Negative tone polyimide photoresist, method for manufacturing concavo-convex pattern, and semiconductor device

By combining a polyimide precursor with a specific structure and a photoinitiator, the problem of short storage and opening stability of negative polyimide photoresist solutions has been solved, achieving longer storage and opening stability, which is suitable for the semiconductor industry.

CN116794930BActive Publication Date: 2026-11-20CHANGZHOU LEADER NEW ELECTRONIC MATERIALS CO LTD +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202210270027.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-18
Publication Date
2026-11-20
Estimated Expiration
2042-03-18

AI Technical Summary

Technical Problem

Existing negative polyimide photoresist solutions have short storage and open-bottle stability periods, which cannot meet the long-term use requirements of the semiconductor industry.

Method used

By employing a combination of polyimide precursors and photoinitiators with specific structures, the storage and opening stability of the adhesive solution is improved through the formation of a conjugated system of imide bonds and large π-bond groups. Sensitizers, polymerization inhibitors, and crosslinking agents are added to enhance photosensitivity and crosslinking effect.

Benefits of technology

It significantly improves the storage and opening stability of the adhesive, extends its shelf life, and is suitable for applications in the semiconductor industry.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116794930B_ABST
    Figure CN116794930B_ABST
Patent Text Reader

Abstract

The application provides a negative polyimide photoresist, a preparation method of a concave-convex pattern and a semiconductor device. The negative polyimide photoresist comprises 100 parts of a polyimide precursor, 0.5-20 parts of a photoinitiator and 100-2000 parts of a solvent by weight; wherein the polyimide precursor has a structure shown in general formula (I), X, Y and R all have specific structures, and m is an integer of 5-10000. The application uses a specific polyimide precursor in combination with a photoinitiator to generate free radicals to initiate crosslinking polymerization reaction in the exposure process. In particular, the oxime ester photoinitiator has a larger conjugated system and stronger intramolecular electron transfer characteristics, is stable in storage and is not prone to generate free radicals to initiate crosslinking polymerization reaction, so that the viscosity and stability of the photoresist solution can be maintained, and the negative polyimide photoresist solution has good storage stability and bottle-opening stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of semiconductor technology, and more specifically, to a negative polyimide photoresist, a method for preparing embossed patterns, and a semiconductor device. Background Technology

[0002] Negative photosensitive polyimide resins have been widely used in the fabrication of micro-patterned circuits in the semiconductor field due to their excellent thermal stability, superior mechanical properties, low dielectric constant, high breakdown voltage, low coefficient of thermal expansion, excellent hydrolytic stability, and long-term stability. During application, a cross-linking chemical reaction occurs in the exposed areas after coating, forming "ionic-covalent-ionic" cross-linking bridges between macromolecules in these areas. These bridges are insoluble in the developer, leaving behind a polymer adhesive that forms various patterns after development. Patents CN1980984B, CN106471089B, CN109867787A, and CN106104381A disclose different combinations of negative photosensitive polyimide resins, which can meet the current needs of the semiconductor industry to varying degrees.

[0003] Negative photosensitive polyimide resin solutions contain photosensitive substances, and prolonged storage can lead to solvent evaporation and loss of photosensitivity. In particular, once opened, the solution is exposed to the external environment and is more susceptible to interference from external light and oxygen, resulting in short storage and open-bottle stability. Open-bottle stability refers to the number of days after opening the solution and placing it at room temperature and in air, testing its viscosity every 7 days, and then performing film preparation, exposure, and development according to a specific method, maintaining unchanged resolution, producing no residue, and with changes in film thickness and viscosity not exceeding 5%. Currently, the storage stability of existing negative polyimide resin solutions is approximately 6 months, and the open-bottle stability is approximately 30 days. However, the duration of storage and open-bottle stability is closely related to the shelf life of negative polyimide photoresist solutions. In practical applications in the semiconductor industry, there is a desire for negative polyimide resin solutions with longer storage and open-bottle stability to extend the shelf life and better align with semiconductor production schedules. Therefore, it is necessary to develop a negative polyimide photoresist with both long storage stability and bottle-opening stability. Summary of the Invention

[0004] The main objective of this invention is to provide a method for preparing negative polyimide photoresist, embossed patterns, and a semiconductor device to solve the problems of short storage stability and short opening stability of negative polyimide photoresist solutions in the prior art.

[0005] To achieve the above objectives, according to one aspect of the present invention, a negative polyimide photoresist is provided, comprising, by weight, 100 parts of a polyimide precursor, 0.5 to 20 parts of a photoinitiator, and 100 to 2000 parts of a solvent; wherein the polyimide precursor has the structure shown in general formula (I): ; General Formula (I) Where m is an integer from 5 to 10000, and X has the structures shown in structures I to VII: , Structural Formula I , Structural Formula II , Structural Formula III , Structural IV , Structural V ; Structural VI

[0006] Structural Formula VII

[0007] Y has the structures shown in structural formulas 1 to 3: , Structural Formula 1 , Structural Formula 2 ; Structural Formula 3 R has the structure shown in structural formula A: ; Structural Formula A The photoinitiator has the structure shown in formula B: .

[0008] Structural formula B

[0009] Furthermore, the repeating unit of the polyimide precursor is selected from one or more of the following units 1 to 3: , Unit 1 , Unit 2 ; Unit 3 Where m is an integer from 5 to 10000, and R has the structure shown in structure A: .

[0010] Structure A

[0011] Further, by weight, the negative polyimide photoresist also includes 2 to 10 parts of polymeric monomers containing unsaturated double bonds; preferably, the polymeric monomers containing unsaturated double bonds are acrylic compounds, more preferably one or more of polyethylene glycol diacrylate, polyethylene glycol dimethacrylate, and N-hydroxymethyl acrylate; more preferably, the number of ethylene glycol units in polyethylene glycol diacrylate is 5 to 10, and the number of ethylene glycol units in polyethylene glycol dimethacrylate is 5 to 10.

[0012] Further, by weight, the negative polyimide photoresist further includes 2 to 10 parts of sensitizer; preferably, by weight, the negative polyimide photoresist further includes 2 to 5 parts of sensitizer; preferably, the sensitizer is one or more of 1-phenyl-5-mercapto-1,2,3,4-tetrazazole, N,N-bis(2-hydroxyethyl)aniline, benzyl-2-naphthyl ether, 1,2-diphenoxyethylene, 4-morpholinobenzophenone, and michalcone.

[0013] Further, by weight, the negative polyimide photoresist also includes 0.01 to 3 parts of polymerization inhibitor; preferably, by weight, the photoresist composition also includes 0.01 to 1 part of polymerization inhibitor; more preferably, the polymerization inhibitor is one or more of N-nitrosodiphenylamine, hydroquinone, methylhydroquinone, p-benzoquinone, p-tert-butylcatechol and N-phenylnaphthylamine.

[0014] Further, by weight, the negative polyimide photoresist also includes 5 to 15 parts of crosslinking agent; preferably, the crosslinking agent is selected from amino resins and their derivatives; more preferably, the crosslinking agent is one or more of urea resin, glycol urea resin, hydroxyethylene urea resin, melamine resin, hexamethoxymethylated melamine, benzoic melamine resin and their derivatives; most preferably, the crosslinking agent is hexamethoxymethylated melamine.

[0015] Further, by weight, the negative polyimide photoresist comprises 100 parts of polyimide precursor, 2 to 10 parts of photoinitiator, 242 to 300 parts of solvent, 2 to 4 parts of sensitizer, 0.05 to 1 part of polymerization inhibitor, and 10 to 15 parts of crosslinking agent.

[0016] Further, the solvent is one or more of N-methyl-2-pyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, tetramethylurea, γ-butyrolactone, tetrahydrofuran, and acetone.

[0017] According to another aspect of the present invention, a method for preparing a raised pattern is also provided, comprising: step S1, coating the surface of a substrate with the aforementioned negative polyimide photoresist to obtain a coating or a substrate containing a coating; step S2, placing a patterned mask between a light source and an optional substrate containing a coating or an optional coating, and exposing the optional substrate containing a coating or the optional coating to the light source; step S3, removing the unexposed portions with a developing solution, and obtaining a raised pattern after heating; wherein the heating temperature is ≤450°C.

[0018] According to another aspect of the present invention, a semiconductor device is also provided, comprising the negative polyimide photoresist described above, or the raised pattern prepared by the above-described raised pattern preparation method.

[0019] By applying the technical solution of this invention, the -COOR group in the polyimide precursor forms an imide bond with the adjacent -CONH- group. Combined with the specific photoinitiator of this invention, a free radical-initiated cross-linking polymerization reaction can be generated during exposure, transforming the polyimide precursor into a polyimide resin. In particular, the oxime ester photoinitiator of this invention introduces large π-bond groups such as naphthalene rings and sulfur-containing heterocycles, possessing a large conjugated system and strong intramolecular electron transfer characteristics. It exhibits stable properties during storage and is less prone to free radical-initiated cross-linking polymerization reactions, thereby maintaining suitable viscosity and stability of the photoresist. This results in the negative polyimide photoresist solution exhibiting excellent storage and open-bottle stability, significantly superior to traditional negative polyimide photosensitive resin combinations, making it more suitable for applications in the semiconductor industry. Detailed Implementation

[0020] It should be noted that, unless otherwise specified, the embodiments and features described in this application can be combined with each other. The present invention will now be described in detail with reference to the embodiments.

[0021] As mentioned in the background section, existing technologies suffer from short storage and opening stability of negative polyimide photoresist solutions. To address these issues, in a typical embodiment of the present invention, a negative polyimide photoresist is provided, comprising, by weight, 100 parts of a polyimide precursor, 0.5–20 parts of a photoinitiator, and 100–2000 parts of a solvent; wherein the polyimide precursor has the structure shown in general formula (I): ; General Formula (I) Where m is an integer from 5 to 10000, and X has the structures shown in structures I to VII: , Structural Formula I , Structural Formula II , Structural Formula III , Structural IV , Structural V ; Structural VI

[0022] Structural Formula VII

[0023] Y has the structures shown in structural formulas 1 to 3: , Structural Formula 1 , Structural Formula 2 ; Structural Formula 3 R has the structure shown in structural formula A: ; Structural Formula A The photoinitiator has the structure shown in formula B: .

[0024] Structural formula B

[0025] In the polyimide precursor of this invention, the X groups are either low-conjugated structures or contain a large number of electron-donating groups, and the Y groups are either low-conjugated structures or contain a large number of electron-withdrawing groups. These features prevent the formation of strongly absorbing charge-transfer complexes, thereby improving photosensitivity or I-ray transmission. Simultaneously, the introduction of large π-bond groups in the aromatic system further enhances the storage and opening stability of the adhesive. During use, the -COOR groups in the polyimide precursor form imide bonds with adjacent -CONH- groups. In conjunction with a photoinitiator, free radicals are generated during exposure to initiate a cross-linking polymerization reaction, transforming the polyimide precursor into a polyimide resin. In particular, the oxime ester photoinitiator of the present invention introduces large π-bond groups such as naphthalene rings and sulfur-containing heterocycles, which have a large conjugated system and strong intramolecular electron transfer characteristics. It is stable during storage and does not easily generate free radicals to initiate cross-linking polymerization reactions, thereby maintaining the appropriate viscosity and stability of the adhesive solution. This makes the negative polyimide photoresist solution have good storage stability and bottle-opening stability, which is significantly better than traditional negative polyimide photosensitive resin combinations and more suitable for semiconductor industry applications.

[0026] Considering cost, the repeating units of the preferred polyimide precursor are selected from one or more of the following units 1 to 3: , Unit 1 , Unit 2 ; Unit 3 Where m is an integer from 5 to 10000, and R has the structure shown in structure A: .

[0027] Structure A

[0028] The aforementioned polyimide precursor can be prepared using conventional processes. To improve production efficiency, the following method is preferred: First, in the presence of an alkaline catalyst such as pyridine or triethylamine, an aromatic tetracarboxylic acid dianhydride having a tetravalent aromatic group X is reacted with an alcohol having photopolymerizable unsaturated bonds. Two carboxylic acid groups in the tetracarboxylic acid group form ester bonds, and the remaining two carboxylic acid groups form a dicarboxylic acid, yielding a diester compound. To further reduce costs, saturated fatty alcohols, such as methanol, ethanol, n-propanol, isopropanol, n-butanol, and tert-butanol, can be mixed into the unsaturated alcohol to effectively reduce the double bond density. The reaction solvent is an amide, lactone, sulfoxide, ketone, ether, halogenated hydrocarbon, hydrocarbon, or tetramethylurea, preferably one or more of N-methyl-2-pyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, tetramethylurea, or γ-butyrolactone, which can completely solubilize the diester and completely dissolve the polyimide precursor.

[0029] Second, under the action of a dehydrating condensing agent, the diester compound undergoes amide polycondensation in solution with a solvent or a dispersed diamine compound having a divalent organic group Y, thereby obtaining a polyimide precursor. The aforementioned dehydrating condensing agent is preferably dicyclohexylcarbodiimide, 1-ethoxycarbonyl-2-ethoxy-1,2-dihydroxyquinoline, 1,1'-carbonyldioxy-di-1,2,3-phenylpropanetriazole, N,N'-disuccinimidyl carbonate, etc. After the amide polycondensation reaction is complete, the dehydration condensation derivatives such as dicyclohexylurea precipitates from the reaction solution are filtered out as needed. Subsequently, the reaction solution is precipitated in water or a lower aliphatic solvent. Then, the precipitated polyimide precursor is dissolved again in the solvent, and the precipitation process is repeated for purification. Finally, vacuum drying is performed to separate the target polyamide. To further improve the purification process, the solution of the polyimide precursor can be passed through an elution column packed with ion exchange resin to remove ionic impurities.

[0030] To improve both the storage and opening stability of the photoresist and its photosensitivity, in a preferred embodiment, the negative polyimide photoresist further includes 2-10 parts by weight of a polymeric monomer containing unsaturated double bonds. Preferably, the polymeric monomer containing unsaturated double bonds is an acrylic compound, which can polymerize more rapidly under the action of a photoinitiator. More preferably, it is one or more of polyethylene glycol diacrylate, polyethylene glycol dimethacrylate, and N-hydroxymethyl acrylate. More preferably, the number of ethylene glycol units in polyethylene glycol diacrylate and polyethylene glycol dimethacrylate is 5-20. These small molecules containing polymerizable functional groups are more stable during the storage of the photoresist, participate in the photocuring reaction during the use of the photoresist to reduce the viscosity of the system, and can further improve the photosensitivity of the photocurable material.

[0031] To further improve the photosensitivity of the photoresist, in a preferred embodiment, the negative polyimide photoresist further includes 2 to 10 parts by weight of a sensitizer; preferably, the negative polyimide photoresist further includes 2 to 5 parts by weight of a sensitizer; preferably, the sensitizer is one or more of 1-phenyl-5-mercapto-1,2,3,4-tetrazazole, N,N-bis(2-hydroxyethyl)aniline, benzyl-2-naphthyl ether, 1,2-diphenoxyethylene, 4-morpholinobenzophenone, and micriton. These sensitizers themselves do not absorb light energy but synergistically participate in the photochemical reaction, working with the photoinitiator to initiate the crosslinking polymerization reaction, thereby improving the initiation efficiency while ensuring the storage stability and opening stability of the photoresist.

[0032] To improve the stability of the viscosity and photosensitivity of the composition solution during storage, in a preferred embodiment, the negative polyimide photoresist further includes 0.01 to 3 parts by weight of a polymerization inhibitor; preferably, the photoresist composition further includes 0.01 to 1 part by weight of a polymerization inhibitor. The polymerization inhibitor within the above range can improve the storage stability and opening stability of the solution without causing a decrease in photosensitivity due to excessive content. More preferably, the polymerization inhibitor is one or more of N-nitrosodiphenylamine, hydroquinone, methylhydroquinone, p-benzoquinone, p-tert-butylcatechol, and N-phenylnaphthylamine. During the storage of the solution, the above-mentioned polymerization inhibitor can better react with the small amount of chain free radicals generated to form non-free radical substances, thereby terminating the polymerization and improving the storage stability and opening stability of the solution, while being more suitable for the negative polyimide photoresist system of this application.

[0033] In a preferred embodiment, when the coating is heated and cured, the negative polyimide photoresist further includes 5-15 parts by weight of a crosslinking agent, thereby crosslinking the polyimide precursor or forming a crosslinked network, thus further enhancing its heat resistance. Preferably, the crosslinking agent is selected from amino resins and their derivatives; more preferably, the crosslinking agent is one or more of urea resin, glycol urea resin, hydroxyethylene urea resin, melamine resin, hexamethoxymethylated melamine, phenyl melamine resin, and their derivatives. These crosslinking agents possess dual photosensitive functional groups, and after exposure, they can more quickly generate dual free radicals and interact with the polyimide precursor phase, forming bridge bonds between polymer molecular chains and transforming into a three-dimensional insoluble substance. Most preferably, the crosslinking agent is hexamethoxymethylated melamine, which, while ensuring the crosslinking effect, further improves the storage stability and opening stability of the adhesive solution.

[0034] In practical applications, preferably, by weight, the negative polyimide photoresist comprises 100 parts of polyimide precursor, 2-10 parts of photoinitiator, 242-300 parts of solvent, 2-4 parts of sensitizer, 0.05-1 part of polymerization inhibitor, and 10-15 parts of crosslinking agent. In addition, various additives such as silane coupling agents can be added as needed to further improve the storage stability and opening stability of the negative polyimide photoresist solution.

[0035] In the preparation of photoresist, viscosity is generally adjusted by changing the concentration. In a preferred embodiment, the solvent is one or more of N-methyl-2-pyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, tetramethylurea, γ-butyrolactone, tetrahydrofuran, and acetone. The above solvents have good solubility for each component in the photoresist solution and are also more stable, further improving the stability of the photoresist solution.

[0036] In another typical embodiment of this application, a method for preparing an embossed pattern is also provided, comprising: step S1, coating the above-mentioned negative polyimide photoresist on the surface of a substrate to obtain a coating or a substrate containing a coating; step S2, placing a patterned mask between a light source and an optional substrate containing a coating or an optional coating, and exposing the optional substrate containing a coating or the optional coating to the light source; step S3, removing the unexposed portions using a developing solution, and obtaining an embossed pattern after heating; wherein the heating temperature is ≤450°C.

[0037] Specifically, the photosensitive resin composition is first coated onto a Si wafer, which serves as the substrate. Coating methods include spin coating, extrusion coating, spray coating, impregnation, printing, blade coating, or axial coating, with spin coating being preferred as it allows for easier adjustment of the coating thickness by adjusting the rotation speed. By setting the solid content of the composition and the coating speed, the final cured film thickness is controlled to be 0.1–20 μm. The coating or the substrate containing the coating is then pre-baked at 80–120°C. After drying, the coating is irradiated with active light in the desired pattern shape through a photomask. The active light can be X-rays, electron beams, ultraviolet light, or visible light, preferably with a wavelength of 200–500 nm, and most preferably i-line with a wavelength of 365 nm. A conventional contact lithography machine or a stepper lithography machine can be used. Alternatively, laser irradiation with chemical rays can be used to directly draw patterns on the coating, followed by exposure baking or pre-development baking at 40~120℃ for 10~240 seconds as needed.

[0038] Finally, the unexposed areas are removed using a developer to obtain the raised pattern. The developer can be a good solvent for the polyimide precursor or a mixture of good and bad solvents. Good solvents include one or more of N-methyl-2-pyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, N-acetyl-2-pyrrolidone, dimethyl sulfoxide, γ-butyrolactone, α-acetyl-γ-butyrolactone, cyclopentanone, and cyclohexanone. Bad solvents include one or more of toluene, xylene, methanol, ethanol, isopropanol, propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, and water. When using a mixture of good and bad solvents, the mixing ratio can be adjusted according to the solubility of the polyamide resin coating to be developed and the development method. The development method can be selected from methods such as immersion, scraper, or spin coating as needed. After development, the negative raised pattern formed by development is cleaned with a rinsing solution to remove the developer. The rinsing solution is one or more of distilled water, methanol, ethanol, isopropanol, toluene, xylene, propylene glycol monomethyl ether acetate, and propylene glycol monomethyl ether. After rinsing, the embossed pattern is heated below 450°C to induce a dehydration cyclization reaction, resulting in a cured embossed pattern made of polyimide resin with excellent heat resistance. The heating cyclization reaction can be carried out in an air or inert gas atmosphere such as nitrogen or helium using equipment such as hot plates, inert ovens, or heating furnaces.

[0039] In another typical embodiment of this application, a semiconductor device is also provided, including the aforementioned negative polyimide photoresist or the aforementioned raised / lowered pattern prepared by the above-described method. In the semiconductor manufacturing process, by using the raised / lowered pattern thus cured as a protective film, insulating film, or α-line cutoff film of the semiconductor, this raised / lowered pattern can be effectively utilized in semiconductor manufacturing.

[0040] The present application will be further described in detail below with reference to specific embodiments, which should not be construed as limiting the scope of protection claimed in the present application.

[0041] Example 1

[0042] Synthesis of polyimide precursor (PAE): 32.2225 g (100 mmol) of 3,3',4,4'-benzophenone tetracarboxylic dianhydride, 50 mL of γ-butyrolactone (GBL), 26.505 g (200 mol) of hydroxyethyl methacrylate, and 15.820 g (200 mmol) of pyridine were added to a 1 L flask and stirred at room temperature for 12 h. Then, after cooling at -10 °C for 20 min, a solution of 41.266 g (200 mmol) of dicyclohexylcarbodiimide dissolved in 20 mL of GBL was added dropwise, and the mixture was stirred at low temperature for 30 min. After reacting for 2 hours, 32.0233 g (90 mmol) of 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl dissolved in 80 mL of GBL was slowly added, and the mixture was stirred for 2 h, followed by stirring at room temperature for 5 h. Subsequently, 6 mL of ethanol was added to the reaction system to quench the reaction, and 80 mL of LGBL was added for dilution. The dehydration condensation precipitate (dicyclohexylurea) was removed by filtration. The reaction solution was then precipitated into methanol, and the precipitated polymer was separated. The polymer was then redissolved in 80 mL of LGBL, passed through an ion exchange resin, and the solution was slowly added dropwise to 1 L of ion-exchanged water. After the polymer was completely precipitated, it was recovered, washed with water, and dried under vacuum at 40°C for 24 hours to obtain the polyimide precursor resin PAE, with the following structure: Where m is 30 and R is The weight-average molecular weight (converted from polystyrene) of PAE, determined by gel permeation chromatography (GPC), was 21,000.

[0043] Preparation of negative polyimide photoresist: 100 parts by weight of the above-mentioned polyimide precursor PAE, 4 parts by weight of tetraethylene glycol methacrylate, 1 part by weight of photoinitiator, 1 part by weight of 1-phenyl-5-mercapto-1,2,3,4-tetraazole, 3 parts by weight of N,N-bis(2-hydroxyethyl)aniline, 0.05 parts by weight of N-nitrosodiphenylamine, and 10 parts by weight of hexamethoxymethylated melamine were dissolved in 242 parts by weight of N-methyl-2-pyrrolidone (NMP) solution. The solution was then filtered through a polytetrafluoroethylene filter with a pore size of 0.5 micrometers to obtain a varnish-like negative polyimide photoresist solution. The photoinitiator has the structure shown in structure B. .

[0044] Structure B

[0045] Example 2

[0046] The only difference between Example 2 and Example 1 is that the photoinitiator is 10 parts by weight.

[0047] Example 3

[0048] The only difference between Example 3 and Example 1 is that the photoinitiator is 20 parts by weight.

[0049] Example 4

[0050] The only difference between Example 4 and Example 1 is that the polyimide precursor is... Where m is 30 and R is .

[0051] Example 5

[0052] The only difference between Example 5 and Example 1 is that the polyimide precursor is... Where m is 30 and R is .

[0053] Example 6

[0054] The only difference between Example 6 and Example 1 is that the polyimide precursor is... , where X is m is 30.

[0055] Example 7

[0056] The only difference between Example 7 and Example 1 is that the polyimide precursor is... , where X is m is 30.

[0057] Example 8

[0058] The only difference between Example 8 and Example 1 is that the polyimide precursor is... , where X is m is 30.

[0059] Comparative Example 1

[0060] The only difference between Comparative Example 1 and Example 1 is that the photoinitiator is 1,3-diphenylpropanetrione-2-(O-ethylcarbonyl).

[0061] Comparative Example 2

[0062] The only difference between Comparative Example 2 and Example 1 is that the photoinitiator is 2,2'-diethoxyacetophenone.

[0063] Comparative Example 3

[0064] The only difference between Comparative Example 3 and Example 1 is that the photoinitiator is benzophenone.

[0065] Comparative Example 4

[0066] The only difference between Comparative Example 4 and Example 1 is that the photoinitiator is 0.2 parts by weight.

[0067] Comparative Example 5

[0068] The only difference between Comparative Example 5 and Example 1 is that the photoinitiator is 0.5 parts by weight.

[0069] Comparative Example 6

[0070] The only difference between Comparative Example 6 and Example 1 is that the photoinitiator is 25 parts by weight.

[0071] Comparative Example 7

[0072] The only difference between Comparative Example 7 and Example 1 is that the polyimide precursor is... , where m is 40.

[0073] The resin compositions of Examples 1-7 and Comparative Examples 1-7 above were coated onto a 5-inch silicon wafer using a spin coater and pre-baked at 80°C for 40 minutes to obtain a film with an initial thickness of 10 micrometers. Using an i-line stepper, with a photomask in between, the film was then exposed to 50-600 mJ / cm². 2 Within the range, at 50 mJ / cm per level 2 The exposure was adjusted incrementally. Thirty minutes after initial exposure, development was performed via spin-spray using a 50 / 50 (v / v) mixture of γ-butyrolactone and xylene. This development time was 1.4 times the time required for the unexposed portions to completely dissolve and disappear. The mixture was then rinsed with isopropanol via spin-spray for 10 seconds to obtain a raised pattern formed from polyimide resin. The raised pattern was observed using an optical microscope (Olympus MX63L) to evaluate the minimum exposure required to obtain a well-defined pattern, the size (resolution) of the aperture irradiated, and the presence or absence of residual resin in the unexposed portions.

[0074] Resin storage stability: After preparing the adhesive solution, it is sealed in a nitrogen-filled glove box and then stored at 0°C in a refrigerator. Every 30 days, a portion of the adhesive solution is taken out from the nitrogen-filled glove box to test its viscosity, and then film preparation, exposure, and development are performed according to the above method. The resolution should remain constant, with no adhesive residue, and changes in film thickness and viscosity not exceeding 5% are defined as no change. The number of days during which these properties remain unchanged is the storage stability of the adhesive solution.

[0075] Open-bottle stability of the adhesive: After opening, the adhesive is placed at room temperature and exposed to air. Every 7 days, a portion of the adhesive is taken out to test its viscosity, and then film is prepared, exposed, and developed according to the method described above. The resolution should remain unchanged, with no adhesive residue, and the film thickness and viscosity changes should not exceed 5% to be considered unchanged. The number of days during which these properties remain unchanged is the open-bottle stability of the adhesive.

[0076] The test results are shown in Tables 1 to 3.

[0077] Table 1

[0078] Table 2

[0079] Table 3

[0080] In Table 3, Comparative Examples 4 and 5, due to their low initiator content, could not form effective photolithographic patterns, thus making it impossible to obtain results regarding resolution, presence or absence of residual adhesive, storage stability, and open-bottle stability of the adhesive solution. Comparative Example 6, due to its excessively high initiator content, resulted in residual adhesive, making it impossible to obtain results regarding storage stability and open-bottle stability of the adhesive solution.

[0081] As can be seen from the above, in the embodiments of the present invention, when the type and content of the photoinitiator are within the scope of the present invention, and when the polyimide precursor used is the precursor of the present invention, better resolution (5 μm), good storage stability, and good bottle-opening stability can be obtained. Compared with the resin combination using other photoinitiators and their contents and other precursors in the comparative examples, the resin using the specific content of the photoinitiator and precursor of the present invention has significantly longer storage stability and bottle-opening stability.

[0082] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A negative polyimide photoresist, characterized in that, By weight, the negative polyimide photoresist comprises 100 parts of polyimide precursor, 0.5 to 20 parts of photoinitiator, and 100 to 2000 parts of solvent; wherein the polyimide precursor has the structure shown in general formula (I): General formula (I); Where m is an integer from 5 to 10000, and X has the structure shown in the following formula: Structural Form II Structural Form III Structural VI; Structural formula VII; Y has the structures shown in structural formulas 1 to 3: Structural Formula 1 Structural Formula 2 Structure 3; R has the structure shown in structural formula A: Structural formula A; The photoinitiator has the structure shown in formula B: Structural formula B.

2. The negative polyimide photoresist according to claim 1, characterized in that, The repeating unit of the polyimide precursor is selected from one or more of the following units 1 to 3: Unit 1 Unit 2 Unit 3; Where m is an integer from 5 to 10000, and R has the structure shown in structure A: Structure A.

3. The negative polyimide photoresist according to claim 1 or 2, characterized in that, The negative polyimide photoresist further includes 2 to 10 parts by weight of polymeric monomers containing unsaturated double bonds.

4. The negative polyimide photoresist according to claim 3, characterized in that, The polymeric monomer containing unsaturated double bonds is an acrylic acid compound.

5. The negative polyimide photoresist according to claim 4, characterized in that, The polymeric monomer containing unsaturated double bonds is one or more of polyethylene glycol diacrylate and polyethylene glycol dimethacrylate.

6. The negative polyimide photoresist according to claim 5, characterized in that, The number of ethylene glycol units in the polyethylene glycol diacrylate is 5 to 10, and the number of ethylene glycol units in the polyethylene glycol dimethacrylate is 5 to 10.

7. The negative polyimide photoresist according to claim 1 or 2, characterized in that, The negative polyimide photoresist further includes 2 to 10 parts of sensitizer by weight.

8. The negative polyimide photoresist according to claim 7, characterized in that, The negative polyimide photoresist further comprises 2 to 5 parts of the sensitizer by weight.

9. The negative polyimide photoresist according to claim 8, characterized in that, The sensitizer is one or more of 1-phenyl-5-mercapto-1,2,3,4-tetrazazole, N,N-bis(2-hydroxyethyl)aniline, benzyl-2-naphthyl ether, 1,2-diphenoxyethylene, 4-morpholinobenzophenone, and michidone.

10. The negative polyimide photoresist according to claim 7, characterized in that, The negative polyimide photoresist further includes 0.01 to 3 parts by weight of polymerization inhibitor.

11. The negative polyimide photoresist according to claim 10, characterized in that, The photoresist further includes 0.01 to 1 part of the polymerization inhibitor by weight.

12. The negative polyimide photoresist according to claim 11, characterized in that, The polymerization inhibitor is one or more of N-nitrosodiphenylamine, hydroquinone, methylhydroquinone, p-benzoquinone, p-tert-butylcatechol, and N-phenylnaphthylamine.

13. The negative polyimide photoresist according to claim 10, characterized in that, The negative polyimide photoresist further comprises 5 to 15 parts by weight of crosslinking agent.

14. The negative polyimide photoresist according to claim 13, characterized in that, The crosslinking agent is selected from amino resins and their derivatives.

15. The negative polyimide photoresist according to claim 14, characterized in that, The crosslinking agent is one or more of urea resin, melamine resin, hexamethoxymethylated melamine, benzoated melamine resin, and their derivatives.

16. The negative polyimide photoresist according to claim 15, characterized in that, The crosslinking agent is hexamethoxymethylated melamine.

17. The negative polyimide photoresist according to claim 13, characterized in that, By weight, the negative polyimide photoresist comprises 100 parts of the polyimide precursor, 2 to 10 parts of the photoinitiator, 242 to 300 parts of the solvent, 2 to 4 parts of the sensitizer, 0.05 to 1 part of the polymerization inhibitor, and 10 to 15 parts of the crosslinking agent.

18. The negative polyimide photoresist according to claim 1, characterized in that, The solvent is one or more of N-methyl-2-pyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, tetramethylurea, γ-butyrolactone, tetrahydrofuran, and acetone.

19. A method for preparing a raised or recessed pattern, characterized in that, The preparation method includes: Step S1: Coating the substrate surface with the negative polyimide photoresist according to any one of claims 1 to 18 to obtain a coating or a substrate containing the coating. Step S2: A patterned mask is placed between the light source and the substrate containing the coating or the coating, and the substrate containing the coating or the coating is exposed using the light source. Step S3: Remove the unexposed areas using a developing solution, and obtain the raised pattern after heating; Wherein, the heating temperature is ≤450℃.

20. A semiconductor device, characterized in that, The semiconductor device includes the negative polyimide photoresist according to any one of claims 1 to 18, or the embossed pattern prepared by the method of claim 19.

Citation Information

Patent Citations

  • Photosensitive resin composition, cured-relief-pattern production method, and semiconductor device

    CN106104381A

  • Heat-generating alkali agents, thermosetting resin compositions and their uses

    CN106471089B

  • Polyimide precursor, resin composition, cured film and preparation methods of polyimide precursor and cured film

    CN109867787A

  • Polyamide

    CN1980984B

  • Photosensitive resin composition, method for manufacturing cured relief pattern and semiconductor device

    JP2011164289A