nanorolls to lithium metal was calculated to be 2:1.

[0086] A small portion of the obtained lithium metal composite electrode material wafer was cut and its surface and cross-section were subjected to scanning electron microscopy (SEM) testing. Figure 15 Images a through c show SEM images of the disc surface at different magnifications. It can be seen that the one-dimensional morphology of MXene nanorolls can still be clearly seen on the surface of the disc, and these one-dimensional MXene nanorolls are cross-linked and misaligned to form a cross-linked network, indicating that the adsorption of liquid lithium metal did not change the one-dimensional morphology of the MXene nanorolls; it can also be seen that the ports and interiors of the MXene nanorolls have obvious white color. Figure 16 Images a through c are SEM images of the cross-section of the disc at different magnifications. It is clear that the MXene nanoroll@lithium composite material retains the morphology of a one-dimensional material, with the hollow rolls filled with metallic lithium. Figure 17The HRTEM images provided show that lithium metal is absorbed inside the hollow rolls of MXene nanorolls, meaning that MXene nanorolls can encapsulate metals.

[0087] After removing the obtained lithium metal composite electrode material discs from the glove box, they were exposed to air for 24 hours. Two discs were then assembled into a battery as electrode plates. A discharge test was performed, and the results are as follows: Figure 18 As shown, after the lithium-absorbing discs were left in the air for a day, the assembled battery could still discharge normally, releasing approximately 7.6 mAh of charge. This indicates that MXene nanoroll materials, due to their unique nanoroll structure and abundant surface functional groups, have a strong adsorption capacity for lithium, and the nanoscale pores inside the tubes achieve the encapsulation of lithium metal, thus enabling them to exist stably in the air.

[0088] Therefore, this invention provides a modification technology path for metals that are difficult to exist stably in air (such as Na, K, Mg, Zn, etc.). Through the preparation method of the MXene nanoroll / metal material of this invention, the metal is encapsulated inside the hollow roll, thereby achieving the technical effect of stable existence in air or specific environments (such as in a liquid phase). Of course, the encapsulated metal is not limited to a single metal; it can also be an alloy of multiple metal elements.

[0089] To further understand the electrochemical performance of MXene nanorolls for lithium storage, MXene nanorolls and nanosheets, as well as pure lithium and Cu-Li batteries, were assembled, and cycle tests were conducted at different rates. Figure 19 a can be seen at 1mAcm -2 1mAh cm -2 At a rate of [missing information], MXene nanorolls can achieve a cycling performance of 2000 hours, while the overpotential remains around 120 mV. Figure 19 b gives the current densities (1-20 mA cm⁻¹) for different current densities. -2 The rate performance of the lithium metal composite electrode shows that MXene nanorolls have excellent rate performance, which also demonstrates from the perspective of electrochemical performance that the MXene nanoroll structure is excellent in terms of lithium storage capacity and performance.

[0090] The superior electrochemical performance of the MXene nanoroll-lithium metal composite electrode can be attributed to the fact that the MXene nanoroll structure facilitates the adsorption and encapsulation of lithium metal, enabling stable storage and release of lithium in air. The MXene nanorolls themselves possess lithium affinity, allowing for uniform dispersion within the lithium metal. Furthermore, the monodisperse one-dimensional morphology of the MXene nanorolls eliminates the stacking of two-dimensional sheets, thus improving the electrochemical performance of lithium storage. Additionally, the unique roll-like structure of the MXene nanorolls, with adjustable tube diameter, provides structural elasticity, acting as a buffer against changes in electrode volume within the metal electrode.

[0091] Example 6

[0092] This embodiment provides another method for combining MXene nanorolls with metal materials, specifically a composite material of MXene nanorolls and lithium metal. The steps include: mixing liquid metal with MXene nanoroll powder to form a slurry, then cooling and molding to obtain the composite material. The molded form can be either a block or a thin film. More specifically, the implementation steps include:

[0093] 1) In a glove box under an argon atmosphere, 50 mg of metallic lithium was heated to 250 °C and melted into a liquid state;

[0094] 2) Add 5 mg of MXene nanoroll powder to molten lithium metal, stir and mix to obtain a viscous slurry, coat the slurry onto copper foil, and cool to room temperature to obtain a composite electrode material of MXene nanoroll and nanoroll.

[0095] In other embodiments, the mass ratio of metal to MXene nanorolls is between (0.1 and 10):1.

[0096] The lithium metal in the above embodiments can also be replaced with other electrochemically active metals, such as at least one of sodium, potassium, calcium, magnesium or zinc, which can be used as electrode materials in these metal batteries and can produce the same technical effects as in this application.

[0097] The foregoing description of specific exemplary embodiments of the invention is for illustrative and explanatory purposes. These descriptions are not intended to limit the invention to the precise forms disclosed, and it will be apparent that many changes and variations can be made in accordance with the foregoing teachings. The exemplary embodiments were chosen and described in order to explain the specific principles of the invention and its practical application, thereby enabling those skilled in the art to implement and utilize various different exemplary embodiments of the invention, as well as various different choices and variations. The scope of the invention is intended to be defined by the claims and their equivalents.

Claims

1. An application of MXene nanorolls as metal encapsulation, characterized in that, The MXene nanoroll is an MXene material with a one-dimensional hollow roll structure. The two ends of the MXene nanoroll are open, and the MXene nanoroll has a linear one-dimensional morphology. The MXene nanoroll is formed by rolling up two-dimensional MXene material. The thickness of the tube wall of the MXene nanoroll is between 0.3 nm and 50 nm, and the tube diameter is between 10 nm and 200 nm.

2. A metal composite electrode material, characterized in that, The metal composite electrode material comprises an electrochemically active metal and MXene nanorolls. The MXene nanorolls are MXene materials with a one-dimensional hollow roll structure. The two ends of the MXene nanorolls are open, and the MXene nanorolls have a linear one-dimensional morphology. The MXene nanorolls are formed by rolling up two-dimensional MXene materials. The thickness of the tube wall of the MXene nanorolls is between 0.3 nm and 50 nm, and the tube diameter is between 10 nm and 200 nm.

3. The metal composite electrode material as described in claim 2, characterized in that, The hollow roll is filled with the electrochemically active metal. And / or, the mass ratio of the electrochemically active metal to the MXene nanoroll is between (0.1~10):

1.

4. The metal composite electrode material as described in claim 2 or 3, characterized in that, The hollow roll structure is formed by rolling up a single piece of the two-dimensional MXene material; And / or, the hollow roll structure is formed by rolling up a single layer of the two-dimensional MXene material.

5. The MXene nanoroll as described in any one of claims 2 or 3, characterized in that, The length of the MXene nanorolls ranges from 0.1 μm to 100 μm.

6. The metal composite electrode material as described in claim 2 or 3, characterized in that, The electrochemically active metal is selected from at least one of lithium, sodium, potassium, calcium, magnesium, or zinc. And / or, the chemical formula of the MXene nanorolls is represented as M n+1 X n T x M includes one, two, or more of the elements Ti, V, Nb, Cr, Ta, Hf, Mo, W, Fe, Mn, Y, or Sc; X is selected from one, two, or three of the elements carbon, nitrogen, or boron. n It can be 1, 2, 3, or 4; T x The functional group includes elements of the sixth and / or seventh main groups.

7. A method for preparing a metal composite electrode material as described in any one of claims 2 to 6, characterized in that the step... include: Transform electrochemically active metals into a liquid state; The liquid metal was mixed with MXene nanorolls.

8. The preparation method according to claim 7, characterized in that, It also includes the steps of: preparing MXene nanorolls into a thin film; and then contacting the thin film with a liquid metal.

9. A metal battery, characterized in that, The metal composite electrode material contained in any one of claims 2 to 6; or the metal composite electrode material obtained by the preparation method described in claim 7 or 8.

10. A means of transportation, characterized in that, It contains the metal battery as described in claim 9.

Citation Information

Patent Citations

  • Composite lithium metal negative electrode based on MXene nanoribbon and general synthesis method of composite lithium metal negative electrode

    CN111293276A

  • Ti3C2Tx MXene one-dimensional hollow nanotube as well as preparation method and application thereof

    CN113201807A