Composite oxide, method for producing the same, hydrogenation catalyst, and use thereof

By preparing a composite oxide support of alumina and titanium dioxide, the problems of low activity and easy deactivation of existing catalysts were solved, realizing low-temperature and high-efficiency alkyne hydrogenation reaction, reducing costs and improving the stability and selectivity of the catalyst.

CN116803502BActive Publication Date: 2026-11-24CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202211376863.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2022-03-24
Filing Date
2022-11-04
Publication Date
2026-11-24
Estimated Expiration
2042-11-04

AI Technical Summary

Technical Problem

Existing selective hydrogenation catalysts for alkynes suffer from low activity and poor selectivity. Precious metal catalysts are prone to loss and are costly, while non-precious metal catalysts are easily deactivated under high concentrations of alkynes, resulting in serious green oil problems and affecting service life.

Method used

A non-precious metal catalyst with a coral-like 3D layered structure was prepared by using a composite oxide of alumina and titanium dioxide as a support. By controlling the pH and temperature during the preparation process, the predominance of anatase titanium dioxide was ensured, thereby improving the specific surface area and pore size distribution of the catalyst and enhancing the active sites and light-harvesting ability.

Benefits of technology

It achieves highly active, highly selective and stable alkyne hydrogenation reactions at low temperatures, reduces catalyst costs, extends service life, and improves resistance to impurity poisoning.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116803502B_ABST
    Figure CN116803502B_ABST
Patent Text Reader

Abstract

This invention relates to a composite oxide comprising 60-95 wt% alumina and 5-40 wt% titanium dioxide, wherein the specific surface area of ​​the composite oxide, determined by the BET method, is expressed as X m. 2 The average pore size of the composite oxide, expressed as Y nm, determined by nitrogen adsorption isotherm method, is denoted by X nm, where the ratio of X to Y is 5 to 30. Furthermore, by X-ray diffraction, the anatase phase titanium dioxide in the composite oxide comprises 95 wt% to 100 wt% of the total titanium dioxide, where X is in the range of 50 to 200, preferably in the range of 60 to 180, more preferably in the range of 80 to 150, and Y is in the range of 5 to 25 nm. This invention also provides a hydrogenation catalyst comprising the composite oxide, which exhibits high vinylacetylene conversion and high 1,3-butadiene selectivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a composite oxide, a method for preparing the composite oxide, a hydrogenation catalyst, and its applications, specifically for the hydrogenation removal of alkynes from C4 fractions and the increase in butadiene production. Background Technology

[0002] C4 fraction refers to a mixture of various alkanes, alkenes, dienes, and alkynes containing four carbon atoms. It mainly originates from refinery gas produced during petroleum refining and byproducts of ethylene production from petroleum hydrocarbon cracking. Cracked C4 fractions contain saturated and unsaturated hydrocarbons such as n-butane, isobutane, 1-butene, trans-2-butene, cis-2-butene, isobutene, 1,2-butadiene, 1,3-butadiene, methylacetylene, ethylacetylene, and vinylacetylene. Industrially, it is mainly used to produce 1,3-butadiene, isobutene, and 1-butene.

[0003] The C4 fraction produced as a byproduct of high-temperature cracking of hydrocarbons to produce ethylene typically contains 40%-60% butadiene by mass. Butadiene is an important monomer in the synthetic rubber industry. The extraction of butadiene from the C4 fraction usually employs solvent extraction methods, such as the acetonitrile method, the N-methylpyrrolidone method, and the dimethylformamide method. Currently, these methods generally meet the requirements for butadiene purity.

[0004] Due to factors such as cracking depth and cracking technology, the alkyne content in the cracked C4 fraction gradually increases, leading to increased butadiene loss and Nectar content during extraction. Simultaneously, with the development of organic synthesis technology, the restrictions on alkyne content in butadiene have become more stringent. These factors all contribute to decreased economic efficiency of butadiene extraction units. Selectively hydrogenating the bulk hydrocarbons during butadiene extraction to recover a portion of the butadiene not only achieves the goal of turning waste into treasure but also plays a crucial role in reducing alkyne emissions and preventing environmental pollution.

[0005] Currently, alkynes in mixed C4 fractions can be removed by catalytic selective hydrogenation. The catalysts used primarily tend to be noble metal catalysts, such as palladium, platinum, and silver, followed by non-noble metal catalysts, such as copper and nickel.

[0006] The selective hydrogenation of alkynes in hydrocarbon streams requires different catalysts and reaction conditions depending on the composition of the feedstock and the desired product. A good selective hydrogenation catalyst, besides possessing high hydrogenation activity, should also exhibit good stability, meaning it should be resistant to impurities and gum deposits to extend its lifespan. Therefore, the support should have low acidity, a small specific surface area, and a large pore size. Furthermore, adding certain promoters during catalyst preparation can also extend the catalyst's lifespan.

[0007] Noble metal catalysts typically employ palladium catalysts supported on a carrier (usually alumina), with the addition of other co-catalyst components such as gold, silver, chromium, copper, iron, rhodium, lithium, potassium, and even lead or zinc. Noble metal catalysts exhibit good low-temperature activity and mild reaction conditions, but their drawbacks include easy loss of active components, high cost, difficulty in regeneration, and slightly poor hydrogenation selectivity. Non-noble metal catalysts require higher temperatures and harsher hydrogenation conditions, but their preparation is simple, they are easy to regenerate repeatedly, and their cost is relatively low, thus still possessing considerable research and development value. In these hydrogenation reactions, semi-hydrogenated free radicals adsorbed on the catalyst react with adjacent alkynes or dienes to form a viscous polymer (commonly known as green oil), mainly composed of compounds with more than six carbon atoms. Because this polymer covers the catalyst surface, it blocks the micropores, reducing catalyst activity and affecting its lifespan. This is especially true for conjugated dienes (such as 1,3-butadiene), whose polymerization reaction is more readily carried out, leading to rapid catalyst deactivation. Therefore, the catalyst must be frequently regenerated for reuse.

[0008] In the application research of selective hydrogenation of C4 alkynes, it has been recognized that nickel-based selective hydrogenation catalysts are safer and more efficient for feedstocks with high alkyne content. However, the activity and selectivity of nickel-based selective hydrogenation catalysts are somewhat inferior to those of noble metal palladium-based catalysts, limiting their application. Therefore, for non-noble metal catalysts used in the selective hydrogenation of alkynes, it is necessary to further improve the activity and selectivity of these catalysts, research countermeasures to address the green oil problem during catalyst use, and extend catalyst life. Using non-noble metal hydrogenation catalysts for the selective hydrogenation of alkynes can improve the catalyst's resistance to impurity poisoning and its stability, which has economic value.

[0009] Research in the field of photocatalysts has shown that the structure and shape of TiO2-based catalytic materials can significantly influence their light absorption efficiency. Coral reefs possess excellent light absorption and reflection structures, thus providing a three-dimensional (3D) environment for many marine plants and animals and absorbing small particles, supporting approximately one-quarter of all known marine life. Coral-like 3D layered structures can have a higher specific surface area, resulting in more active sites and stronger light-harvesting capabilities, and have been shown to exhibit better photocatalytic performance than other structures. Using specific catalytic materials with coral reef-like morphologies can improve the performance of TiO2-supported catalysts. Summary of the Invention

[0010] To address the shortcomings of existing technologies, the present invention aims to provide a non-precious metal selective hydrogenation catalyst that exhibits high low-temperature activity, high selectivity, and high stability. Compared to precious metal selective hydrogenation catalysts for acetylene removal, the catalyst disclosed herein can reduce investment costs by more than 80%, and also possesses better resistance to impurity poisoning and better adaptability to feedstocks.

[0011] In a first aspect, the present invention provides a composite oxide comprising aluminum oxide and titanium dioxide, wherein the specific surface area of ​​the composite oxide is expressed as X m 2 / g, the average pore size of the composite oxide is expressed as Y nm, where the ratio of X to Y is 5 to 30; and wherein in the composite oxide, anatase titanium dioxide accounts for 95 wt%-100 wt% of the total titanium dioxide. Preferably, the ratio of X to Y is 5 to 15. More preferably, the ratio of X to Y is 5 to 10. Preferably, in the composite oxide, anatase titanium dioxide accounts for 96 wt%-100 wt% of the total titanium dioxide. Preferably, in the composite oxide, anatase titanium dioxide accounts for 97 wt%-100 wt% of the total titanium dioxide. Preferably, in the composite oxide, anatase titanium dioxide accounts for 98 wt%-100 wt% of the total titanium dioxide. Preferably, in the composite oxide, anatase titanium dioxide accounts for 99 wt%-100 wt% of the total titanium dioxide.

[0012] In this invention, the proportion of anatase phase titanium dioxide to total titanium dioxide can be measured by X-ray diffraction analysis.

[0013] In this invention, the specific surface area of ​​the composite oxide can be determined by the BET method.

[0014] In this invention, the average pore size of the composite oxide can be determined by the nitrogen adsorption isotherm method.

[0015] In some embodiments of the present invention, the diffraction peak area representing the crystal structure of anatase titanium dioxide, as measured by X-ray diffraction analysis, accounts for 95wt%-100wt% of the diffraction peak area of ​​all titanium dioxide crystal structures.

[0016] In some embodiments of the present invention, the diffraction peak area representing the crystal structure of anatase titanium dioxide, as measured by X-ray diffraction analysis, accounts for 96 wt% to 100 wt% of the diffraction peak area of ​​all titanium dioxide crystal structures.

[0017] In some embodiments of the present invention, the diffraction peak area representing the crystal structure of anatase titanium dioxide, as measured by X-ray diffraction analysis, accounts for 97wt%-100wt% of the diffraction peak area of ​​all titanium dioxide crystal structures.

[0018] In some embodiments of the present invention, the diffraction peak area representing the crystal structure of anatase titanium dioxide, as measured by X-ray diffraction analysis, accounts for 98 wt% to 100 wt% of the diffraction peak area of ​​all titanium dioxide crystal structures.

[0019] In some embodiments of the present invention, the pore volume of the composite oxide, determined by a P / Po single-point desorption curve, is Z mL / g, and the ratio of X to Z is 220 to 400, preferably 250 to 350. In some embodiments, the ratio of X to Z is 250, 260, 270, 280, 290, 300, 310, 320, 330, 340, 350, or any combination thereof.

[0020] In some embodiments of the invention, X is 90 to 150. In some embodiments, X is 90, 100, 110, 120, 130, 140, 150, or any combination thereof.

[0021] In some embodiments of the invention, Y is 9 to 20, preferably 12 to 16. In some embodiments, Y is 12, 13, 14, 15, 16, or any combination thereof.

[0022] In some embodiments of the present invention, in the composite oxide, pores with a diameter in the range of 10-20 nm account for at least 85% of all pores by volume.

[0023] In some embodiments of the invention, Z is 0.3 to 0.5, preferably 0.3 to 0.4. In some embodiments, Z is 0.31, 0.32, 0.33, 0.34, 0.35, 0.36, 0.37, 0.38, 0.39, 0.40, or any combination thereof.

[0024] In some embodiments of the invention, the composite oxide contains 5 wt% to 21 wt% titanium dioxide, based on the total weight of the composite oxide. In some embodiments, the composite oxide contains 5 wt%, 6 wt%, 8 wt%, 10 wt%, 12 wt%, 15 wt%, 18 wt%, 20 wt%, 21 wt% titanium dioxide, or any combination thereof.

[0025] According to some embodiments of the present invention, the composite oxide contains 79 wt% to 95 wt% alumina, based on the total weight of the composite oxide.

[0026] In some embodiments of the present invention, the composite oxide has a coral-like 3D layered structure. The coral-like 3D layered structure can have a higher specific surface area, thereby possessing more active sites and stronger light-harvesting capabilities.

[0027] In a second aspect, the present invention provides a method for preparing a composite oxide, which yields an alumina-titanium dioxide composite oxide with a coral reef 3D microstructure. The preparation method of the present invention includes the following steps:

[0028] Step I. Dissolve the soluble aluminum source in water to form an aluminum source solution, dissolve the titanium source in an acid solution to form a titanium source solution, and mix the ammonium salt and the alkaline solution to form a mixed alkaline solution;

[0029] Step II. (a) Add the titanium source solution and the mixed alkaline solution to the aluminum source solution, so that the resulting mixture is maintained at a first pH value for a first time period; (b) Add an additional mixed alkaline solution to the mixture, so that the resulting mixture is maintained at a second pH value for a second time period; (c) Add an additional titanium source solution to the mixture, so that the resulting mixture is maintained at a third pH value for a third time period.

[0030] Step III. After step II.(c), the temperature of the mixture is raised and maintained for a fourth time period to obtain a precipitate;

[0031] Step IV. The precipitate is dried and calcined to obtain a composite oxide containing alumina and titanium dioxide. Preferably, the precipitate is also washed and filtered before drying (to remove unwanted impurities).

[0032] The resulting composite oxide has the compositional and structural features described in the first aspect of the invention.

[0033] In some embodiments of the method of the present invention, in step II, the first pH value is less than 5, preferably 3 to 4. In some embodiments of the method of the present invention, in step II, the second pH value is greater than 8.5, preferably 9 to 10. In some embodiments of the method of the present invention, in step II, the third pH value is greater than 7 and less than 9, preferably 7.5 to 8.5.

[0034] In some embodiments of the method of the present invention, in step II, the first time period, the second time period, and the third time period are 5 to 20 minutes, preferably 10 to 15 minutes.

[0035] In some embodiments of the method of the present invention, in step III, the fourth time period is 20 to 60 minutes.

[0036] In some embodiments of the method of the present invention, in step II, the operating temperature is 25°C to 60°C, preferably 50°C to 60°C.

[0037] In some embodiments of the method of the present invention, in step III, the temperature is raised to 80°C to 150°C, preferably 80°C to 100°C. In some embodiments, in step III, the temperature is raised to 80°C, 85°C, 90°C, 92°C, or 95°C.

[0038] In some embodiments of the method of the present invention, in step IV, the drying temperature is 110°C to 130°C. The drying time is 4-12 hours, preferably 6-10 hours.

[0039] In some embodiments of the method of the present invention, in step IV, the calcination temperature is 800°C to 1000°C. In some embodiments, in step IV, the calcination temperature is within the range of 800°C, 850°C, 900°C, 950°C, or any combination thereof. The calcination time is 4-12 hours, preferably 5-8 hours.

[0040] In some embodiments of the method of the present invention, the aluminum concentration of the aluminum source solution is 0.5 to 2.5 mol / L. The aluminum source is a soluble aluminum salt, and may be selected from one or more of aluminum sulfate, aluminum chloride, aluminum nitrate, and organic aluminum such as aluminum isopropoxide, aluminum sec-butoxide, aluminum monoacetate, and aluminum diacetate.

[0041] In some embodiments of the method of the present invention, the titanium concentration of the titanium source solution is 0.2 to 1.2 mol / L. The titanium source is a soluble titanium source, which may be selected from titanium salts such as titanium acetate, hydrochloride, sulfate, nitrate, or from titanate esters such as tetraethyl titanate, tetra-n-propyl titanate, tetraisopropyl titanate, and tetrabutyl titanate.

[0042] In some embodiments of the method of the present invention, the concentration of the ammonium salt in the mixed alkaline solution is 0.1 to 0.3 mol / L. The ammonium salt may be selected from one or more of ammonium bicarbonate, ammonium carbonate, and organic ammonium salts.

[0043] In some embodiments of the method of the present invention, the concentration of the alkaline solution is 0.2 to 0.4 mol / L. The alkaline solution may be selected from one or more of ammonia, sodium hydroxide, potassium hydroxide, and organic bases such as triethylamine, N,N-2-toluidine, pyridine, and quinoline.

[0044] In some embodiments of the method of the present invention, the acid solution may be selected from one or more of sulfuric acid, nitric acid, hydrochloric acid, and organic acids such as formic acid, acetic acid, citric acid, and oxalic acid.

[0045] In some embodiments of the method of the present invention, the reactant feed examples in steps II(a), II(b), and II(c) are as follows:

[0046] The feeding ratio of the titanium source solution in steps II(a) and II(c) can be 1:4-2:3. Alternatively, the amount of titanium source solution fed in step II(a) accounts for 20%-40% of the total titanium source solution volume in the method, and the amount fed in step II(c) accounts for 60%-80% of the total titanium source solution volume in the method.

[0047] The ratio of the mixed alkaline solution in steps II(a) and II(b) can be in the range of 2:1 to 1:2, or in the range of 1.5:1 to 1:1. Alternatively, the amount of the mixed alkaline solution in step II(a) can be 33%-67%, preferably 50%-60%, and in step II(b) can be 33%-670%, preferably 40%-50%, relative to the total volume of the mixture in II(a) and II(b).

[0048] In some embodiments of the method of the present invention, in step IV, the precipitate washing process includes washing with deionized water until the acid radical ions are undetectable, drying at a temperature of 100°C to 120°C, drying for 4°C to 12 hours, and calcining at a temperature of 800°C to 1000°C.

[0049] The composite oxide prepared according to the method provided by the present invention contains 5 wt% to 21 wt% titanium dioxide, which is uniformly mixed with alumina. Furthermore, the inventors have surprisingly discovered that the surface microstructure of this composite oxide exhibits a coral-like 3D layered structure. This coral-like 3D layered structure allows the composite oxide to have a higher specific surface area, thereby possessing more active sites and a stronger electron-capturing capacity. This helps to promote the co-catalytic effect of TiO2 as an electron promoter, thus improving the overall performance of the catalyst, including its activity and selectivity.

[0050] Furthermore, it is generally believed that rutile formation begins at calcination temperatures of 500℃ for TiO2, and above 700℃, the majority of the crystalline phases of TiO2 transform from anatase to rutile. However, the composite oxide prepared by the method provided in this invention, after calcination at 800℃ or higher, shows, through X-ray diffraction analysis, that anatase-type titanium dioxide accounts for 95wt%-100wt% of all crystalline phases of TiO2, defying conventional wisdom. It is believed that in the composite oxide, TiO2 existing in the anatase form possesses an electron-inducing effect, effectively inducing a decrease in the electron cloud density of the active metal Ni in the prepared catalyst (compared to the rutile phase formed by high-temperature calcination), thereby enhancing the adsorption capacity for alkynes in the reactants and improving the selective hydrogenation activity and selectivity of the catalyst.

[0051] In a third aspect, the present invention also provides an application of the composite oxide, including the application of the composite oxide according to the first aspect of the present invention or the composite oxide prepared by the method according to the second aspect as a catalyst support.

[0052] According to the present invention, the type of catalyst is not particularly limited.

[0053] In some embodiments, the present invention provides a hydrogenation catalyst comprising a composite oxide according to the first aspect of the invention or a composite oxide prepared according to the second aspect of the invention, and an active component, such as palladium, nickel, iron, or cobalt.

[0054] According to some embodiments of the hydrogenation catalyst of the present invention, the hydrogenation metal is nickel. In some embodiments, the nickel content of the hydrogenation catalyst may be 8-25 wt%, preferably 12-20 wt%. In other embodiments, the hydrogenation catalyst contains palladium, the content of which may be 0.1-2 wt%, for example 0.15-1.5 wt%.

[0055] In a fourth aspect, the present invention also provides a method for selective hydrogenation of alkynes, the method comprising selectively hydrogenating a distillate oil in the presence of the hydrogenation catalyst described in the third aspect to increase butadiene production, wherein the distillate oil comprises C4 distillate oil, preferably high-alkyne tail gas byproduct of a butadiene extraction unit.

[0056] Furthermore, in the selective hydrogenation of alkynes, the reaction temperature is 20°C to 40°C, the molar ratio of hydrogen to alkynes is 1:1 to 2.5:1, the pressure is 0.5 MPa to 0.8 MPa, and the recycle ratio is 10:1 to 30:1.

[0057] The catalyst provided by this invention exhibits high vinylacetylene conversion and high 1,3-butadiene selectivity in the selective hydrogenation of alkynes. Brief description of the attached figures

[0058] Figure 1 The 3D microstructure of the coral reef prepared by the alumina-titanium dioxide composite oxide in Example 1 is shown.

[0059] Figure 2 The XRD pattern of the alumina-titanium dioxide composite oxide prepared in Example 1 is shown. Detailed Implementation

[0060] To facilitate understanding of the present invention, the present invention will be described in detail below with reference to embodiments. These embodiments are for illustrative purposes only and are not limited to the scope of application of the present invention.

[0061] Unless otherwise specified, all raw materials or components used in this invention can be obtained through commercial means or conventional methods.

[0062] The specific surface area and pore structure of the composite oxides were determined using an ASAP 2020 adsorption analyzer (N2 adsorption-desorption method) from Micron Instruments, Inc., USA. Before testing, the composite oxide samples were degassed at 623 K for 4 h, and nitrogen was adsorbed at liquid nitrogen temperature. Sample data were processed using AMSM software, and the specific surface area was obtained using the Brunauer-Emmet-Teller (BET) method. The average pore size was obtained from the nitrogen adsorption isotherm using the Barrett-Joyner-Halenda (BJH) method, and the pore volume was obtained using the P / Po single-point desorption curve.

[0063] The morphology of the composite oxide was observed using a QUANTA 200 scanning electron microscope from FEI.

[0064] The crystal structure of the composite oxide was characterized using an EMPYREAN X-ray diffractometer from Panaco GmbH, Netherlands. The radiation source was Cu Kα, with an X-ray tube voltage of 40 kV, a tube current of 40 mA, a slit width of 10 mm, a scanning range of 5–90°, and a scanning speed of 0.013° / s.

[0065] Example 1

[0066] 328.02 g of Al₂(SO₄)₃ was dissolved in deionized water to prepare 1000 mL of aluminum sulfate solution. 21.14 g of TiO(OH)₂ was dissolved in 16 mL of 98 wt% sulfuric acid solution, and deionized water was added to prepare 500 mL of dilute sulfuric acid solution containing metatitanic acid. 18 g of NH₄HCO₃ was dissolved in 600 mL of deionized water to prepare ammonium bicarbonate solution, and then 250 mL of 27 wt% ammonia solution was added. The mixture was stirred until homogeneous, and then deionized water was added to prepare 1000 mL of mixed alkali solution.

[0067] At atmospheric pressure and 55°C, 230 mL of the above-mentioned dilute sulfuric acid solution of metatitanic acid and 360 mL of mixed alkali solution were added concurrently to 1000 mL of the prepared aluminum sulfate solution, while maintaining vigorous stirring and keeping the pH of the mixed solution within the range of 3 to 4 for 15 min. Then, another 320 mL of mixed alkali solution was added to adjust the pH to 9 to 10, and the solution was held within this range for 15 min. Then, the remaining dilute sulfuric acid solution of the above-mentioned metatitanic acid was added to adjust the pH to 7.5 to 8.5, and the solution was held for 6 to 10 min. Then, the temperature was raised to 92°C and held for 20 min. The mixture was filtered, and the filter cake was washed five times with 20 times its volume of deionized water. The washed filter cake was dried at 110°C for 6 h and calcined at 850°C for 5 h. 114.3 g of a composite oxide with a TiO2 content of 15.0 wt% was obtained.

[0068] pass Figure 1SEM images show that the surface microstructure of the composite oxide exhibits a coral-like 3D layered structure. Figure 2 The XRD pattern of the alumina-titanium dioxide composite oxide prepared in Example 1 is shown. For titanium dioxide, the characteristic diffraction peak of anatase appears only at 2θ = 25.4°, and no diffraction peaks of other crystal phases appear at other positions, indicating that the TiO2 component in the composite oxide exists in the form of anatase crystal phase, that is, the anatase crystal phase of titanium dioxide accounts for 100 wt% of the total titanium dioxide.

[0069] Example 2

[0070] 256.04 g of Al₂(SO₄)₃ was dissolved in deionized water to prepare 1000 mL of aluminum sulfate solution. 32.15 g of Ti(SO₄)₂ was dissolved in deionized water, and 5 mL of 98% concentrated sulfuric acid was added to prepare 500 mL of titanium sulfate in dilute sulfuric acid solution. 18 g of NH₄HCO₃ was dissolved in 600 mL of deionized water to prepare ammonium bicarbonate solution, and then 250 mL of 27 wt% ammonia solution was added. The mixture was stirred until homogeneous, and then deionized water was added to prepare 1000 mL of mixed alkali solution.

[0071] At atmospheric pressure and 60°C, 280 mL of the above-mentioned titanium sulfate dilute sulfuric acid solution and 320 mL of mixed alkali solution were added concurrently to 1000 mL of aluminum sulfate solution, with vigorous stirring, maintaining the pH of the mixed solution within the range of 3 to 4 for 15 min. Then, 240 mL of mixed alkali solution was added to adjust the pH to 9 to 10, and held within this range for 15 min. Next, the remaining titanium sulfate dilute sulfuric acid solution was added, adjusting the pH to 7.5 to 8.5. The temperature was raised to 85°C and maintained for 40 min. The mixture was filtered, and the filter cake was washed five times repeatedly with 20 times its volume of deionized water. The washed filter cake was dried at 110°C for 6 h and calcined at 950°C for 5 h. 86.8 g of alumina-titanium dioxide composite oxide with a TiO2 content of 12.3% was obtained.

[0072] Example 3

[0073] The preparation process of the titanium dioxide-alumina composite oxide in Example 1 was repeated, except that 379.79g of Al(NO) was used. 3)3 A 1000 mL aluminum nitrate solution was prepared by dissolving the aluminum nitrate in deionized water. 25.99 g of Ti(OCH3CH2)4 was dissolved in anhydrous ethanol to prepare a 500 mL tetraethyl titanate ethanol solution. Finally, a 9.1% aluminum oxide-titanium dioxide composite oxide was obtained.

[0074] Example 4

[0075] The preparation process of the titanium dioxide-alumina composite oxide in Example 1 was repeated, except that 396.92 g of Al(NO3)3 was dissolved in deionized water to prepare 1000 mL of aluminum nitrate solution. 6.13 g of TiO(OH)2 was dissolved in sulfuric acid solution, and deionized water was added to prepare 500 mL of dilute sulfuric acid solution containing metatitanic acid. Finally, a 5.0% alumina-titanium dioxide composite oxide was obtained.

[0076] Example 5

[0077] The preparation process of the titanium dioxide-alumina composite oxide in Example 1 was repeated, except that 396.92 g of Al(NO3)3 was dissolved in deionized water to prepare 1000 mL of aluminum nitrate solution. 6.13 g of TiO(OH)2 was dissolved in sulfuric acid solution, and deionized water was added to prepare 500 mL of dilute sulfuric acid solution containing metatitanic acid. The filter cake calcination temperature was changed to 800 °C, finally yielding 5.0% alumina-titanium dioxide composite oxide.

[0078] Example 6

[0079] The preparation process of the titanium dioxide-alumina composite oxide in Example 1 was repeated, except that 374.13 g of AlCl3·6H2O was dissolved in deionized water to prepare 1000 mL of aluminum chloride solution. 59.99 g of Ti(OCH3CH2)4 was dissolved in anhydrous ethanol to prepare 500 mL of tetraethyl titanate ethanol solution. Finally, an alumina-titanium dioxide composite oxide with a content of 21.0% was obtained.

[0080] Scanning electron microscopy and XRD results show that the composite oxides prepared in Examples 2-6 are similar to those in Example 1, with a surface microstructure of coral cluster 3D layered structure, and the TiO2 component in the composite oxides exists in the form of anatase crystal phase.

[0081] Comparative Example 1

[0082] 268.46 g of Al2(SO4)3 was dissolved in deionized water to prepare 1000 mL of aluminum sulfate solution. 24.5 g of TiO(OH)2 was dissolved in sulfuric acid solution, and deionized water was added to prepare 1000 mL of dilute sulfuric acid solution containing metatitanic acid. 18 g of NH4HCO3 was dissolved in 600 mL of deionized water to prepare ammonium bicarbonate solution, then 250 mL of 24-28 wt% ammonia solution was added, stirred until well mixed, and deionized water was added to prepare 1000 mL of mixed alkali solution.

[0083] Under normal pressure and at a temperature of 70-75℃, the above-mentioned three solutions—a deionized aqueous solution of aluminum sulfate, a dilute sulfuric acid solution of metatitanic acid, and a mixed alkaline solution—were co-precipitated in parallel flow. The flow rate of the mixed alkaline solution was controlled to maintain the pH of the precipitate within the range of 5.0-6.0 for 8 minutes. Then, the flow rate of the mixed alkaline solution was increased to maintain the pH of the mixed solution within the range of 8.5-9.5 for 8 minutes. Next, the flow rate of the mixed alkaline solution was decreased to maintain the pH of the mixed solution within the range of 5.0-6.0 for 8 minutes. The flow rate of the mixed alkaline solution was then increased again to maintain the pH of the precipitate within the range of 8.5-9.5. This process was repeated until all solutions A1 and B1 were added. The reaction solution was allowed to stand at 70℃ for 30 minutes, filtered, and the filter cake was washed with 15 times its volume of deionized water for 30 minutes. This process was repeated four times. Finally, the filter cake was dried at 100-120℃ for 8-12 hours and calcined at 950℃ for 5 hours to obtain the titanium dioxide-alumina composite. Its structure and properties are shown in Table 1.

[0084] Comparative Example 2

[0085] Take 401.88g of analytically pure AlCl3·6H2O and dissolve it in 1000ml of deionized water to prepare solution A1; take 43.25g of chemically pure Ti(OCH2CH3)4 and dissolve it in 500ml of benzene (benzene content is 99.8(wt)%) to prepare solution B1; take 18g of analytically pure NH4HCO3 and dissolve it in 600ml of deionized water, add 250ml of ammonia water with a concentration of 24-28wt%, stir and mix evenly, and then add deionized water to prepare 1000ml of solution C1.

[0086] Under normal pressure and at a temperature of 70-75℃, solutions A1, B1, and C1 were co-precipitated by parallel flow. The flow rate of solution C1 was controlled to maintain the pH of the precipitate in the range of 5.0-6.0 for 8 minutes. Then, the flow rate of solution C1 was increased to maintain the pH of the mixed solution in the range of 8.5-9.5 for 8 minutes. Then, the flow rate of solution C1 was decreased to maintain the pH of the mixed solution in the range of 5.0-6.0 for 8 minutes. Then, the flow rate of solution C1 was increased again to maintain the pH of the precipitate in the range of 8.5-9.5. This process was repeated until all solutions A1 and B1 were added. The reaction solution was allowed to stand at 70℃ for 30 minutes, filtered, and the filter cake was washed with 15 times the volume of deionized water for 30 minutes. This process was repeated four times. Finally, the filter cake was dried at 100-120℃ for 8-12 hours and calcined at 550℃ for 5 hours to obtain 42.7g of titanium dioxide-alumina composite. The results of its structure and performance are shown in Table 1.

[0087] Comparative Example 3

[0088] The preparation process of the titanium dioxide-alumina composite oxide in Comparative Example 2 was repeated, except that the calcination temperature after drying was changed to 950℃.

[0089] Scanning electron microscopy and XRD results show that the composite oxides prepared in Comparative Examples 1-3 do not have a coral cluster 3D layered structure, and the TiO2 crystal phase is mainly rutile titanium dioxide.

[0090] The specific surface area and pore structure of the composite oxide were determined using the N2 adsorption-desorption method on the carrier prepared above.

[0091] Table 1. Analytical data of titanium dioxide-alumina composites

[0092]

[0093]

[0094] Table 2 Pore distribution of the titanium dioxide-alumina composite support

[0095] The proportion of pores with a diameter in the range of 10-20 nm to all pores, by volume Example 1 86% Example 2 88% Example 3 89% Example 4 90% Example 5 85% Example 6 85% Comparative Example 1 78% Comparative Example 2 34% Comparative Example 3 82%

[0096] Catalyst preparation

[0097] Example 7

[0098] Take 100 mL of 24.72 g Ni / 100 mL of nickel nitrate aqueous solution to impregnate 156 g of the composite oxide prepared in Example 1 above for 1 h, dry at 110 °C for 6 h, filter dry and calcine at 600 °C for 4 h to obtain Ni / Al2O3-TiO2 catalyst A with Ni content of 13.68%.

[0099] Example 8

[0100] 180g of the composite oxide prepared in Example 1 was impregnated with 100mL of a 20.0g Ni / 100mL nickel nitrate aqueous solution for 0.5h. After filtration, it was dried at 110℃ for 5h and calcined at 550℃ for 5h. Then, 100g of the calcined catalyst precursor was impregnated with 100mL of a 12.24g Ni / 100mL nickel nitrate aqueous solution for 0.5h. After filtration, it was dried at 110℃ for 4h and calcined at 550℃ for 6h to obtain Ni / Al2O3-TiO2 catalyst B with a Ni content of 19.82%.

[0101] Example 9

[0102] Take 100 mL of 13.56 g Ni / 100 mL of nickel nitrate aqueous solution and impregnate 156 g of the composite oxide prepared in Example 6 above for 1 h. Dry at 110 °C for 6 h, filter dry and calcine at 600 °C for 4 h to obtain Ni / Al2O3-TiO2 catalyst C with 8% Ni content.

[0103] Example 10

[0104] 180g of the composite oxide prepared in Example 4 was impregnated with 100mL of a 20.0g Ni / 100mL nickel nitrate aqueous solution for 0.5h. After filtration, it was dried at 110℃ for 5h and calcined at 550℃ for 5h. Then, 100g of the calcined catalyst precursor was impregnated with 100mL of a 20g Ni / 100mL nickel nitrate aqueous solution for 0.5h. After filtration, it was dried at 110℃ for 4h and calcined at 550℃ for 6h to obtain Ni / Al2O3-TiO2 catalyst D with a Ni content of 25%.

[0105] Example 11

[0106] 180g of the composite oxide prepared in Example 2 was impregnated with 100mL of a 20.0g Ni / 100mL nickel nitrate aqueous solution for 0.5h. After filtration, it was dried at 110℃ for 5h and calcined at 550℃ for 5h. Then, 100g of the calcined catalyst precursor was impregnated with 100mL of a 12.24g Ni / 100mL nickel nitrate aqueous solution for 0.5h. After filtration, it was dried at 110℃ for 4h and calcined at 550℃ for 6h to obtain Ni / Al2O3-TiO2 catalyst E with a Ni content of 19.82%.

[0107] Example 12

[0108] 180g of the composite oxide prepared in Example 3 was impregnated with 100mL of a 20.0g Ni / 100mL nickel nitrate aqueous solution for 0.5h. After filtration, it was dried at 110℃ for 5h and calcined at 550℃ for 5h. Then, 100g of the calcined catalyst precursor was impregnated with 100mL of a 12.24g Ni / 100mL nickel nitrate aqueous solution for 0.5h. After filtration, it was dried at 110℃ for 4h and calcined at 550℃ for 6h to obtain Ni / Al2O3-TiO2 catalyst F with a Ni content of 19.82%.

[0109] Example 13

[0110] Take 100 mL of 24.72 g Ni / 100 mL of nickel nitrate aqueous solution to impregnate 156 g of the composite oxide prepared in Example 5 above for 1 h, dry at 110 °C for 6 h, filter dry and calcine at 600 °C for 4 h to obtain Ni / Al2O3-TiO2 catalyst G with Ni content of 13.68%.

[0111] Example 14

[0112] 100g of the composite oxide prepared in Example 1 was immersed in 85mL of an aqueous solution of palladium chloride with a palladium atomic content of 0.32g / 100mL. After 1.5 hours, it was removed, the impregnated composite support was filtered out, and it was reduced with 120mL of 10wt% hydrazine hydrate aqueous solution at room temperature for 1 hour. It was then repeatedly rinsed with deionized water until chloride ions were removed. After draining the water, it was dried at 120°C for 6 hours and then calcined at 480°C for 4 hours to obtain a Pd / Al2O3-TiO2 catalyst H with a palladium content of 0.3% and a Pd content of 0.3%.

[0113] Comparative Example 4

[0114] Take 100 mL of 24.72 g Ni / 100 mL of nickel nitrate aqueous solution and impregnate 156 g of the composite oxide prepared in Comparative Example 1 above for 1 h. After filtration, dry at 110 °C for 6 h and calcine at 600 °C for 4 h to obtain Ni / Al2O3-TiO2 catalyst I with Ni content of 13.68%.

[0115] Comparative Example 5

[0116] Take 100 mL of 24.72 g Ni / 100 mL of nickel nitrate aqueous solution and impregnate 156 g of the above-prepared composite oxide in Comparative Example 2 for 1 h. After filtration, dry at 110 °C for 6 h and calcine at 600 °C for 4 h to obtain Ni / Al2O3-TiO2 catalyst J with Ni content of 13.68%.

[0117] Comparative Example 6

[0118] Take 100 mL of 24.72Ni / 100 mL nickel nitrate aqueous solution and impregnate 156 g of the above-prepared composite oxide in Comparative Example 3 for 1 h. After filtration, dry at 110 °C for 6 h and calcine at 600 °C for 4 h to obtain Ni / Al2O3-TiO2 catalyst K with Ni content of 13.68%.

[0119] Example 15

[0120] This embodiment demonstrates the application of a catalyst in the selective hydrogenation reaction of butadiene extraction tail gas.

[0121] The catalyst used in this embodiment is catalyst AK.

[0122] The raw material used in this embodiment is butadiene extraction tail gas from a certain factory. The composition is shown in Table 3.

[0123] Table 3. Composition of butadiene extraction tail gas from a certain factory.

[0124]

[0125]

[0126] In this embodiment, a fixed-bed pilot-scale evaluation device from Tuochuan Scientific Equipment Co., Ltd. was used, with 50 mL of catalyst loaded, to carry out a selective hydrogenation reaction of butadiene extraction tail gas.

[0127] Reaction conditions: reaction pressure 0.5 to 0.7 MPa, hydrogen flow rate 1.92 L / h, reactor inlet temperature 25℃, recycle ratio 20:1, feed rate 25 mL / h.

[0128] Catalyst AK was evaluated under the same conditions, and the results of hydrogenation and alkyne removal are shown in Table 4.

[0129] Table 4 Results of selective hydrogenation of butadiene extraction tail gas

[0130]

[0131] **1,3-Butadiene Selectivity = (1,3-Butadiene in Product - 1,3-Butadiene in Feed) / (Vinylacetylene in Feed - Vinylacetylene in Product)**

[0132] As can be seen from the table above, the catalyst provided by this invention exhibits a high conversion rate of vinylacetylene and a high selectivity for 1,3-butadiene. Because the vinylacetylene in the hydrogenation product can be controlled within a low range, the hydrogenation product can be directly returned to the extraction system to achieve increased butadiene production.

[0133] Example 16

[0134] Catalyst A prepared in Example 7 was subjected to long-term stability experiments under the same conditions as in Example 15. The stability evaluation experimental data after 1000 h are shown in Table 5 below:

[0135] Table 5

[0136]

[0137] As shown in Table 5, the catalyst provided by this invention exhibits high stability in the selective hydrogenation reaction of butadiene tail gas feedstock with high alkyne content. The hydrogenation catalyst of this invention not only possesses high 1,3-butadiene selectivity (%) and vinylacetylene conversion (%), but also maintains high levels for extended periods, thus making it suitable for long-term operation.

[0138] It should be noted that the embodiments described above are only for explaining the present invention and do not constitute any limitation on the present invention. The present invention has been described with reference to typical embodiments, but it should be understood that the words used therein are descriptive and explanatory terms, not limiting terms. Modifications can be made to the present invention within the scope of the claims, and revisions can be made to the present invention without departing from the scope and spirit of the present invention. Although the present invention described herein relates to specific methods, materials, and embodiments, it does not mean that the present invention is limited to the specific examples disclosed herein; on the contrary, the present invention can be extended to all other methods and applications with the same function.

Claims

1. A composite oxide comprising 60-95 wt% alumina and 5-40 wt% titanium dioxide, wherein the specific surface area of ​​the composite oxide, as determined by the BET method, is expressed as X m. 2 / g, the average pore size of the composite oxide, as determined by the nitrogen adsorption isotherm method, is expressed as Y nm, where the ratio of X to Y is 5 to 15, and as determined by X-ray diffraction, the anatase phase titanium dioxide in the composite oxide accounts for 95wt%-100wt% of the total titanium dioxide, where X is in the range of 50-200 nm and Y is in the range of 9-20 nm.

2. The composite oxide according to claim 1, wherein X is in the range of 60-180.

3. The composite oxide according to claim 1, wherein X is in the range of 80-150.

4. The composite oxide according to claim 1, characterized in that, The pore volume of the composite oxide is expressed as Z mL / g, where Z is in the range of 0.3 to 0.5, and where the ratio of X to Z is 220 to 400.

5. The composite oxide according to claim 4, wherein the ratio of X to Z is 250 to 350.

6. The composite oxide according to any one of claims 1-5, having at least one of the following characteristics: - X is between 90 and 150; - At least 85% of the pores by volume have a pore size in the range of 10-20 nm. -Z is between 0.3 and 0.4; - The composite oxide contains 5 wt% to 21 wt% titanium dioxide; and - The composite oxide has a coral-like 3D layered structure.

7. The composite oxide according to any one of claims 1-5, wherein Y is 12 to 16.

8. A method for preparing a composite oxide according to any one of claims 1-7, comprising the following steps: Step I. Dissolve the soluble aluminum source in water to form an aluminum source solution, dissolve the titanium source in an acid solution to form a titanium source solution, and mix the ammonium salt and the alkaline solution to form a mixed alkaline solution; Step II. (a) Add the titanium source solution and the mixed alkaline solution to the aluminum source solution, so that the resulting mixture is maintained at a first pH value for a first time period; (b) Add an additional amount of the mixed alkaline solution to the mixture, so that the resulting mixture is maintained at a second pH value for a second time period; (c) Add an additional amount of titanium salt solution to the mixture, so that the resulting mixture is maintained at a third pH value for a third time period. Step III. After step II.(c), the temperature of the mixture is raised and maintained for a fourth time period to obtain a precipitate; Step IV. The precipitate is dried and calcined to obtain a composite oxide containing alumina and titanium dioxide.

9. The method of claim 8, wherein in step IV, washing and filtration are further performed prior to drying.

10. The method according to claim 8, characterized in that, In step II, the first pH value is less than 5, the second pH value is greater than 8.5, and the third pH value is greater than 7 and less than 9.

11. The method according to claim 8, characterized in that, In step II, the first pH value is 3 to 4, the second pH value is 9 to 10, and the third pH value is 7.5 to 8.

5.

12. The method according to claim 8, characterized in that, The first, second, and third time periods are each 5 to 20 minutes; and / or The fourth time period is from 20 to 60 minutes.

13. The method according to claim 8, wherein the first time period, the second time period, and the third time period are each 10 minutes to 15 minutes.

14. The method according to any one of claims 8-13, characterized in that, In step II, the operating temperature is 25°C to 60°C; and / or in step III, the temperature is increased to 80°C to 150°C; and / or in step IV, the drying temperature is 110°C to 130°C; and / or the calcination temperature is 800°C to 1000°C.

15. The use of a composite oxide according to any one of claims 1-7 or a composite oxide prepared by any one of claims 8-14 as a catalyst support.

16. A hydrogenation catalyst comprising a composite oxide according to any one of claims 1-7 or a composite oxide prepared by the method according to any one of claims 8-14 and an active component.

17. The hydrogenation catalyst of claim 16, wherein the active component is nickel.

18. The hydrogenation catalyst of claim 17, wherein the nickel content in the catalyst is 8-25 wt%.

19. The hydrogenation catalyst of claim 18, wherein the nickel content in the catalyst is 12-20 wt%.

20. A method for selective hydrogenation of alkynes, comprising selectively hydrogenating a distillate oil in the presence of a hydrogenation catalyst according to any one of claims 16-19 to increase butadiene production, wherein the distillate oil comprises a C4 distillate oil.

21. The selective hydrogenation method for alkynes according to claim 20, wherein the distillate oil comprises high-alkyne tail gas produced as a byproduct of a butadiene extraction unit.

22. The selective hydrogenation method for alkynes according to claim 20, wherein during the selective hydrogenation of alkynes, the reaction temperature is 20°C to 40°C, the molar ratio of hydrogen to alkynes is 1:1 to 2.5:1, the pressure is 0.5 MPa to 0.8 MPa, and the recycle ratio is 10:1 to 30:1.

Citation Information

Patent Citations

  • Catalyst for selective hydrogenation of petroleum hydrocarbon and preparation method and application thereof

    CN101856613A

  • C4 alkyne selective hydrogenation catalyst and preparation method and application thereof

    CN102886262A

  • Titanium oxide-aluminum oxide compound as well as preparation method and application thereof

    CN103721693A

  • Composite oxide carrier, hydrofining catalyst as well as preparation method and application thereof

    CN113828289A

  • Titanium oxide - aluminum oxide composite carrier, preparation method and application thereof

    CN1689702A