Skin-like synthetic mica and method of making
By adding iron oxide and manganese carbonate to the synthetic mica raw material to form a light red color, adding nano-titanium oxide to improve brightness, and using behenic acid surface treatment, the problem of synthetic mica being difficult to achieve a skin tone similar to that of Asians has been solved, achieving high transparency, weather resistance and shear resistance, simplifying the process and reducing costs.
Patent Information
- Application Number
- CN202310739946.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-21
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2043-06-21
AI Technical Summary
Existing synthetic mica is difficult to color-match to achieve a similar effect to Asian skin tones, and the process is complex, costly, and not resistant to shearing and high-energy ball milling.
By adding iron oxide and manganese carbonate to the synthetic mica raw material to form a light red color, and then adding nano-titanium oxide to improve the brightness, and using behenic acid for surface treatment, a skin-colored synthetic mica is prepared, avoiding multi-layer coating and simplifying the process.
The prepared synthetic mica has a color similar to Asian skin tones, high transparency and brightness, high shear resistance, weather resistance and no color bleeding, making it suitable for base makeup products. It does not require frequent color adjustment, and the use of natural raw materials improves safety and performance.
Smart Images

Figure CN116789145B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of synthetic mica technology, and in particular to a skin-colored synthetic mica and its preparation method. Background Technology
[0002] Base makeup products are an important category of cosmetics. They can change the skin tone and texture of the face, making the skin appear smoother, softer, and healthier.
[0003] In base makeup products such as primers, concealers, and foundations, it is necessary to have a certain level of coverage, a color close to the skin tone, and to enhance the skin's smoothness and radiance. Engineers often use pigments and fillers such as mica, titanium dioxide, iron oxide red, iron oxide yellow, and iron oxide black for color matching. This process is complex and often results in color floating and migration. To achieve a skin-toned effect with synthetic mica, researchers proposed using a "synthetic mica / Fe2O3" or "synthetic mica / TiO2 / Fe2O3" coating method. However, these two coating methods produce dark brick red and orange colors, failing to achieve the tender pink (pale yellowish-red) color similar to Asian skin. Furthermore, they are not resistant to shearing and high-energy ball milling, and the multi-layer coating method increases the number of processing steps and significantly increases costs. Summary of the Invention
[0004] In view of this, the purpose of the present invention is to provide a skin-colored synthetic mica and its preparation method, so that when the synthetic mica is applied in layers, it resembles the color of skin, has high transparency and good brightness, does not contain any coating layer, and the synthetic mica itself is resistant to high shear without losing its original color, is weather resistant, temperature resistant, does not bleed, and can be matched with other base makeup products.
[0005] The present invention solves the above-mentioned technical problems through the following technical means: A skin-colored synthetic mica comprises the following raw materials in parts by weight: 30-35 parts by weight of quartz sand, 20-25 parts by weight of magnesia, 10-15 parts by weight of alumina, 20-25 parts by weight of potassium fluorosilicate, 5-10 parts by weight of iron oxide, 3-6 parts by weight of potassium carbonate, 0.02-0.1 parts by weight of manganese carbonate, and 0.02-0.1 parts by weight of nano-titanium oxide.
[0006] By adding iron oxide to the raw materials of conventional synthetic mica, the synthetic mica turns red. Then, by adding manganese carbonate, the synthetic mica turns light red, thus producing a synthetic mica that resembles the skin tone of Asians. Furthermore, by adding nano-titanium oxide, the refractive index of the synthetic mica can be increased. This allows the synthetic mica to be used directly in foundation makeup. When applied directly, it blends and resembles the skin tone, with high transparency, excellent brightness, and high stability. It also does not bleed, eliminating the need for frequent color adjustments to achieve a skin-like effect, as was done with previous foundations.
[0007] Preferably, the quartz sand, magnesia, alumina, potassium fluorosilicate, iron oxide, potassium carbonate, manganese carbonate, and nano titanium dioxide have a purity greater than 98%.
[0008] By selecting raw materials with a purity greater than 98%, it is beneficial to improve the apparent color of the synthetic mica.
[0009] Preferably, the synthetic mica comprises the following raw materials in parts by weight: 32-34 parts by weight of quartz sand, 21-23 parts by weight of magnesia, 11-13 parts by weight of alumina, 21-23 parts by weight of potassium fluorosilicate, 6-8 parts by weight of iron oxide, 3-5 parts by weight of potassium carbonate, 0.05-0.07 parts by weight of manganese carbonate, and 0.03-0.05 parts by weight of nano-titanium oxide.
[0010] Preferably, the synthetic mica comprises the following raw materials in parts by weight: 33 parts by weight of quartz sand, 22 parts by weight of magnesia, 12 parts by weight of alumina, 22 parts by weight of potassium fluorosilicate, 7 parts by weight of iron oxide, 4 parts by weight of potassium carbonate, 0.06 parts by weight of manganese carbonate, and 0.04 parts by weight of nano-titanium oxide.
[0011] In this scheme, aluminum oxide is preferably aluminum oxide, and iron oxide is preferably ferric oxide.
[0012] By controlling the optimal ratio of each raw material, the resulting synthetic mica can exhibit the best skin tone appearance. In particular, the ratio of iron oxide and manganese carbonate can produce the best skin-like appearance. By controlling the ratio of nano titanium oxide, the brightness of the synthetic mica can be improved even with a small amount added.
[0013] This application also discloses a method for preparing the skin-colored synthetic mica as described above, comprising the following steps: S1. Ingredients: Prepare quartz sand, magnesia, alumina, potassium fluorosilicate, iron oxide, potassium carbonate, manganese carbonate and nano titanium oxide in proportion, then put them into a V-type mixer and mix them evenly to obtain a mixture for later use. S2. Calcination: The mixture is put into a high-temperature calcining furnace for melting and calcination. After calcination, the temperature is gradually reduced to room temperature to obtain mica single crystals. S3. Post-processing: The mica single crystals are crushed and sieved to obtain crushed mica crystals. The crushed mica crystals are then subjected to ball milling, surface treatment, filtration, washing, drying, and air jet pulverization to obtain hydrophobic skin-colored synthetic mica.
[0014] Synthetic mica is prepared directly from raw materials by high-temperature melting in steps S1 and S2. The preparation method is simple and conducive to large-scale industrial production. The prepared synthetic mica can present a skin-like color without the inclusion of a coating layer. It also has the effects of high shear resistance, weather resistance, temperature resistance and non-bleeding. This allows synthetic mica to be used directly and can be matched with any base makeup.
[0015] By post-processing skin-toned synthetic mica, it is possible to give it excellent hydrophobic properties, further enhancing the application experience.
[0016] It should be noted that the sheet diameter of synthetic mica will change during high shear processes, but the color of the synthetic mica in this application will not change. However, the sheet diameter and color of synthetic mica with multiple layers will change during high shear processes.
[0017] Preferably, in step S2, the gradient cooling condition is: cooling to room temperature at a rate of 5-15℃ / h.
[0018] Gradient cooling helps to improve the saturation and flake size uniformity of synthesized mica crystals.
[0019] Preferably, in step S3, before ball milling, the mica crystals are subjected to acid treatment. The specific conditions for the acid treatment are as follows: the crushed mica crystals are soaked in an 8% hydrochloric acid solution and then stirred at room temperature for 48 hours.
[0020] In this method, the broken mica crystals can be placed in a perforated frame or bag, the diameter of which is smaller than the diameter of the broken mica crystals, so that they will not fall out of the frame or bag during the soaking and stirring process, while still being in full contact with hydrochloric acid.
[0021] Treating broken mica crystals with hydrochloric acid can, on the one hand, dissolve impurity ions on the surface of the broken mica crystals, improving their purity; on the other hand, it can also improve the structure of Al... 3+ The dissolution of the layer leads to an increase in the negative charge of the layer, which is beneficial for surface treatment.
[0022] Preferably, the surface treatment in step S3 includes the following steps: S301: Stir and heat the ball-milled mica crystal slurry to 25-30℃, add basic aluminum acetate solution, and stir evenly at a constant temperature. S302: In step S301, slowly add acid solution to control the pH of the slurry to 5.0-6.0, and then stir at a constant temperature for 1-2 hours; S303: Heat the slurry treated in step S302 to 80-90℃, add the surface treatment solution, stir at a constant temperature for 0.5-1.5h, slowly add acid solution again, control the pH of the slurry to 5.0-6.0, stir at a constant temperature for 0.5-1.5h, and then cool down to 50-60℃ to obtain the slurry of surface-treated mica crystals.
[0023] In this scheme, the amount of basic aluminum acetate added is 2.0-8.0% of the crushed synthetic mica, with the optimal amount being 4.0%.
[0024] Preferably, in step S303, the surface treatment solution includes anhydrous ethanol, an organic surface treatment agent, and a strong alkali, and the pH of the surface treatment solution is controlled to be 9-10 when preparing the surface treatment solution.
[0025] A further preferred method is to use sodium hydroxide as the strong base. A transparent solution is obtained by dissolving the organic surface treatment agent in anhydrous ethanol and adjusting the pH of the solution to 9-10 with sodium hydroxide.
[0026] Preferably, the organic surface treatment agent is one or more combinations of lauric acid, myristic acid, palmitic acid, stearic acid, isostearic acid and behenic acid.
[0027] Further preferably, the organic surface treatment agent is behenic acid, which is a type of fatty acid and a natural compound. The newly peeled synthetic mica has potassium and aluminum ion vacancies on its surface, giving it a negative charge. Basic aluminum acetate hydrolyzes in an acidic solution at a pH of 5-6 to produce positively charged aluminum hydroxide colloidal particles, which adhere firmly to the surface of the synthetic mica due to electrostatic adsorption. At the same time, behenic acid undergoes chelation and esterification reactions with the hydroxyl groups in the aluminum hydroxide colloids, forming a more stable bridge.
[0028] Simultaneously, behenic acid is dissolved in anhydrous ethanol, and the pH of the surface treatment solution is adjusted to 9-10 with sodium hydroxide to make it a transparent solution. When this solution is added to the synthetic mica slurry, the ethanol in the behenic acid mixture undergoes an esterification reaction with the acetic acid produced by the hydrolysis of basic aluminum acetate, generating ethyl acetate. At 80-90℃, ethyl acetate exhibits some volatility, shifting the reaction to the right and promoting the entire coating reaction. This results in a more stable coating of behenic acid onto the synthetic mica, improving the hydrophobic properties of the synthetic mica and enhancing its application in base makeup. The reaction equation is shown below:
[0029] By using natural raw material behenic acid, compared with traditional silicone-based surface treatment agents, it can not only replace them in terms of performance, but also reduce the potential harm to the skin caused by synthetic compounds.
[0030] In this scheme, the amount of behenic acid added is 0.5-3.0% of the crushed synthetic mica, with the optimal amount being 2.0%.
[0031] By controlling the amount of behenic acid added, we can avoid adding too little, which would result in incomplete coating, and at the same time avoid adding too much, which would lead to waste.
[0032] The invention employing the above solution has the following beneficial effects: 1. By adding ferric oxide to the raw materials for preparing synthetic mica to form a red base color, and then adding a small amount of Mn, the resulting red color can be transformed into a pale yellowish-red similar to skin color, so that the prepared synthetic mica will have a skin color similar to that of Asians. At the same time, the addition of titanium oxide can increase the refractive index of synthetic mica, thereby increasing the brightness of synthetic mica. 2. This application prepares a skin-colored synthetic mica that, when applied in layers, resembles skin color, exhibits high transparency and brightness, and contains no encapsulation layer. It is also resistant to high shear, weather, and temperature, and does not bleed. Unlike traditional foundations, it does not require frequent color adjustments to achieve a skin-colored effect, thus solving the problems of tedious color adjustments and poor stability in foundations. 3. By using behenic acid to surface-treat skin-colored synthetic mica, it has unique skin-colored effects, excellent hydrophobic properties, a unique sense of clarity and smoothness when applied, and is derived from natural raw materials. In terms of performance, it can replace silicone-surface-treated powder products. 4. In the process of synthesizing mica by surface treatment of behenic acid, a mixed solvent of alcohol and water is used to avoid flammable and explosive solvents such as ketones, ethers and hydrocarbons, thereby improving the safety and environmental friendliness of actual production. Attached Figure Description
[0033] This application can be further illustrated by the non-limiting embodiments given in the accompanying drawings; Figure 1 This is one of the electron microscope scan images of the skin-colored synthetic mica in Embodiment 2 of this application; Figure 2 This is the second electron microscope scan image of the skin-colored synthetic mica in Embodiment 2 of this application; Figure 3 This is the XRD pattern of the skin-colored synthetic mica in Embodiment 2 of this application; Figure 4 This is the XRF image of the skin-colored synthetic mica in Embodiment 2 of this application; Figure 5This is one of the infrared spectra of behenic acid-coated mica prepared in the skin-colored synthetic mica preparation method of Example 2 of this application; Figure 6 This is the second infrared spectrum of behenic acid coating in the skin-colored synthetic mica preparation method of Example 2 of this application. Detailed Implementation
[0034] The following specific embodiments illustrate the implementation of the present invention. Those skilled in the art can understand the advantages and effects of the present invention from the content disclosed in this specification: Example 1: Preparation method of skin-colored synthetic mica In this embodiment, the quartz sand, magnesia, alumina, potassium fluorosilicate, and potassium carbonate were purchased commercially. The manganese carbonate and basic aluminum acetate were sourced from Sinopharm Chemical Reagent Co., Ltd., the iron oxide from NEELIKON Food Dyes & Chemicals Ltd., the titanium oxide from Jiangsu Nao New Materials Technology Co., Ltd., and the behenic acid (purity ≥85%) from Shanghai Maclean Biochemical Technology Co., Ltd.
[0035] The L, a, and b values of the powder were measured using an SC-100 fully automatic colorimeter (Beijing Kangguang Optical Instrument Co., Ltd.).
[0036] The structure and phase composition of the composite material were analyzed using a Fourier 460 infrared spectrometer (FT-IR, Nicolet, USA) and a D / Max 2500PC X-ray diffractometer (XRD, Cu target, λ = 0.154056 nm, scan rate 6 (°) / min, scan range 5°–80°, Rigaku, Japan).
[0037] Hydrophobicity test of synthetic mica powder: 1g of surface-treated powder and 100mL of water were added to a 250mL beaker, sealed and shaken vigorously for 1min, allowed to stand, and the solution state was observed. X: The powder dissolves uniformly in water, forming a cloudy white solution; X: The powder is immiscible with water and floats completely on the surface. (Part of the powder floats on the water surface, while part is dispersed in the water).
[0038] S1. Ingredients: Prepare 30 parts by weight of quartz sand, 20 parts by weight of magnesia, 10 parts by weight of alumina, 20 parts by weight of potassium fluorosilicate, 5 parts by weight of iron oxide, 3 parts by weight of potassium carbonate, 0.02 parts by weight of manganese carbonate and 0.02 parts by weight of nano titanium oxide, put them into a V-type mixer and mix evenly to obtain a mixture for later use. S2. Calcination: The mixture is put into a high-temperature calcining furnace for melting and calcination at 1450℃ for 30 minutes. After calcination, the mixture is gradually cooled to room temperature in the furnace at a rate of 5-15℃ / h to obtain mica single crystals. S3. Post-processing: The mica single crystals obtained in step S2 are crushed, passed through a 10-mesh sieve to remove large particle impurities, and the crushed mica crystals are obtained. S300: After loading the crushed synthetic mica obtained in step S3, soak it in an 8% dilute hydrochloric acid solution and stir at room temperature for 48 hours. Then, put it into a vertical stirred ball mill, control a certain solid-liquid ratio (control the water content to be 40-50%), and stop grinding the product when the particle size D50 is 5-8μm. Add water to settle and classify, and further remove the unground synthetic mica to obtain ultrafine synthetic mica powder. S301: The synthesized mica after ball milling in step S301 is redispersed with deionized water at a ratio of 1:10-20 to form a slurry. The mixture is stirred and heated to 25°C. 0.5 mol / L basic aluminum acetate solution is added (the amount of basic aluminum acetate added is 2% of the amount of synthesized mica), and the mixture is stirred evenly at a constant temperature of 25°C. S302: In step S301, slowly add a 2% dilute hydrochloric acid solution to control the pH of the slurry to 5.0-6.0, and then stir at a constant temperature for 1-2 hours. S303: The slurry treated in step S302 is heated to 80°C, and a mixed solution of anhydrous ethanol, sodium hydroxide and behenic acid is added. The pH of the mixed solution is 9-10, and the amount of behenic acid added is 0.5% of the synthetic mica, so that the solubility of behenic acid in the slurry is 0.25 g / ml. The mixture is stirred at 80°C for 1.5 h, and then a 2% dilute hydrochloric acid solution is slowly added dropwise to control the pH of the slurry to 5.0-6.0. The mixture is stirred at 80°C for another 1.5 h, and then cooled to 50-60°C to obtain a slurry of surface-treated mica crystals. S304: Filter the mica crystal slurry after step S303, wash it with deionized water 3-5 times, dry it at 120℃, and then air-jet pulverize it to obtain hydrophobic skin-colored synthetic mica.
[0039] Example 2, Method 2 for preparing skin-colored synthetic mica In this embodiment, the raw materials and testing methods used are the same as in Example 1.
[0040] S1. Ingredients: Prepare 33 parts by weight of quartz sand, 22 parts by weight of magnesia, 12 parts by weight of alumina, 22 parts by weight of potassium fluorosilicate, 7 parts by weight of iron oxide, 4 parts by weight of potassium carbonate, 0.06 parts by weight of manganese carbonate and 0.04 parts by weight of nano titanium oxide, put them into a V-type mixer and mix evenly to obtain a mixture for later use. S2. Calcination: The mixture is put into a high-temperature calcining furnace for melting and calcination at 1450℃ for 30 minutes. After calcination, the mixture is gradually cooled to room temperature in the furnace at a rate of 5-15℃ / h to obtain mica single crystals. S3. Post-processing: The mica single crystals obtained in step S2 are crushed, passed through a 10-mesh sieve to remove large particle impurities, and the crushed mica crystals are obtained. S300: After loading the crushed synthetic mica obtained in step S3, soak it in an 8% dilute hydrochloric acid solution and stir at room temperature for 48 hours. Then, put it into a vertical stirred ball mill, control a certain solid-liquid ratio (control the water content to be 40-50%), and stop grinding the product when the particle size D50 is 5-8μm. Add water to settle and classify, and further remove the unground synthetic mica to obtain ultrafine synthetic mica powder. S301: The synthesized mica after ball milling in step S301 is redispersed with deionized water at a ratio of 1:10-20 to form a slurry. The mixture is stirred and heated to 25°C. 0.5 mol / L basic aluminum acetate solution is added (wherein, the amount of basic aluminum acetate added is 4.0% of the synthetic mica), and the mixture is stirred evenly at a constant temperature of 25°C. S302: In step S301, slowly add a 2% dilute hydrochloric acid solution to control the pH of the slurry to 5.0-6.0, and then stir at a constant temperature for 1-2 hours. S303: The slurry treated in step S302 is heated to 85°C, and a mixed solution of anhydrous ethanol, sodium hydroxide and behenic acid is added. The pH of the mixed solution is 9-10, and the amount of behenic acid added is 2.0% of the synthetic mica, so that the solubility of behenic acid in the slurry is 0.25 g / ml. The mixture is stirred at 85°C for 1 hour, and then a 2% dilute hydrochloric acid solution is slowly added dropwise to control the pH of the slurry to 5.0-6.0. The mixture is stirred at 85°C for another hour, and then cooled to 50-60°C to obtain a slurry of surface-treated mica crystals. S304: Filter the mica crystal slurry after step S303, wash it with deionized water 3-5 times, dry it at 120℃, and then air-jet pulverize it to obtain hydrophobic skin-colored synthetic mica.
[0041] Example 3, Preparation method of skin-colored synthetic mica (Part 3) In this embodiment, the raw materials and testing methods used are the same as in Example 1.
[0042] S1. Ingredients: Prepare 35 parts by weight of quartz sand, 25 parts by weight of magnesia, 15 parts by weight of alumina, 25 parts by weight of potassium fluorosilicate, 10 parts by weight of iron oxide, 6 parts by weight of potassium carbonate, 0.1 parts by weight of manganese carbonate and 0.1 parts by weight of nano titanium oxide, and put them into a V-type mixer to mix evenly to obtain a mixture for later use. S2. Calcination: The mixture is put into a high-temperature calcining furnace for melting and calcination at 1450℃ for 30 minutes. After calcination, the mixture is gradually cooled to room temperature in the furnace at a rate of 5-15℃ / h to obtain mica single crystals. S3. Post-processing: The mica single crystals obtained in step S2 are crushed, passed through a 10-mesh sieve to remove large particle impurities, and the crushed mica crystals are obtained. S300: After loading the crushed synthetic mica obtained in step S3, soak it in an 8% dilute hydrochloric acid solution and stir at room temperature for 48 hours. Then, put it into a vertical stirred ball mill, control a certain solid-liquid ratio (control the water content to be 40-50%), and stop grinding the product when the particle size D50 is 5-8μm. Add water to settle and classify, and further remove the unground synthetic mica to obtain ultrafine synthetic mica powder. S301: The synthesized mica after ball milling in step S301 is redispersed with deionized water at a ratio of 1:10-20 to form a slurry. The mixture is stirred and heated to 30°C. 0.5 mol / L basic aluminum acetate solution is added (the amount of basic aluminum acetate added is 8% of the amount of synthesized mica), and the mixture is stirred evenly at a constant temperature of 30°C. S302: In step S301, slowly add a 2% dilute hydrochloric acid solution to control the pH of the slurry to 5.0-6.0, and then stir at a constant temperature for 1-2 hours. S303: The slurry treated in step S302 is heated to 90°C, and a mixed solution of anhydrous ethanol, sodium hydroxide and behenic acid is added. The pH of the mixed solution is 9-10, and the amount of behenic acid added is 3.0% of the synthetic mica, so that the solubility of behenic acid in the slurry is 0.25 g / ml. The mixture is stirred at 90°C for 0.5 h, and then a 2% dilute hydrochloric acid solution is slowly added dropwise to control the pH of the slurry to 5.0-6.0. The mixture is stirred at 90°C for another 0.5 h, and then cooled to 50-60°C to obtain a slurry of surface-treated mica crystals. S304: Filter the mica crystal slurry after step S303, wash it with deionized water 3-5 times, dry it at 120℃, and then air-jet pulverize it to obtain hydrophobic skin-colored synthetic mica.
[0043] Example 4 (Comparative Example 1), Method 4 for preparing skin-colored synthetic mica In this embodiment, the raw materials and testing methods used are the same as in Example 1. Behenic acid is used directly for surface treatment, but basic aluminum acetate is not used in the surface treatment process.
[0044] S1. Ingredients: Prepare 33 parts by weight of quartz sand, 22 parts by weight of magnesia, 12 parts by weight of alumina, 22 parts by weight of potassium fluorosilicate, 7 parts by weight of iron oxide, 4 parts by weight of potassium carbonate, 0.06 parts by weight of manganese carbonate and 0.04 parts by weight of nano titanium oxide, put them into a V-type mixer and mix evenly to obtain a mixture for later use. S2. Calcination: The mixture is put into a high-temperature calcining furnace for melting and calcination at 1450℃ for 30 minutes. After calcination, the mixture is gradually cooled to room temperature in the furnace at a rate of 5-15℃ / h to obtain mica single crystals. S3. Post-processing: The mica single crystals obtained in step S2 are crushed, passed through a 10-mesh sieve to remove large particle impurities, and the crushed mica crystals are obtained. S300: After loading the crushed synthetic mica obtained in step S3, soak it in an 8% dilute hydrochloric acid solution and stir at room temperature for 48 hours. Then, put it into a vertical stirred ball mill, control a certain solid-liquid ratio (control the water content to be 40-50%), and stop grinding the product when the particle size D50 is 5-8μm. Add water to settle and classify, and further remove the unground synthetic mica to obtain ultrafine synthetic mica powder. S301: The synthesized mica after ball milling in step S300 is redispersed with deionized water at a ratio of 1:10-20 to form a slurry. A mixed solution of anhydrous ethanol, sodium hydroxide and behenic acid is added. The pH of the mixed solution is 9-10, and the amount of behenic acid added is 2.0% of the synthetic mica, so that the solubility of behenic acid in the slurry is 0.25 g / ml. Stir at room temperature for 1 hour, and then slowly add 2% dilute hydrochloric acid solution to control the pH of the slurry to 5.0-6.0. After stirring for another hour, a slurry of surface-treated mica crystals is obtained. S302: Filter the mica crystal slurry obtained from step S301, wash it with deionized water 3-5 times, dry it at 120℃, and then air-jet pulverize it to obtain hydrophobic skin-colored synthetic mica.
[0045] Example 5 (Comparative Example 2), Method for preparing skin-colored synthetic mica In this embodiment, the raw materials and testing methods used are the same as in Example 1, but basic aluminum acetate and behenic acid are not used to treat the surface of the prepared synthetic mica.
[0046] S1. Ingredients: Prepare 33 parts by weight of quartz sand, 22 parts by weight of magnesia, 12 parts by weight of alumina, 22 parts by weight of potassium fluorosilicate, 7 parts by weight of iron oxide, 4 parts by weight of potassium carbonate, 0.06 parts by weight of manganese carbonate and 0.04 parts by weight of nano titanium oxide, put them into a V-type mixer and mix evenly to obtain a mixture for later use. S2. Calcination: The mixture is put into a high-temperature calcining furnace for melting and calcination at 1450℃ for 30 minutes. After calcination, the mixture is gradually cooled to room temperature in the furnace at a rate of 5-15℃ / h to obtain mica single crystals. S3. Post-processing: The mica single crystals obtained in step S2 are crushed, passed through a 10-mesh sieve to remove large particle impurities, and the crushed mica crystals are obtained. S300: After loading the crushed synthetic mica obtained in step S3, soak it in an 8% dilute hydrochloric acid solution and stir at room temperature for 48 hours. Then, put it into a vertical stirred ball mill, control a certain solid-liquid ratio (control the water content to be 40-50%), and stop grinding the product when the particle size D50 is 5-8μm. Add water to settle and classify, and further remove the unground synthetic mica to obtain ultrafine synthetic mica powder.
[0047] Example 6 (Comparative Example 3), Method for preparing skin-colored synthetic mica In this embodiment, the raw materials and testing methods used are the same as in Example 1, but ferric oxide and manganese carbonate are not added.
[0048] S1. Ingredients: Prepare 33 parts by weight of quartz sand, 22 parts by weight of magnesia, 12 parts by weight of alumina, 22 parts by weight of potassium fluorosilicate, 4 parts by weight of potassium carbonate and 0.04 parts by weight of nano titanium dioxide, put them into a V-type mixer and mix evenly to obtain a mixture for later use. S2. Calcination: The mixture is put into a high-temperature calcining furnace for melting and calcination at 1450℃ for 30 minutes. After calcination, the mixture is gradually cooled to room temperature in the furnace at a rate of 5-15℃ / h to obtain mica single crystals. S3. Post-processing: The mica single crystals obtained in step S2 are crushed, passed through a 10-mesh sieve to remove large particle impurities, and the crushed mica crystals are obtained. S300: After loading the crushed synthetic mica obtained in step S3, soak it in an 8% dilute hydrochloric acid solution and stir at room temperature for 48 hours. Then, put it into a vertical stirred ball mill, control a certain solid-liquid ratio (control the water content to be 40-50%), and stop grinding the product when the particle size D50 is 5-8μm. Add water to settle and classify, and further remove the unground synthetic mica to obtain ultrafine synthetic mica powder.
[0049] Example 7 (Comparative Example 4), Method 7 for preparing skin-colored synthetic mica In this embodiment, the raw materials and testing methods used are the same as in Example 1, but manganese carbonate is not added.
[0050] S1. Ingredients: Prepare 33 parts by weight of quartz sand, 22 parts by weight of magnesia, 12 parts by weight of alumina, 22 parts by weight of potassium fluorosilicate, 7 parts by weight of iron oxide, 4 parts by weight of potassium carbonate and 0.04 parts by weight of nano titanium oxide, put them into a V-type mixer and mix evenly to obtain a mixture for later use. S2. Calcination: The mixture is put into a high-temperature calcining furnace for melting and calcination at 1450℃ for 30 minutes. After calcination, the mixture is gradually cooled to room temperature in the furnace at a rate of 5-15℃ / h to obtain mica single crystals. S3. Post-processing: The mica single crystals obtained in step S2 are crushed, passed through a 10-mesh sieve to remove large particle impurities, and the crushed mica crystals are obtained. S300: After loading the crushed synthetic mica obtained in step S3, soak it in an 8% dilute hydrochloric acid solution and stir at room temperature for 48 hours. Then, put it into a vertical stirred ball mill, control a certain solid-liquid ratio (control the water content to be 40-50%), and stop grinding the product when the particle size D50 is 5-8μm. Add water to settle and classify, and further remove the unground synthetic mica to obtain ultrafine synthetic mica powder.
[0051] Example 8 (Comparative Example 5): Method for preparing skin-colored synthetic mica In this embodiment, the raw materials and testing methods used are the same as in Example 1, but ferric oxide is not added.
[0052] S1. Ingredients: Prepare 33 parts by weight of quartz sand, 22 parts by weight of magnesia, 12 parts by weight of alumina, 22 parts by weight of potassium fluorosilicate, 4 parts by weight of potassium carbonate, 0.06 parts by weight of manganese carbonate and 0.04 parts by weight of nano titanium dioxide, and put them into a V-type mixer to mix evenly to obtain a mixture for later use. S2. Calcination: The mixture is put into a high-temperature calcining furnace for melting and calcination at 1450℃ for 30 minutes. After calcination, the mixture is gradually cooled to room temperature in the furnace at a rate of 5-15℃ / h to obtain mica single crystals. S3. Post-processing: The mica single crystals obtained in step S2 are crushed, passed through a 10-mesh sieve to remove large particle impurities, and the crushed mica crystals are obtained. S300: After loading the crushed synthetic mica obtained in step S3, soak it in an 8% dilute hydrochloric acid solution and stir at room temperature for 48 hours. Then, put it into a vertical stirred ball mill, control a certain solid-liquid ratio (control the water content to be 40-50%), and stop grinding the product when the particle size D50 is 5-8μm. Add water to settle and classify, and further remove the unground synthetic mica to obtain ultrafine synthetic mica powder.
[0053] The skin-colored synthetic mica prepared in Examples 1-8 was subjected to performance tests, including its appearance, L, a, b values, and hydrophobicity, as shown in the table below:
[0054] The data in the table shows that the skin-colored synthetic mica prepared in Examples 1-3 are all yellowish-red, but the shades of yellowish-red vary. Similar to skin color, the color depth varies depending on the amount of ferric oxide, manganese oxide, and titanium oxide added. Among them, the mica in Example 2 has the best overall performance in terms of appearance color and brightness, and its hydrophobicity also meets the requirements due to the coating with behenic acid. In Example 3, although the hydrophobicity also meets the requirements, the amount of behenic acid added is too large, which increases the cost.
[0055] The synthetic mica prepared in Example 2 was subjected to electron microscopy scanning. The electron microscopy scanning was performed without behenic acid coating. Figure 1-2 As shown, the synthetic mica prepared in this application has high transparency and good brightness, and its composition does not contain any coating layer. Its accumulated color can present a skin-like color.
[0056] The synthetic mica prepared in Example 2 was subjected to component analysis. The component analysis was performed without behenic acid coating. Figure 3-4 As shown, the synthetic mica prepared in this application contains ferric oxide, manganese oxide and titanium oxide crystals, which form eutectic crystals with other raw materials of synthetic mica, rather than being directly doped, thereby enabling the synthetic mica to form a skin-colored appearance.
[0057] By coating the synthetic mica prepared in Example 2 with behenic acid and using basic aluminum acetate as a bridging agent, the behenic acid can be more stably coated onto the synthetic mica. Infrared spectroscopy analysis of the behenic acid-coated synthetic mica was performed, such as... Figure 5-6 As shown, the infrared FT-IR spectrum and local peak segments (3000-1400 cm⁻¹) are analyzed. -1 From this, we can deduce that the coordinates are 2917.8 and 2850.3 cm. -1 This is the absorption peak of the nonpolar aliphatic carbon chain in behenic acid; 1635.3 cm⁻¹ -1 The absorption peaks are for the carbonyl group on -COOH and show a significant increase in intensity, at 1467.5 and 1589.0 cm⁻¹. -1 The absorption peaks represent the symmetric and antisymmetric stretching vibrations of the carbon-oxygen double bond formed by the coupling of C=O and CO in aluminum behenate, respectively. This indicates that the synthesis of mica, aluminum hydroxide, and behenic acid yielded an effective composite.
[0058] in, Figure 5-6 In the text, 'a' indicates that the skin-colored synthetic mica was directly subjected to infrared spectroscopy analysis; 'b' indicates that the mica was coated with behenic acid before infrared spectroscopy analysis.
[0059] The data from Examples 2 and 4 show that after preparing synthetic mica, directly coating it with behenic acid results in very little difference in appearance and brightness, but a significant difference in hydrophobicity. This indicates that using basic aluminum acetate helps behenic acid to be coated more stably on the synthetic mica.
[0060] The data from Examples 2 and 5 show that without coating the synthetic mica with basic aluminum acetate and behenic acid, the synthetic mica lacks hydrophobicity and will dissolve completely in water, resulting in poor performance when used as a base makeup.
[0061] The data from Examples 2 and 6 show that, in the preparation process of synthetic mica, without the addition of ferric oxide and manganese oxide to other conventional raw materials, white synthetic mica will be formed, and skin-colored synthetic mica will not be formed.
[0062] The data from Examples 2 and 7 show that, in the preparation of synthetic mica, adding only ferric oxide to other conventional raw materials will only form dark red synthetic mica, not skin-colored synthetic mica. That is, adding ferric oxide and manganese oxide can synergistically adjust the color of synthetic mica, thereby forming skin-colored synthetic mica.
[0063] The data from Examples 2 and 8 show that, in the preparation of synthetic mica, if only manganese oxide is added to other conventional raw materials, the resulting synthetic mica will not exhibit a skin-colored pale yellow-red hue. That is, only by adding both ferric oxide and manganese oxide to the conventional raw materials for synthetic mica can a skin-colored synthetic mica be formed.
[0064] In summary, by adding ferric oxide and manganese oxide to the conventional raw materials of synthetic mica, skin-toned synthetic mica can be formed. Adding titanium oxide can increase the brightness of the skin-toned synthetic mica. Furthermore, by using basic aluminum acetate and behenic acid to coat the skin-toned synthetic mica, the behenic acid can be more firmly coated onto the skin-toned synthetic mica, giving it better hydrophobicity and skin-adhering feel during use, and thus a wider range of applications.
[0065] The foregoing provides a detailed description of a skin-colored synthetic mica and its preparation method provided by the present invention. The specific embodiments are provided only to aid in understanding the method and core ideas of the present invention. It should be noted that those skilled in the art can make various improvements and modifications to the present invention without departing from its principles, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.
[0066] It should be noted that: for experimental steps or conditions not specified in the examples, the procedures and conditions described in conventional experimental procedures in the literature of this art can be followed. Reagents or instruments whose manufacturers are not specified are all commercially available conventional reagent products.
[0067] The above examples are provided to better understand the present invention and are not limited to the preferred embodiments described. They do not constitute a limitation on the content and scope of protection of the present invention. Any product that is the same as or similar to the present invention, derived by anyone under the guidance of the present invention or by combining the features of the present invention with other prior art, falls within the scope of protection of the present invention.
Claims
1. A skin-colored synthetic mica, characterized in that, The raw materials include the following parts by weight: 30-35 parts by weight of quartz sand, 20-25 parts by weight of magnesia, 10-15 parts by weight of alumina, 20-25 parts by weight of potassium fluorosilicate, 5-10 parts by weight of iron oxide, 3-6 parts by weight of potassium carbonate, 0.02-0.1 parts by weight of manganese carbonate, and 0.02-0.1 parts by weight of nano-titanium oxide. The synthetic mica is prepared by high-temperature melting and has a light yellow-red color.
2. The skin-colored synthetic mica according to claim 1, characterized in that, The purity of the quartz sand, magnesia, alumina, potassium fluorosilicate, iron oxide, potassium carbonate, manganese carbonate, and nano titanium dioxide is greater than 98%.
3. The skin-colored synthetic mica according to claim 1, characterized in that, The synthetic mica comprises the following raw materials in parts by weight: 32-34 parts by weight of quartz sand, 21-23 parts by weight of magnesia, 11-13 parts by weight of alumina, 21-23 parts by weight of potassium fluorosilicate, 6-8 parts by weight of iron oxide, 3-5 parts by weight of potassium carbonate, 0.05-0.07 parts by weight of manganese carbonate, and 0.03-0.05 parts by weight of nano-titanium oxide.
4. A skin-toned synthetic mica according to claim 1 or 3, characterized in that, The synthetic mica comprises the following raw materials in parts by weight: 33 parts by weight of quartz sand, 22 parts by weight of magnesia, 12 parts by weight of alumina, 22 parts by weight of potassium fluorosilicate, 7 parts by weight of iron oxide, 4 parts by weight of potassium carbonate, 0.06 parts by weight of manganese carbonate, and 0.04 parts by weight of nano titanium dioxide.
5. A method for preparing skin-colored synthetic mica as described in any one of claims 1-3, characterized in that, Includes the following steps: S1. Ingredients: Prepare quartz sand, magnesia, alumina, potassium fluorosilicate, iron oxide, potassium carbonate, manganese carbonate and nano titanium oxide in proportion, then put them into a V-type mixer and mix them evenly to obtain a mixture for later use. S2. Calcination: The mixture is put into a high-temperature calcining furnace for melting and calcination. After calcination, the temperature is gradually reduced to room temperature to obtain mica single crystals. S3. Post-processing: The mica single crystals are crushed and sieved to obtain crushed mica crystals. The crushed mica crystals are then subjected to ball milling, surface treatment, filtration, washing, drying, and air jet pulverization to obtain hydrophobic skin-colored synthetic mica.
6. The method for preparing a skin-colored synthetic mica according to claim 5, characterized in that, In step S2, the gradient cooling condition is: cooling to room temperature at a rate of 5-15℃ / h.
7. The method for preparing a skin-colored synthetic mica according to claim 5, characterized in that, In step S3, before ball milling, the mica crystals are treated with acid. The specific conditions for the acid treatment are as follows: the crushed mica crystals are soaked in an 8% hydrochloric acid solution and then stirred at room temperature for 48 hours.
8. The method for preparing a skin-colored synthetic mica according to claim 5, characterized in that, In step S3, the specific surface treatment operations include the following steps: S301: Stir and heat the ball-milled mica crystal slurry to 25-30℃, add basic aluminum acetate solution, and stir evenly at a constant temperature. S302: In step S301, slowly add acid solution to control the pH of the slurry to 5.0-6.0, and then stir at a constant temperature for 1-2 hours; S303: Heat the slurry treated in step S302 to 80-90℃, add the surface treatment solution, stir at a constant temperature for 0.5-1.5h, slowly add acid solution again, control the pH of the slurry to 5.0-6.0, stir at a constant temperature for 0.5-1.5h, and then cool down to 50-60℃ to obtain the slurry of surface-treated mica crystals.
9. The method for preparing a skin-colored synthetic mica according to claim 8, characterized in that, In step S303, the surface treatment solution includes anhydrous ethanol, an organic surface treatment agent, and a strong alkali. When preparing the surface treatment solution, the pH of the surface treatment solution is controlled to be 9-10.
10. The method for preparing a skin-colored synthetic mica according to claim 9, characterized in that, The organic surface treatment agent is one or more combinations of lauric acid, myristic acid, palmitic acid, stearic acid, isostearic acid and behenic acid.
Citation Information
Patent Citations
Artificial synthetic mica powder based on iron substitution coloring and preparation method thereof
CN115304065A
Red synthetic mica, its production and ultraviolet screening agent containing the same mica
JP1994009210A
Mica powder, method for producing the same and cosmetic containing the same
JP2001288040A
Process for rendering nacreous pigments hydrophobic
US4490179A