A high temperature resistant low compression set hydrogenated nitrile rubber

By modifying carbon black and glass flakes, the interaction and heat resistance of hydrogenated nitrile butadiene rubber are enhanced, solving the problems of low compression set and aging resistance at high temperatures, while maintaining the sealing performance at high temperatures and low temperatures.

CN116804097BActive Publication Date: 2026-11-20NANJING UNIV +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310886531.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-19
Publication Date
2026-11-20
Estimated Expiration
2043-07-19

Smart Images

  • Figure BDA0004346488260000051
    Figure BDA0004346488260000051
  • Figure BDA0004346488260000061
    Figure BDA0004346488260000061
Patent Text Reader

Abstract

A kind of high-temperature-resistant low compression permanent deformation hydrogenated nitrile rubber, the raw materials used include hydrogenated nitrile rubber 90-100 parts, modified carbon black 30-60 parts, modified glass flake 5-20 parts, plasticizer 0.5-10 parts, white carbon black 1-20 parts, antioxidant 1-3 parts, peroxide vulcanizing agent 3-8 parts, oxide 3-10 parts, stearic acid 0.5-2 parts and vulcanizing agent 0.1-3 parts, wherein the carbon black and glass flake are surface modified by silane coupling agent compounded of γ-methacryloyloxypropyltrimethoxysilane and isooctyl acrylate modified γ-aminopropylmethyldiethoxysilane.The prepared hydrogenated nitrile rubber has the characteristics of high-temperature-resistant aging and low compression permanent deformation, and is a high-performance high-temperature-resistant sealing material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of rubber technology, and more specifically to a high-temperature resistant, low-compression-deformation hydrogenated nitrile butadiene rubber. Background Technology

[0002] Hydrogenated nitrile butadiene rubber (HNBR) is a highly saturated polymer made by hydrogenating nitrile butadiene rubber. It has high elasticity, heat aging resistance and chemical resistance, as well as high strength, high tear resistance and excellent wear resistance. It can be widely used in automobiles, oil fields, aviation, wind power and other fields.

[0003] Depending on the application environment, researchers have designed various hydrogenated nitrile butadiene rubber (NBR) formulations to focus on improving certain performance aspects. Patent application CN114369298A discloses a low-temperature, low-pressure variable hydrogenated NBR for wind power applications. The raw materials include 100 parts hydrogenated NBR raw rubber, 30-50 parts filler, 10-30 parts plasticizer, 1-5 parts antioxidant, 1-10 parts vulcanizing agent, 1-10 parts accelerator, and 1-20 parts kaolin. The kaolin, activated with water glass and stearic acid or a coupling agent, is used to improve the tensile strength of the rubber compound, reduce heat generation and compression set, thus meeting the sealing requirements of wind power equipment in harsh climatic environments. Invention patent application CN110591191A discloses a hydrogenated nitrile butadiene rubber for automotive sealing rings and its preparation method. The rubber sealing ring is used in electric motors in automobiles. The raw materials include 90-105 parts of hydrogenated nitrile butadiene rubber, 17-23 parts of silica, 45-55 parts of silica VM56, 1-3 parts of vinyltris(β-methoxyethoxy)silane, 4-6 parts of zinc oxide, 8-11 parts of di-tert-butyl peroxide, 13-17 parts of dioctyl sebacate, 0.5-2 parts of stearic acid, 0.5-3 parts of antioxidant, and 2-4 parts of additives. The tensile strength of the material is approximately 15 MPa. Invention patent application CN112321921A discloses a rubber composition for automotive air conditioning pipes and its preparation method. The rubber composition comprises the following raw material components in parts by weight: 80-90 parts of hydrogenated nitrile rubber, 10-20 parts of poly(terephthalamide) nonadiamine, 2-4 parts of antioxidant, 7-12 parts of heat resistant agent, 20-40 parts of carbon black, 102-202 parts of permeation barrier agent, 10-30 parts of damping agent, 10-15 parts of peroxide crosslinking agent, and 3-6 parts of co-crosslinking agent. The permeation barrier agent includes graphene and DK2 polymer-grade organic clay. Preferred heat resistant agents include cerium oxide and lithium carbonate. The rubber composition has good heat resistance life and resistance to carbon dioxide permeation.

[0004] Refrigerant R744, based on carbon dioxide, has broad application prospects in air conditioning systems due to its environmental friendliness, wide availability, low cost, and safety / non-toxicity. However, because carbon dioxide has a high critical temperature, compressors using R744 refrigerant generate very high pressures (up to 15 MPa or more), temperatures, and suction / discharge pressure differences, with temperatures potentially reaching 165-180°C. This presents a significant challenge to the design and manufacture of elastic sealing rings for air conditioning system piping. These rings must not only withstand aging at 165-180°C but also exhibit low compression set at these temperatures to maintain compressive stress and ensure airtightness. Existing materials based on HNBR technology sometimes have low tensile strength, making them unable to withstand the bursting effect of carbon dioxide gas penetration. Other materials struggle to simultaneously achieve both high-temperature resistance and low compression set. Furthermore, after high-temperature operation, plasticizer migration from the surface reduces the sealing ring's low-temperature performance. Summary of the Invention

[0005] To solve the above-mentioned technical problems, the present invention provides a high-temperature resistant, low-compression-per-shape hydrogenated nitrile butadiene rubber, wherein the raw materials used, by weight, include 90-100 parts of hydrogenated nitrile butadiene raw rubber, 30-60 parts of modified carbon black, 5-20 parts of modified glass flakes, 0.5-10 parts of plasticizer, 1-20 parts of silica, 1-3 parts of antioxidant, 3-8 parts of peroxide vulcanizing agent, 3-10 parts of oxide, 0.5-2 parts of stearic acid, and 0.1-3 parts of co-vulcanizing agent.

[0006] Preferably, the hydrogenated nitrile butadiene rubber has a bound acrylonitrile content of 34-44% and an unsaturation degree of 4%-8%.

[0007] Preferably, the oxide is one or a mixture of zinc oxide and magnesium oxide.

[0008] Preferably, the peroxide sulfiding agent is 2,4-di-tert-butyl peroxide cumene.

[0009] Preferably, the plasticizer is trioctyl trimellitate.

[0010] Preferably, the vulcanizing agent is one or a mixture of two of diphenylmethane bismaleimide and N,N′-m-phenylene bismaleimide.

[0011] Preferably, the antioxidant is one or a mixture of two of 2,2,4-trimethyl-1,2-dihydroquinoline polymer (antioxidant RD) and 4,4′-bis(phenylisopropyl)diphenylamine (antioxidant 445).

[0012] The modified carbon black is prepared by surface modification of one or a mixture of two or more of the grades 330 carbon black, 550 carbon black and 774 carbon black through a compounded silane coupling agent.

[0013] The modified glass flakes, preferably with a particle size of 400-2000 mesh, are prepared by surface modification with a compounded silane coupling agent.

[0014] The compounded silane coupling agent, by weight, is composed of 40-80 parts of γ-methacryloyloxypropyltrimethoxysilane (KH570) and 20-60 parts of isooctyl acrylate-modified γ-aminopropylmethyldiethoxysilane (Si-902).

[0015] The preparation steps of the compounded silane coupling agent are as follows: Under the condition of excluding water vapor, 1.5-2 moles of isooctyl acrylate and 1 mole of Si-902 coupling agent are mixed, and the double bond in isooctyl acrylate is added to the amino group in Si-902 coupling agent to form an addition reaction. The reaction is carried out at room temperature for 1-2 hours, and then heated at 60-80°C for 1 hour. After cooling, a certain amount of KH570 coupling agent is added to the above product, and the mixture is mixed to obtain the compounded silane coupling agent.

[0016] The method for modifying the filler with the compounded silane coupling agent is as follows: Weigh 0.5% to 5% of the compounded silane coupling agent by weight of the filler, prepare a 5% ethanol solution, add it dropwise to the filler, stir and mix during addition, let it stand at room temperature for 3 to 5 hours, dry it at 80°C for 1 to 3 hours, and cool it for later use.

[0017] The present invention discloses a method for preparing high-temperature resistant, low-compression-permanent hydrogenated nitrile butadiene rubber, comprising the following steps: Step 1, mixing in an internal mixer: Weigh all raw materials (except peroxide) and add them to an internal mixer, mixing at room temperature for 10-15 minutes; Step 2, adding peroxide to a two-roll mill: Add the rubber compound prepared in Step 1 to a two-roll mill with a roll gap of 2-3 mm, and after passing the rubber compound through the rolls twice, add the peroxide by wrapping the rolls. After adding the material, pass the compound through a thin mill 4-6 times to obtain the mixed rubber; Step 3, vulcanization: Vulcanization conditions are 160-170℃ for 10-20 minutes, and after removal, vulcanize again in a 170℃ oven for 60-120 minutes.

[0018] Invention Principle: Through repeated research and verification, the inventors discovered that the mechanical properties of HNBR materials decrease and compression set increases after high-temperature thermal aging. One of the main reasons for this is the weakened interaction between the rubber molecular chains in HNBR and reinforcing fillers such as carbon black after prolonged high temperatures. The principle of this invention is as follows: 1) Surface modification of the filler: The compounded coupling agent contains double bonds (derived from KH570 coupling agent) and branched alkane long chains (derived from isooctyl acrylate modified Si-902 coupling agent). The double bonds are grafted onto the rubber backbone via free radical polymerization after oxide decomposition, and the branched alkane long chains entangle with the rubber backbone, thus enhancing the interaction between the filler and the HNBR backbone rubber from two aspects, reducing their dissociation at high temperatures, thereby improving the high-temperature thermal aging resistance of HNBR and reducing compression set. 2) The flaky glass flakes also prevent the HNBR molecular chains from slipping and isolate oxygen, further contributing to improved heat aging resistance and reduced compression set. 3) Furthermore, the branched alkane long chains grafted onto the filler have a long-term plasticizing effect, which can avoid the surface migration and precipitation of general plasticizers under long-term high temperatures, and is conducive to maintaining the low-temperature glass transition temperature of the material, that is, maintaining low-temperature resistance. 4) In addition, if KH570 is used alone to modify the filler, the introduction of double bonds will lead to a significant increase in the degree of crosslinking of the vulcanized rubber, thereby causing an increase in the hardness of the material. When combined with the Si-902 coupling agent modified with isooctyl acrylate, the plasticizing effect of the branched alkane long chains buffers the increase in hardness caused by the addition of KH570.

[0019] Beneficial effects: The invented hydrogenated nitrile butadiene rubber (NBR) possesses the advantages of both high-temperature aging resistance and low compression set. After heat aging in air at 180°C for 72 hours, the tensile strength retention rate of the hydrogenated NBR can reach 90% or higher, while the compression set is reduced to below 25%. The material maintains its glass transition temperature at low temperatures after heat aging, making it suitable as a high-temperature sealing material for air conditioning ducts, meeting the environmental requirements for refrigerant R744. Detailed Implementation

[0020] Example 1

[0021] A high-temperature resistant, low-compression-per-weight hydrogenated nitrile butadiene rubber, comprising the following raw materials by weight: 100 parts hydrogenated nitrile butadiene raw rubber, 20 parts modified 774 carbon black, 25 parts modified 550 carbon black, 10 parts modified glass flakes, 2 parts trioctyl trimellitate, 10 parts silica, 2 parts 4,4′-bis(phenylisopropyl)diphenylamine antioxidant, 5 parts 2,4-di-tert-butyl peroxide isopropylbenzene, 5 parts magnesium oxide, 1 part stearic acid, and 1 part N,N′-m-phenylenebismaleimide.

[0022] The hydrogenated nitrile butadiene rubber has a bound acrylonitrile content of 34%.

[0023] The modified 774 carbon black, modified 550 carbon black, and modified glass flakes are prepared by modification with a compounded silane coupling agent, wherein the compounded silane coupling agent, by weight, consists of 70 parts of γ-methacryloyloxypropyltrimethoxysilane (KH570) and 30 parts of isooctyl acrylate-modified γ-aminopropylmethyldiethoxysilane (Si-902).

[0024] The preparation steps of the compounded silane coupling agent are as follows: Under the condition of excluding water vapor, 2 moles of isooctyl acrylate and 1 mole of Si-902 coupling agent are mixed and reacted at room temperature for 2 hours, and then reacted at 80°C for 1 hour; after cooling, 2.33 times the weight of KH570 coupling agent is added to the above product and mixed to obtain the compounded silane coupling agent.

[0025] The method for modifying the filler with the compounded silane coupling agent is as follows: Weigh 1.5% of the compounded silane coupling agent by weight of the filler, prepare a 5% ethanol solution, add it dropwise to the filler, mix quickly, let it stand at room temperature for 3 hours, then continue to dry at 80°C for 3 hours, and cool before use.

[0026] Hydrogenated nitrile butadiene rubber was prepared according to the following vulcanization steps: Step 1, mixing in an internal mixer: except for the peroxide, all other raw materials were put into the internal mixer and mixed at room temperature for 10 minutes; Step 2, adding peroxide to a two-roll mill: the rubber compound prepared in Step 1 was put into a two-roll mill with a roll gap of 2 mm. After the rubber compound passed through the rolls twice, the peroxide was added around the rolls. After adding the material, it was passed through the mill five times to prepare the compound; Step 3, vulcanization: the vulcanization conditions were 170℃ for 15 minutes, and after taking it out, it was vulcanized a second time in a 170℃ oven for 120 minutes.

[0027] Example 2

[0028] A high-temperature resistant, low-compression-per-shape hydrogenated nitrile butadiene rubber, comprising the following raw materials by weight: 100 parts hydrogenated nitrile butadiene raw rubber, 20 parts modified 774 carbon black, 20 parts modified 550 carbon black, 10 parts modified glass flakes, 2 parts trioctyl trimellitate, 12 parts silica, 2 parts antioxidant RD, 5 parts 2,4-di-tert-butyl peroxide, 5 parts zinc oxide, 1 part stearic acid, and 1 part diphenylmethane bismaleimide.

[0029] The modified 774 carbon black, modified 550 carbon black, and modified glass flakes are prepared by modification with a compounded silane coupling agent, wherein the compounded silane coupling agent, by weight, consists of 75 parts KH570 and 25 parts isooctyl acrylate-modified γ-aminopropylmethyldiethoxysilane.

[0030] The preparation of the compounded silane coupling agent, the method of modifying the filler, and the vulcanization steps are the same as in Example 1.

[0031] Comparative Example

[0032] A hydrogenated nitrile butadiene rubber, the raw materials used by weight include 100 parts of hydrogenated nitrile butadiene raw rubber, 20 parts of 774 carbon black, 25 parts of 550 carbon black, 10 parts of glass flakes, 2 parts of trioctyl trimellitate, 10 parts of silica, 2 parts of 4,4′-bis(phenylisopropyl)diphenylamine antioxidant, 5 parts of 2,4-di-tert-butyl peroxide isopropylbenzene, 5 parts of magnesium oxide, 1 part of stearic acid, and 1 part of N,N′-m-phenylenebismaleimide.

[0033] The difference between the comparative example and the embodiment is that the carbon black and glass flakes were not modified with a compounded coupling agent, while the other processes such as mixing, open milling and vulcanization are the same.

[0034] Table 1 shows the test results of high-temperature aging resistance and compression set of the examples and comparative examples.

[0035]

[0036]

[0037] Further citing relevant data from embodiments in the background patent literature: In invention patent application CN11059119lA, the tensile strength of Examples 1-3 was 14.6 MPa to 15.2 MPa. In invention patent application CN114369298A, the tensile strength of Examples 1-4 was 12 MPa, and the average compressive settling after aging at 150°C for 72 hours was 35%. In invention patent application CN112321921A, the initial tensile strengths of Examples 1-4 were 18.5 MPa, 16.5 MPa, 17.1 MPa, and 19.8 MPa, respectively; the changes in tensile strength after aging at 180°C for 70 hours were -13.8%, -15.2%, -9.9%, and -10.4%, respectively; and the changes in elongation at break were -35.4%, -31.7%, -34.5%, and -41.7%, respectively.

[0038] Compared with literature and comparative data, the hydrogenated nitrile rubber of the present invention exhibits excellent comprehensive properties: (1) high bulk tensile strength, with an initial strength greater than 20 MPa. (2) excellent high-temperature aging resistance. In this embodiment, after aging at 180°C for 72 hours, the tensile strength change rates were -5.6% and -2.9%, and the elongation at break change rates were -24.3% and -20.9%, respectively, which are better than the tensile strength change rates of -9.9% to -15.2% and the elongation at break change rates of -31.7% to -41.7% in the literature. (3) maintaining low compression set at high temperatures. In this embodiment, after aging at 150°C for 72 hours, the compression set were 12.9% and 12.4%, respectively, which are better than the 35% in the literature. Even after aging at 180°C for 72 hours, the compression set of this embodiment remained as low as 18.1% and 19.1%. In addition, after high-temperature aging, the low-temperature glass transition temperature Tg of the material remained unchanged.

[0039] The specific embodiments described in this invention are merely preferred embodiments and are not intended to limit the scope of the invention. All equivalent changes and modifications made within the scope of the claims of this invention should be considered within the technical scope of this invention.

Claims

1. A high-temperature resistant, low-compression-per-weight hydrogenated nitrile butadiene rubber, comprising, by weight, 90-100 parts of hydrogenated nitrile butadiene raw rubber, 0.5-10 parts of plasticizer, 1-20 parts of silica, 1-3 parts of antioxidant, 3-8 parts of peroxide vulcanizing agent, 3-10 parts of oxide, 0.5-2 parts of stearic acid, and 0.1-3 parts of co-vulcanizing agent, characterized in that... It also includes 30-60 parts of modified carbon black and 5-20 parts of modified glass flakes; wherein, the modified carbon black and modified glass flakes are prepared by surface modification with a compounded silane coupling agent at 0.5%-5% of the weight of carbon black and glass flakes; the compounded silane coupling agent is composed of 40-80 parts of γ-methacryloyloxypropyltrimethoxysilane and 20-60 parts of isooctyl acrylate-modified γ-aminopropylmethyldiethoxysilane; the isooctyl acrylate-modified γ-aminopropylmethyldiethoxysilane is prepared by reacting 1.5-2 moles of isooctyl acrylate with 1 mole of γ-aminopropylmethyldiethoxysilane.

Citation Information

Patent Citations

  • Hydrogenated butadiene-acrylonitrile rubber for automobile sealing ring and preparation method thereof

    CN110591191A

  • Rubber composition for automobile air conditioner pipe and preparation method thereof

    CN112321921A

  • Low-temperature-resistant and low-pressure-change hydrogenated butadiene-acrylonitrile rubber for wind power and preparation method thereof

    CN114369298A

  • Refrigerant-resistant HNBR sealing element and preparation method thereof