Boron phosphide fiber and its preparation method and application

By preparing boron phosphide fibers through vacuum high-temperature reaction, the problems of high melting point and high decomposition pressure in existing technologies are solved, realizing efficient and safe preparation of boron phosphide fibers, which are suitable for semiconductors and optoelectronic devices.

CN116791236BActive Publication Date: 2026-11-20SUZHOU INST OF NANO TECH & NANO BIONICS CHINESE ACEDEMY OF SCI
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310724856.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-19
Publication Date
2026-11-20
Estimated Expiration
2043-06-19

AI Technical Summary

Technical Problem

Existing technologies for preparing boron phosphide nanostructures suffer from high melting points and high decomposition pressures, and often use flammable and toxic fluxes, making it difficult to control impurities and resulting in long reaction times, thus hindering the application of high-quality boron phosphide materials.

Method used

Boron phosphide fibers were prepared by reacting boron source with black phosphorus at high temperature in a vacuum-sealed environment, avoiding the use of metal fluxes and catalysts, and by controlling the heating and cooling rates and reaction time.

Benefits of technology

This process reduces byproducts, simplifies the process, shortens the reaction time, and improves preparation efficiency. The resulting boron phosphide fibers have high purity and are suitable for semiconductor electronic and optoelectronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116791236B_ABST
    Figure CN116791236B_ABST
Patent Text Reader

Abstract

The application discloses boron phosphide fibers and a preparation method and application thereof. The preparation method comprises the following steps: reacting a boron source and black phosphorus at high temperature in a vacuum sealed environment to obtain boron phosphide fibers. The preparation method of the boron phosphide fibers provided by the application does not use metal fluxing agents, catalysts and the like, only uses a phosphorus source and a boron source, the by-products are greatly reduced, and the reaction time is shortened to about 3 days. Meanwhile, the preparation method provided by the application has the advantages of safe raw materials, simple process and short reaction period.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of materials preparation technology, specifically relating to a boron phosphide fiber, its preparation method, and its application. Background Technology

[0002] With the rapid development of global science and technology, the world has entered the information age. As the lifeblood of the information field, micro-nano electronics and optoelectronics have become the focus of technological development. Breaking the predictions of Moore's Law requires, on the one hand, continuous optimization of device structures to reduce short-channel effects; on the other hand, the search for new materials to replace traditional silicon-based semiconductors. Therefore, researching new semiconductor materials with high mobility, high thermal conductivity, wide bandgap, and the ability to operate in harsh environments is urgently needed.

[0003] Boron phosphide (BP) is one of the earliest discovered semiconductor materials in the III-V group. It possesses excellent physicochemical properties; its small lattice constant, strong covalent bonds, and high thermal conductivity contribute to its strong chemical and thermodynamic stability. BP's very high hardness, ultra-high thermal conductivity, and excellent stability and heat dissipation capabilities make it an ideal semiconductor material for operation in extreme environments and under high power conditions. Furthermore, BP itself exists in both n-type and p-type semiconductor forms. Theoretical calculations show that BP can achieve its own pn-type transition, providing new convenience and possibilities for the construction of pn-junction devices. However, due to its high melting point (3000℃) and decomposition pressure (10⁵ atm at 2500℃), the controllable synthesis of BP nanostructures remains a significant challenge. In addition, the preparation of high-quality BP is difficult, often involving flammable and toxic hazardous substances, and the preparation process is extremely prone to unintentionally introducing impurities. These factors are also important reasons hindering the research on the microscopic properties of BP materials and their application in devices. For example, patent CN110284195A discloses a boron phosphide single crystal, its preparation method, and its uses. In the preparation of the boron phosphide single crystal, Ni is used as a flux. The subsequent products need to be acid-washed to remove byproducts such as white phosphorus and NixP. Furthermore, the reaction time is relatively long, requiring approximately 7 days. Patent CN111333079A discloses a boron phosphide fiber material and its preparation method. After mixing boron and phosphorus source materials, the second powder is reacted at high temperature under vacuum conditions with a metal flux. The mixture is then sequentially acid-washed, water-washed, and dried to obtain the boron phosphide fiber material. Meanwhile, literature (ACS Nano, 2022, 16, 4004-4013) also... 10Boron phosphide (B) reacts with Ni and red phosphorus. The resulting product is washed with an acidic mixture of hydrochloric acid and nitric acid (regional aqueous solution) to remove white phosphorus and nickel phosphide byproducts. Then, it is treated with concentrated HF solution to remove silica. Finally, the product is washed and dried with acetone and ethanol. It can be seen that patent CN111333079A and other literature both use flux in the preparation of boron phosphide, and the subsequent product requires acid washing to remove byproducts such as white phosphorus and nickel phosphide. Furthermore, the reaction time is relatively long, requiring approximately 7 days. Summary of the Invention

[0004] The main objective of this invention is to provide boron phosphide fiber, its preparation method, and its application, so as to overcome the shortcomings of the prior art.

[0005] To achieve the aforementioned objectives, the technical solution adopted by this invention includes:

[0006] This invention provides a method for preparing boron phosphide fibers, which includes: reacting a boron source with black phosphorus at high temperature in a vacuum-sealed environment to obtain boron phosphide fibers.

[0007] The present invention also provides boron phosphide fibers prepared by the aforementioned preparation method.

[0008] The present invention also provides the use of the aforementioned boron phosphide fibers in the preparation of semiconductor electronic devices or semiconductor optoelectronic devices.

[0009] Compared with the prior art, the beneficial effects of the present invention are at least as follows:

[0010] (1) The method for preparing boron phosphide fiber provided by the present invention does not use metal flux, catalyst, etc., but only phosphorus source and boron source, which greatly reduces by-products and shortens the reaction time to about 3 days.

[0011] (2) The present invention utilizes boron and phosphorus sources to grow boron phosphide fibers under high temperature conditions. The preparation method provided by the present invention has safe raw materials, simple process and short reaction cycle. Attached Figure Description

[0012] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0013] Figure 1 This is a SEM image of the boron phosphide fibers prepared in Example 1 of the present invention;

[0014] Figure 2This is the Raman spectrum of the boron phosphide fiber prepared in Example 1 of this invention;

[0015] Figures 3a-3c This is a high-resolution TEM mapping image of the boron phosphide fibers prepared in Example 1 of this invention;

[0016] Figures 4a-4c This is a diagram showing the electrical properties of the boron phosphide semiconductor device prepared in Example 1 of this invention;

[0017] Figure 5 This is a SEM image of the boron phosphide fibers prepared in Example 2 of this invention;

[0018] Figure 6 This is a SEM image of the boron phosphide fibers prepared in Example 3 of the present invention;

[0019] Figure 7 This is the XRD pattern of the boron phosphide fiber prepared in Example 3 of the present invention. Detailed Implementation

[0020] In view of the deficiencies of the prior art, the inventors of this case, through long-term research and extensive practice, have proposed the technical solution of this invention. The technical solution of this invention will be clearly and completely described below. Obviously, the described embodiments are only some, not all, of the embodiments of this invention. All other embodiments obtained by those skilled in the art based on the embodiments of this invention without creative effort are within the scope of protection of this invention.

[0021] Specifically, as one aspect of the technical solution of the present invention, a method for preparing boron phosphide fiber includes: reacting a boron source with black phosphorus at high temperature under vacuum conditions to obtain boron phosphide fiber.

[0022] In some preferred embodiments, the preparation method specifically includes: thoroughly mixing a boron source with black phosphorus and placing it in a vacuum-sealed environment, then heating it to 600-1200°C at a rate of 1-15°C / min and reacting for 1-7 days, then cooling it to 100-400°C at a rate of 0.01-5°C / min, and then naturally cooling it to room temperature to obtain the boron phosphide fiber.

[0023] Furthermore, the boron source and black phosphorus can be thoroughly mixed and placed in a vacuum-sealed environment, then heated to 900-1050°C at a rate of 5-10°C / min and reacted for 1-2 days. After that, the temperature can be cooled to 200-300°C at a rate of 0.5-1°C / min, and then naturally cooled to room temperature to obtain the boron phosphide fiber.

[0024] For example, the boron source and black phosphorus can be thoroughly mixed and placed in a vacuum-sealed environment, then heated to 950-1050°C at a heating rate of 10°C / min and reacted for 2 days. After that, the temperature can be cooled to 200°C at a cooling rate of 1°C / min and then naturally cooled to room temperature to obtain the boron phosphide fiber.

[0025] Furthermore, the vacuum degree of the vacuum-sealed environment is 10. -3 Below Pa.

[0026] Furthermore, the boron source reacts with black phosphorus at 1050-1200℃ to prepare boron phosphide fibers with a beaded structure.

[0027] Furthermore, the boron source is reacted with black phosphorus at 900-1000℃ to prepare boron phosphide fibers with a smooth rod-like structure.

[0028] In some preferred embodiments, the boron source includes boron powder, but is not limited thereto.

[0029] Furthermore, the boron powder includes any one or more combinations of amorphous boron powder, single-crystal boron, and boron iodide, and is not limited thereto.

[0030] In some preferred embodiments, the molar ratio of the boron source to black phosphorus is 1:(1-4).

[0031] For example, the molar ratio of the boron source to black phosphorus is 1:1.

[0032] In some preferred embodiments, the preparation method specifically includes: subjecting a uniformly mixed boron source and black phosphorus to the high-temperature reaction in a vacuum-sealed environment under conditions where neither metal flux nor catalyst is present.

[0033] In some preferred embodiments, the preparation method further includes washing and drying the obtained product after the high-temperature reaction is completed.

[0034] Furthermore, the washing reagents used in the washing process include any one or more combinations of ethanol, acetone, and water, and are not limited thereto.

[0035] Furthermore, the drying temperature is 50-100℃, preferably 80℃.

[0036] In some more specific embodiments, the method for preparing the boron phosphide fiber includes:

[0037] Amorphous boron powder and black phosphorus were weighed in a molar ratio of 1:1, then ground and mixed in an agate mortar. The resulting mixture was then placed into a quartz tube and connected to a vacuum sealing machine, where it was slowly evacuated to a vacuum degree of 10. -3Pa, using a high-temperature flame torch to heat and seal the neck of the quartz tube and the quartz plug in a vacuum environment.

[0038] The vacuum-sealed quartz tube was placed in a tube furnace for a high-temperature reaction. Specifically, the temperature was increased to 950–1050°C at a rate of 10°C / min, held at that temperature for 2 days, and then decreased to 200°C at a rate of 1°C / min, finally allowed to cool naturally to room temperature. The product was then washed with ethanol and acetone, followed by centrifugation with deionized water. The resulting precipitate was dried in a drying oven at 80°C to obtain boron phosphide fibers.

[0039] Another aspect of the present invention provides boron phosphide fibers prepared by the aforementioned preparation method.

[0040] Furthermore, the boron phosphide fiber has a length of 20–200 μm and a diameter of 100–400 nm.

[0041] Furthermore, the surface of the boron phosphide fiber is smooth.

[0042] Furthermore, the boron phosphide fibers have a rod-like structure or a beaded structure.

[0043] Another aspect of this invention provides the use of the aforementioned boron phosphide fibers in the fabrication of semiconductor electronic devices or semiconductor optoelectronic devices. The semiconductor electronic device or semiconductor optoelectronic device may be a pn junction device.

[0044] The technical solution of the present invention will be further described in detail below with reference to several preferred embodiments and accompanying drawings. This embodiment is implemented on the premise of the technical solution of the invention, and provides detailed implementation methods and specific operation processes. However, the protection scope of the present invention is not limited to the following embodiments.

[0045] Unless otherwise specified, the experimental materials used in the examples below can be purchased from conventional biochemical reagent companies.

[0046] Example 1

[0047] Amorphous boron powder and black phosphorus were weighed in a molar ratio of 1:1, then ground and mixed in an agate mortar. The resulting mixture was then placed into a quartz tube and connected to a vacuum sealing machine, where it was slowly evacuated to a vacuum degree of 10. -3 Pa, using a high-temperature flame torch to heat and seal the neck of the quartz tube and the quartz plug in a vacuum environment.

[0048] The vacuum-sealed quartz tube was placed in a tube furnace for a high-temperature reaction. Specifically, the temperature was increased to 950°C at a rate of 10°C / min, held at that temperature for 2 days, and then decreased to 200°C at a rate of 1°C / min, finally allowed to cool naturally to room temperature. The product was then washed with ethanol and acetone, followed by centrifugation with deionized water. The resulting precipitate was dried in a drying oven at 80°C to obtain boron phosphide fibers.

[0049] Performance characterization:

[0050] The SEM image of the boron phosphide fibers prepared in this embodiment is shown below. Figure 1 As shown in the figure, the boron phosphide fiber is approximately several hundred micrometers long and has a diameter of 100nm to 400nm.

[0051] The Raman spectrum of the boron phosphide fiber prepared in this embodiment is as follows: Figure 2 As shown in the figure, the TO and LO peaks of the boron phosphide fiber are located at 799.1 cm⁻¹. -1 and 828.4cm -1 At this point, the two peaks LO and TO correspond to specific vibrational modes of boron phosphide phonons. By comparing with standard results, it was confirmed that the sample in this embodiment is boron phosphide.

[0052] The high-resolution TEM mapping image of the boron phosphide fibers prepared in this embodiment is as follows: Figures 3a-3c As shown in the figure, the distribution of boron and phosphorus elements is relatively uniform, further confirming that the sample in this embodiment is boron phosphide.

[0053] The electrical properties of the boron phosphide fibers prepared in this embodiment are as follows: Figures 4a-4c As shown, a field-effect transistor device was fabricated on a SiO2 substrate to study the carrier mobility of boron phosphide fibers (device diagram shown). Figure 4a ). Figure 4b As shown in the output characteristic curve, the source-drain current of the BP nanowire continuously decreases as the gate voltage increases from -80V to 80V, illustrating the p-type semiconductor nature of boron phosphide fibers. The transfer characteristic curve is shown in... Figure 4c As shown, the type of negative growth curve corresponds to the output characteristic curve. Calculations using the formula yield the carrier mobility of boron phosphide fiber to be μ = 2.38 × 10⁻⁶. -1 cm 2 V -1 s -1 .

[0054] Example 2

[0055] Single-crystal boron powder and black phosphorus were weighed in a molar ratio of 1:1, then ground and mixed in an agate mortar. The resulting mixture was then placed into a quartz tube and connected to a vacuum sealing machine, where it was slowly evacuated to a vacuum degree of 10. -3Pa, using a high-temperature flame torch to heat and seal the neck of the quartz tube and the quartz plug in a vacuum environment.

[0056] The vacuum-sealed quartz tube was placed in a tube furnace for a high-temperature reaction. Specifically, the temperature was increased to 950°C at a rate of 1°C / min, held at that temperature for 7 days, and then decreased to 400°C at a rate of 1°C / min, finally allowed to cool naturally to room temperature. The product was then washed with ethanol and acetone, followed by centrifugation with deionized water. The resulting precipitate was dried in a drying oven at 50°C to obtain boron phosphide fibers.

[0057] Performance characterization:

[0058] The SEM image of the boron phosphide fibers prepared in this embodiment is shown below. Figure 5 As shown in the figure, the boron phosphide fiber is approximately several hundred micrometers long and has a diameter of 100nm to 400nm.

[0059] Example 3

[0060] Amorphous boron powder and black phosphorus were weighed in a molar ratio of 1:1, then ground and mixed in an agate mortar. The resulting mixture was then placed into a quartz tube and connected to a vacuum sealing machine, where it was slowly evacuated to a vacuum degree of 10. -3 Pa, using a high-temperature flame torch to heat and seal the neck of the quartz tube and the quartz plug in a vacuum environment.

[0061] The vacuum-sealed quartz tube was placed in a tube furnace for a high-temperature reaction. Specifically, the temperature was increased to 1050°C at a rate of 10°C / min, held at that temperature for 2 days, and then decreased to 200°C at a rate of 1°C / min, finally allowed to cool naturally to room temperature. The product was then washed with ethanol and acetone, followed by centrifugation with deionized water. The resulting precipitate was dried in a drying oven at 80°C to obtain boron phosphide fibers.

[0062] Performance characterization:

[0063] The SEM image of the boron phosphide fibers prepared in this embodiment is shown below. Figure 6 As shown in the figure, the boron phosphide fibers are beaded, with a length of about several hundred micrometers and a diameter of 100nm to 400nm.

[0064] The XRD pattern of the boron phosphide fibers prepared in this embodiment is shown below. Figure 7 As shown, the peak positions of the synthesized sample match the cubic lattice structure of boron phosphide very well, proving the phase composition of the synthesized sample.

[0065] Example 4

[0066] Amorphous boron powder and black phosphorus were weighed in a molar ratio of 1:2, then ground and mixed in an agate mortar. The resulting mixture was then placed into a quartz tube and connected to a vacuum sealing machine, which was slowly evacuated to a vacuum degree of 10. -3 Pa, using a high-temperature flame torch to heat and seal the neck of the quartz tube and the quartz plug in a vacuum environment.

[0067] The vacuum-sealed quartz tube was placed in a tube furnace for a high-temperature reaction. Specifically, the temperature was increased to 900°C at a rate of 5°C / min, held at that temperature for 2 days, and then decreased to 200°C at a rate of 0.5°C / min, finally allowed to cool naturally to room temperature. The product was then washed with ethanol and acetone, followed by centrifugation with deionized water. The resulting precipitate was dried in a drying oven at 80°C to obtain boron phosphide fibers.

[0068] Example 5

[0069] Amorphous boron powder and black phosphorus were weighed in a molar ratio of 1:4, then ground and mixed in an agate mortar. The resulting mixture was then placed into a quartz tube and connected to a vacuum sealing machine, where it was slowly evacuated to a vacuum degree of 10. -3 Pa, using a high-temperature flame torch to heat and seal the neck of the quartz tube and the quartz plug in a vacuum environment.

[0070] The vacuum-sealed quartz tube was placed in a tube furnace for a high-temperature reaction. Specifically, the temperature was increased to 1050°C at a rate of 10°C / min, held at that temperature for one day, and then decreased to 300°C at a rate of 5°C / min, finally allowed to cool naturally to room temperature. The product was then washed with ethanol and acetone, followed by centrifugation with deionized water. The resulting precipitate was dried in a drying oven at 80°C to obtain boron phosphide fibers.

[0071] Comparative Example 1

[0072] The method is the same as in the example, except that the black phosphorus in Example 1 is replaced with red phosphorus, and boron phosphide fibers cannot be prepared in the end.

[0073] In addition, the inventors of this case also conducted experiments with other raw materials, process operations, and process conditions described in this specification, referring to the aforementioned embodiments, and obtained relatively ideal results in all cases.

[0074] It should be understood that the technical solutions of the present invention are not limited to the specific embodiments described above. Any technical modifications made to the technical solutions of the present invention without departing from the spirit and scope of the claims are within the scope of protection of the present invention.

Claims

1. A method for preparing boron phosphide fibers, characterized in that, include: Boron powder and black phosphorus were thoroughly mixed in the absence of metal flux and catalyst and placed in a vacuum-sealed environment. The mixture was then heated to 900-1050°C at a rate of 5-10°C / min and reacted for 1-2 days. After that, the mixture was cooled to 200-300°C at a rate of 0.5-1°C / min and then allowed to cool naturally to room temperature. The mixture was then washed with ethanol and acetone, followed by centrifugation with deionized water. The resulting precipitate was placed in a drying oven and dried at 80°C to obtain boron phosphide fibers.

2. The preparation method according to claim 1, characterized in that: The vacuum level of the vacuum-sealed environment is 10. -3 Below Pa.

3. The preparation method according to claim 1, characterized in that: The boron powder includes any one or a combination of two of amorphous boron powder and single-crystal boron powder.

4. The preparation method according to claim 1, characterized in that: The molar ratio of boron powder to black phosphorus is 1:(1-4).

5. Boron phosphide fibers prepared by any one of claims 1-4.

6. The boron phosphide fiber according to claim 5, characterized in that: The boron phosphide fiber has a length of 20~200 μm and a diameter of 100~400 nm.

7. The boron phosphide fiber according to claim 5, characterized in that: The boron phosphide fibers have a rod-like structure or a beaded structure.

8. Use of boron phosphide fiber according to any one of claims 5-7 in the preparation of semiconductor electronic devices.

Citation Information

Patent Citations

  • Boron phosphide single crystals and preparation method and application thereof

    CN110284195A

  • Boron phosphide material and preparation method thereof

    CN111333079A