Method for preparing a12o3 passivation layer, structure and method for testing moisture resistance
By using ALD technology to prepare Al₂O₃ passivation layers, the adhesion and compactness issues of existing passivation layer materials in semiconductor devices are solved, improving the moisture resistance and luminous efficiency of LED chips and achieving better photoelectric performance.
Patent Information
- Application Number
- CN202310371298.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-10
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-04-10
AI Technical Summary
Existing SiO₂, Si₃N₄ and SiON passivation layer materials have problems such as poor adhesion, low density, high surface charge, unsatisfactory refractive index and insufficient protection in semiconductor devices, which affect the chip's moisture resistance and light emission effect.
An Al₂O₃ passivation layer was prepared using ALD technology. A dense Al₂O₃ film was formed by controlling the pulsed chemisorption reaction of TMA vapor and water vapor. A SiO₂ passivation layer was then coated on the surface of the LED chip to form a moisture resistance test structure.
The Al₂O₃ passivation layer improves the moisture resistance and luminous efficiency of LED chips. It has good adhesion and density, which is better than that of SiO₂ passivation layer, and can maintain good photoelectric performance in high temperature and high humidity environments.
Smart Images

Figure CN116805661B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of semiconductor device technology, specifically to a method for preparing an Al2O3 passivation layer, and a structure and method for testing its moisture resistance. Background Technology
[0002] Common passivation materials include SiO2, Si3N4, SiNx, and SiON, but the passivation effect of these materials is insufficient.
[0003] 1. SiO2 is usually used as the passivation layer material deposited after the metal electrode of the chip is fabricated. In order to reduce the impact on the electrode performance, a high deposition temperature cannot be used, which results in poor adhesion and easy detachment, failing to form effective protection. In addition, SiO2 has low density and high pinhole density, and its moisture resistance and corrosion resistance are not ideal. 2. Si3N4 thin films have good resistance to moisture and corrosion, but as a passivation layer, they will generate a large amount of surface charge with semiconductor devices. The high-density surface will cause defects. Moreover, the high refractive index of Si3N4 will affect the light output of the test structure and reduce the brightness. 3. Currently, the known refractive indices of SiO2 and SiNx are 1.5 and 2.07, respectively, while the refractive index of SiON is between 1.5 and 1.9. The ideal passivation layer material has a refractive index of 1.93, which is closest to that of SiON. However, SiON also suffers from insufficient protection. Summary of the Invention
[0004] To address the shortcomings of existing technologies, the present invention aims to provide a method for preparing an Al2O3 passivation layer, a structure and method for testing its moisture resistance, and to provide a passivation layer with excellent moisture resistance that does not reduce luminescence performance, thereby maximizing the moisture resistance of the luminescent chip while ensuring its luminescence performance.
[0005] A first aspect of the present invention is to provide a method for preparing an Al2O3 passivation layer, the method comprising: An LED chip is placed in a reaction chamber, and TMA vapor is controlled to enter the reaction chamber in a pulsed manner, where a chemical adsorption reaction occurs on the wafer surface of the LED chip. An inert gas is first purged into the reaction chamber to allow some TMA vapor and the reaction byproduct methane to exit the reaction chamber. Water vapor is controlled to enter the reaction chamber in a pulsed manner, and continues to carry out surface chemical reaction with the wafer surface adsorbed with TMA precursor; The inert gas is purged into the reaction chamber again to remove excess water vapor and reaction byproduct methane, resulting in a single-layer Al2O3 film. Repeat the above steps multiple times to obtain an Al2O3 passivation layer of the preset thickness.
[0006] According to one aspect of the above technical solution, the duration of the chemical adsorption reaction on the wafer surface of the LED chip is 50s-100s, and the reaction temperature of the reaction chamber is 200℃-300℃.
[0007] According to one aspect of the above technical solution, the inert gas purging the reaction chamber is N2, and the duration of the first purging and the second purging of the inert gas is 30s-50s.
[0008] According to one aspect of the above technical solution, the continuous reaction time for water vapor to continue the surface chemical reaction with the wafer surface adsorbed with the TMA precursor is 50s-100s.
[0009] According to one aspect of the above technical solution, the number of cycles to form the Al2O3 passivation layer is 120-160.
[0010] According to one aspect of the above technical solution, the preset thickness is 600Å-800Å.
[0011] A second aspect of the present invention is to provide a moisture resistance test structure for a passivation layer on the surface of an LED chip, the test structure comprising: A substrate, an N-type semiconductor layer, a multiple quantum well layer and a P-type multiple quantum well layer stacked on the substrate, and an electron blocking layer and a transparent conductive layer stacked on the P-type multiple quantum well layer. An N-type metal electrode and a P-type metal electrode, wherein the N-type metal electrode is disposed on the N-type semiconductor layer and the P-type metal electrode is disposed on the P-type semiconductor layer, wherein one of the N-type metal electrode and the P-type metal electrode is a Ti-containing metal electrode whose outermost layer contains Ti metal and the other is a Ti-free metal electrode whose outermost layer does not contain Ti metal. The passivation layer includes an Al2O3 passivation layer prepared by the preparation method shown in the above technical solution, the Al2O3 passivation layer covering the wafer surface of the test structure and exposing the Ti-free metal electrode, and a SiO2 passivation layer covering the wafer surface and exposing the Ti-containing metal electrode.
[0012] A third aspect of the present invention provides a method for testing the moisture resistance of a passivation layer on the surface of an LED chip, the method employing the test structure described in the above technical solution, the method comprising: The LED chip is placed on a preset yellow film, and the LED chip is powered on. The positive terminal of the power supply is connected to the P-type metal electrode of the LED chip, and the negative terminal of the power supply is connected to the N-type metal electrode of the LED chip. A preset electrolyte is dropped onto the wafer surface of the LED chip until it covers the wafer surface; Obtain the initial voltage Vf0 at the initial moment; Starting from the initial moment, a preset time is started and the power is turned off. The initial voltage Vf0 at the initial moment is repeatedly acquired to generate the electrical data of the LED chip within the preset time. When the output voltage Vf and the initial voltage Vf0 meet the preset conditions, the LED chip is determined to be faulty.
[0013] According to one aspect of the above technical solution, the electrolyte is 0.1g NaCl + 100mL ultrapure water.
[0014] According to one aspect of the above technical solution, the method further includes performing a high-temperature and high-humidity aging test on the test structure, including: The test structure was placed in a constant temperature and humidity test chamber at 85℃ / 85%RH and continuously tested with a -5V reverse voltage. A 20mA current was applied to light the device at 24h, 96h, and 168h, and the test time was gradually increased to 1000h to obtain the changes in its positive voltage and brightness.
[0015] Compared with existing technologies, the advantages of using the Al2O3 passivation layer preparation method, moisture resistance testing structure and method shown in this invention are as follows: By preparing an Al2O3 passivation layer and testing the structure with the Al2O3 passivation layer, it was verified that the Al2O3 passivation layer has good adhesion, high density, and strong resistance to moisture and corrosion, making it more advantageous than SiO2 as a passivation layer material. Furthermore, the effects of Al2O3 and SiO2 passivation layers on LED photoelectric properties were compared experimentally. It was found that Al2O3 passivation resulted in better output light power and a more effective passivation effect. Additionally, LED chips using the Al2O3 passivation layer exhibited stronger resistance to moisture and high-temperature / high-humidity aging than those using the Al2O3 passivation layer. Attached Figure Description
[0016] The above and / or additional aspects and advantages of the present invention will become apparent and readily understood from the description of the embodiments taken in conjunction with the following drawings, in which: Figure 1 This is a schematic flowchart of the method for preparing the Al2O3 passivation layer shown in the embodiment of the present invention; Figure 2 This is a schematic diagram of the forward voltage variation characteristic curve of the test structure sample shown in the embodiment of the present invention over time; Figure 3 This is a schematic diagram of the characteristic curve of the forward voltage of the test structure sample shown in the embodiment of the present invention under high temperature and high humidity conditions of 85℃ / 85%RH for 1000h as a function of aging time. Figure 4 This is a schematic diagram of the brightness variation characteristic curve of the test structure sample shown in the embodiment of the present invention under high temperature and high humidity conditions of 85℃ / 85%RH for 1000h as a function of aging time. Detailed Implementation
[0017] To make the objectives, features, and advantages of the present invention more apparent and understandable, specific embodiments of the present invention will be described in detail below with reference to the accompanying drawings. Several embodiments of the present invention are shown in the drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. Rather, these embodiments are provided so that the disclosure of the present invention will be more thorough and complete.
[0018] It should be noted that when a component is said to be "fixed to" another component, it can be directly on the other component or there may be an intervening component. When a component is said to be "connected to" another component, it can be directly connected to the other component or there may be an intervening component. The terms "vertical," "horizontal," "left," "right," and similar expressions used in this document are for illustrative purposes only.
[0019] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein in the description of the invention is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.
[0020] Please see Figure 1 The first aspect of the present invention is to provide a method for preparing an Al2O3 passivation layer, the method comprising steps S01-S05: Step S01: Place the LED chip in the reaction chamber and control the TMA vapor to enter the reaction chamber in a pulsed manner, so that a chemical adsorption reaction occurs on the wafer surface of the LED chip. Step S02: First, inert gas is purged into the reaction chamber to allow some TMA vapor and reaction byproduct methane to exit the reaction chamber. Step S03: Control water vapor to enter the reaction chamber in a pulsed manner, and continue to carry out surface chemical reaction with the surface on which the TMA precursor is adsorbed; Step S04: Purge the inert gas into the reaction chamber again to remove excess water vapor and reaction byproduct methane, thus obtaining a single-layer Al2O3 film. Step S05: Repeat the above steps multiple times to obtain an Al2O3 passivation layer of a predetermined thickness in the form of a thin film.
[0021] In this invention, the chemical adsorption reaction on the wafer surface of the LED chip lasts for 50-100 seconds, and the reaction temperature in the reaction chamber is 200-300°C.
[0022] In this invention, the inert gas purging the reaction chamber is N2, and the duration of the first and second purging of the inert gas is 30s-50s.
[0023] In this invention, the continuous reaction time for water vapor to continue the surface chemical reaction with the surface adsorbed with the TMA precursor is 50s-100s.
[0024] In this invention, the number of cycles for forming the Al2O3 passivation layer is 120-160, and the preset thickness is 600Å-800Å.
[0025] Example 1 This embodiment provides a method for preparing an Al2O3 passivation layer, which includes steps S01-S05: Step S01: Place the LED chip in the reaction chamber and control the TMA vapor to enter the reaction chamber in a pulsed manner, so that a chemical adsorption reaction occurs on the wafer surface of the LED chip. Step S02: First, inert gas is purged into the reaction chamber to allow some TMA vapor and reaction byproduct methane to exit the reaction chamber. Step S03: Control water vapor to enter the reaction chamber in a pulsed manner, and continue to carry out surface chemical reaction with the surface on which the TMA precursor is adsorbed; Step S04: Purge the inert gas into the reaction chamber again to remove excess water vapor and reaction byproduct methane, thus obtaining a single-layer Al2O3 film. Step S05: Repeat the above steps multiple times to obtain an Al2O3 passivation layer of a predetermined thickness in the form of a thin film.
[0026] In this embodiment, the chemical adsorption reaction on the wafer surface of the LED chip lasts for 50 seconds, and the reaction temperature in the reaction chamber is 230°C.
[0027] In this embodiment, the inert gas purging the reaction chamber is N2, and the duration of the first and second purging of the inert gas is 30 seconds.
[0028] In this embodiment, the continuous reaction time for water vapor to continue the surface chemical reaction with the surface where the TMA precursor is adsorbed is 50 seconds.
[0029] In this embodiment, the Al2O3 passivation layer is formed by 140 cycles and has a thickness of 700 Å.
[0030] An Al2O3 passivation layer was obtained using the above preparation method. A chip with an Al2O3 passivation layer thickness of 700 Å was used. After covering with encapsulant, the chip was tested. A point test was performed using a 20 mA current. The output voltage vf was measured to be 2.57 V and the brightness Po was 20.51 mW.
[0031] Example 2 This embodiment also provides an Al2O3 passivation layer. The difference between this embodiment and Embodiment 1 is that the Al2O3 passivation layer is formed by 200 cycles and has a thickness of 1000 Å. Using a chip with an Al2O3 passivation layer of 1000 Å thickness, after covering it with encapsulant, the chip is tested. A point test is performed using a 20 mA current, and the output voltage vf is measured to be 2.58 V and the brightness Po is 20.21 mW.
[0032] Example 3 This embodiment also provides an Al2O3 passivation layer. The difference between this embodiment and Embodiment 1 is that the Al2O3 passivation layer is formed by 80 cycles and has a thickness of 400 Å. Using a chip with an Al2O3 passivation layer of 400 Å thickness, after covering it with encapsulant, the chip is tested. A point test is performed using a 20 mA current, and the output voltage vf is measured to be 2.58 V and the brightness Po is 19.55 mW.
[0033] Comparative Example 1 This comparative example provides a SiO2 passivation layer, which differs from Example 1 in that the type of passivation layer and the preparation method are different. The SiO2 passivation layer is prepared using a PECVD device, and the specific operation steps are as follows: The SiO2 deposition temperature was 230℃. The first step was vacuuming; the second step was preheating at a pressure of 120 Pa, with 1000 sccm of N2 introduced for 30 s; the third step was a holding stage at a pressure of 90 Pa, with N2, N2O, and SiH4 introduced at gas volumes of 600 sccm, 1000 sccm, and 206 sccm respectively, for 15 s; the fourth step was the first stage deposition at a power of 90 W and a pressure of 90 Pa, with N2, N2O, and SiH4 introduced at gas volumes of 600 sccm, 1000 sccm, and 206 sccm respectively, for 15 s; the fifth step was the N2O purging stage. The first step was a vacuum breaking process. The chip was filled with N2O at a power of 80W and a pressure of 120Pa, with a gas volume of 1200 sccm and a duration of 120s. The sixth step was a holding stage, with a pressure of 90Pa, filled with N2, N2O, and SiH4, with gas volumes of 600 sccm, 1000 sccm, and 206 sccm respectively, for a duration of 15s. The seventh step was the second deposition stage, with a power of 90W and a pressure of 90Pa, filled with N2, N2O, and SiH4, with gas volumes of 600 sccm, 1000 sccm, and 206 sccm respectively, for a duration of 180s. Finally, a 1000Å thick SiO2 layer was obtained. The last step was vacuum breaking. Using the 1000Å thick SiO2 passivation layer, after covering with encapsulant, the chip was tested. Point measurements were performed using a 20mA current, and the measured output voltage (vf) was 2.57V, and the brightness (Po) was 19.48mW.
[0034] Table 1 is a parameter comparison table for Examples 1-3 and Comparative Example 1.
[0035] Table 1 Based on Examples 1-3, Comparative Example 1, and Table 1, it can be seen that when the passivation layer type is the same, excessively high or low passivation layer thickness will reduce the luminous efficiency of the light-emitting chip using this passivation layer at 20mA to some extent. However, when the passivation layer type is different but the passivation layer thickness is equal, and other structures of the light-emitting chip are the same, using an Al2O3 passivation layer has a certain advantage in luminous efficiency at 20mA compared to a SiO2 passivation layer. In summary, using Al2O3 to prepare the passivation layer and using this Al2O3 passivation layer to encapsulate the light-emitting chip results in a significantly higher luminous efficiency.
[0036] A second aspect of the present invention is to provide a moisture resistance test structure for a passivation layer on the surface of an LED chip, the test structure comprising: A substrate, an N-type semiconductor layer, a multiple quantum well layer and a P-type multiple quantum well layer stacked on the substrate, and an electron blocking layer and a transparent conductive layer stacked on the P-type multiple quantum well layer. An N-type metal electrode and a P-type metal electrode, wherein the N-type metal electrode is disposed on the N-type semiconductor layer and the P-type metal electrode is disposed on the P-type semiconductor layer, wherein one of the N-type metal electrode and the P-type metal electrode is a Ti-containing metal electrode whose outermost layer contains Ti metal and the other is a Ti-free metal electrode whose outermost layer does not contain Ti metal. The passivation layer includes an Al2O3 passivation layer prepared by the method described above, which covers the wafer surface of the test structure and exposes the Ti-free metal electrode, and a SiO2 passivation layer covering the wafer surface and exposing the Ti-containing metal electrode, wherein the SiO2 passivation layer is fabricated using a PECVD process.
[0037] A third aspect of the present invention provides a method for testing the moisture resistance of a passivation layer on the surface of an LED chip, the method employing the test structure described in the second aspect above, the method comprising: The LED chip is placed on a preset yellow film, and the LED chip is powered on. The positive terminal of the power supply is connected to the P-type metal electrode of the LED chip, and the negative terminal of the power supply is connected to the N-type metal electrode of the LED chip. A preset electrolyte is dropped onto the wafer surface of the LED chip until it covers the wafer surface; Obtain the initial voltage Vf0 at the initial moment; Starting from the initial moment, a preset time is started and the power is turned off. The initial voltage Vf0 at the initial moment is repeatedly acquired to generate the electrical data of the LED chip within the preset time. When the output voltage Vf and the initial voltage Vf0 meet the preset conditions, the LED chip is determined to be faulty.
[0038] In this invention, the electrolyte is 0.1g NaCl + 100mL ultrapure water.
[0039] In this invention, the method further includes performing a high-temperature and high-humidity aging test on the test structure, including: The test structure was placed in a constant temperature and humidity test chamber at 85℃ / 85%RH and continuously tested with a -5V reverse voltage. A 20mA current was applied to light the device at 24h, 96h, and 168h, and the test time was gradually increased to 1000h to obtain the changes in its positive voltage and brightness.
[0040] As a novel functional semiconductor material, Al2O3 with a refractive index of 1.77 offers better protection. This is because Al2O3 has good adhesion, high density, and strong resistance to moisture and corrosion, making it more advantageous than SiO2 as a passivation layer material. Through experiments comparing the effects of Al2O3 and SiO2 passivation layers on LED photoelectric properties, it was found that Al2O3 passivation resulted in better output light power and a more effective passivation effect.
[0041] The following are experimental data on the effects of Al2O3 and SiO2 passivation layers on LED photoelectric properties (before humidity resistance and high temperature and humidity aging tests): ① Preparation of experimental samples: The sample used in this experiment was a GaN-based LED chip with sapphire as the substrate. The fabrication process was as follows: First, the morphology of n-GaN was etched and exposed using inductively coupled plasma (ICP) etching technology. Next, SiO2 was deposited on the chip surface as a current blocking layer using plasma-enhanced chemical vapor deposition (PECVD) to improve the current congestion near the P-type metal electrode. Then, an ITO transparent conductive film was deposited using electron beam evaporation. Subsequently, the P-type and N-type metal electrodes of the chip were fabricated, with two electrode structures, one of which consisted of C... In the Cr / Al / Ti / Ni / Pt / Ni / Pt / Au electrode structure, since SiO2 has poor adhesion, Ti is needed as a transition layer to enhance its adhesion. In the other electrode structure, Al2O3 passivation layer is used, and Al2O3 has good adhesion, so there is no need to add an outermost Ti layer. The electrode structure is Cr / Al / Ti / Ni / Pt / Ni / Pt / Au. Finally, SiO2 is deposited by PECVD as a passivation layer on the electrode structure with Ti on the outer layer, and Al2O3 is deposited by ALD as a passivation layer on the electrode structure without Ti on the outer layer.
[0042] The preparation process steps for the Al2O3 passivation layer deposited by ALD are as follows: ALD process: cross-chemical adsorption of reactants → surface reaction → desorption; The ALD deposition technique used here is thermal atomic layer deposition (TALD), which utilizes heating to provide activation energy for chemisorption during the thin film deposition process. Taking trimethylaluminum (TMA) as the aluminum source and water vapor as the oxygen source, the reaction for depositing an Al2O3 thin film is as an example. Each unit cycle consists of four steps: TMA vapor is controlled to enter the reaction chamber in a pulsed manner, where it undergoes a chemical adsorption reaction on the wafer surface of the LED chip; An inert gas is first purged into the reaction chamber to allow some TMA vapor and the reaction byproduct methane to exit the reaction chamber. Water vapor is controlled to enter the reaction chamber in a pulsed manner, and continues to carry out surface chemical reaction with the surface on which the TMA precursor is adsorbed. The inert gas is purged into the reaction chamber again to remove excess water vapor and the reaction byproduct methane, resulting in a single-layer Al2O3 film.
[0043] Figure 1 This is a schematic diagram of an LED chip. The PV layer is the passivation layer of the LED chip, namely the SiO2 passivation layer and the Al2O3 passivation layer.
[0044] To compare the effects of different passivation layer materials and thicknesses on the moisture resistance of the chip, this embodiment uses a PECVD-deposited 100nm SiO2 passivation layer as the control group and an ALD-prepared Al2O3 passivation layer as the experimental group, with deposition thicknesses of 100nm, 70nm, and 40nm, respectively. The chip with the PECVD-deposited 100nm SiO2 passivation layer is designated as sample A, and the chips with ALD-deposited 100nm, 70nm, and 40nm Al2O3 passivation layers are designated as samples B, C, and D, respectively.
[0045] Table 2 shows the photoelectric properties of the chip under a bare die current of 20mA. As can be seen from the table, the forward voltage Vf and wavelength Wd of each sample are not much different. However, the output light power Po of sample A is the highest, and the output light power of sample C is greater than that of samples B and D. The Al2O3 passivation layer does not seem to show better photoelectric properties than the SiO2 passivation layer, and the output light power is not necessarily higher with a larger coating thickness.
[0046] Table 2 Previous studies on Al2O3 passivation layers have tested photoelectric properties by encapsulating LED chips into LED beads. To verify the accuracy of the data, encapsulant was subsequently applied to LED chips to simulate LED beads and the photoelectric properties were retested. As shown in Table 3, after encapsulation, the output light power of samples B, C, and D all exceeded that of sample A. This indicates that the Fresnel loss between the Al2O3 passivation layer and the encapsulant is reduced, thereby improving the output light power. Among them, the 70nm Al2O3 passivation layer of sample C exhibited the best photoelectric properties.
[0047] Table 3 It should be noted that traditional SiO2 passivation layers are deposited using plasma-enhanced chemical vapor deposition (PECVD). PECVD offers low deposition temperatures and high rates, but suffers from poor film uniformity. Atomic layer deposition (ALD) offers unparalleled advantages over other thin film preparation techniques in terms of film uniformity and thickness control. Al2O3 passivation layers prepared using ALD exhibit the best coating effect, with a uniform and compact film texture and excellent resistance to moisture and corrosion. For LEDs, the moisture resistance of the passivation layer directly affects the reliability of the chip. Therefore, this study compares Al2O3 films prepared using ALD with traditional PECVD-prepared SiO2 passivation layers, using moisture resistance tests and high-temperature, high-humidity aging tests to evaluate the moisture resistance of the two passivation layers.
[0048] In this embodiment, the experimental equipment and procedures for the moisture resistance test and the high temperature and high humidity aging test are as follows: Prior to the moisture resistance test and the high temperature and humidity test, the chip experimental samples prepared under the above conditions were subjected to photoelectric property testing using a wafer spot tester with an operating current of 20mA. To specifically test the moisture resistance of LED chips, this test employed reverse electrolysis testing. The required equipment included a current source, electrolyte, spot test probe (tungsten carbide needle), and a yellow film. This method increases the ionization rate through the electrolyte, accelerating the hydrolysis of the LED chip. This not only effectively shortens the testing time but also ensures that the bare die test is unaffected by factors such as encapsulation adhesive and substrate, thus more accurately reflecting the moisture resistance of the LED chip itself. The specific testing procedure is as follows: (1) Place the chip on the yellow film, connect the probe to the current source, connect the positive terminal of the probe to the P-type metal electrode of the chip, and connect the negative terminal to the N-type metal electrode of the chip. Set the input voltage of the current source to -3.8V and the current limit to 50uA. (2) Use a syringe to draw some of the prepared electrolyte (0.1g NaCl + 100mL ultrapure water) and drop it onto the chip surface until it is covered; (3) Click the current source input terminal I, output terminal V, click the output switch, and record the output voltage Vf0 at this moment. The data at this moment is the 0min data for comparison reference. (4) Next, turn on the current source input terminal V and input terminal I, click the output switch, and turn off the output switch after timing for 2 minutes. Repeat step 3 and record the data for 2 minutes. Repeat steps (3) and (4) until the output voltage Vf increases by 1.05 times compared to the output voltage Vf0 at 0 minutes (Vf>Vf0*1.05), then the chip is determined to be faulty.
[0049] To ensure the accuracy of the experimental results, the samples were also subjected to high-temperature and high-humidity aging tests. The high-temperature and high-humidity aging test involved placing the samples in a constant temperature and humidity test chamber at 85℃ / 85%RH, followed by continuous burning with a -5V reverse voltage. A 20mA current was applied at 24h, 96h, and 168h to activate the light, and the test time was gradually increased to 1000h before observing changes in forward voltage and brightness.
[0050] Experimental Results and Discussion: Four different passivation layer samples were tested using reverse electrolysis, such as... Figure 2 The figure shows the characteristic curve of the forward voltage of the sample changing over time. Based on the failure criterion of Vf > Vf0 * 1.05, the testing times for samples A, B, C, and D were 34 min, 68 min, 50 min, and 42 min, respectively. The forward voltage increased with increasing testing time. The forward voltages at 0 min were 2.638 V, 2.644 V, 2.642 V, and 2.632 V, respectively. Due to the resistance of the electrolyte dripped onto the chip surface, the measured voltage was higher than that measured by the spot tester. The failure voltages of the failed samples were 2.853 V, 2.850 V, 2.865 V, and 2.842 V, respectively, all exceeding 1.05 times the initial voltage. Comparative data reveals that sample B reached failure time the longest, indicating that the 100nm Al2O3 passivation layer deposited by ALD has the best moisture resistance. The failure times for samples C and D are both longer than that for sample A, suggesting that the moisture resistance of the ALD-deposited Al2O3 passivation layer is superior to that of the PECVD-deposited SiO2 passivation layer. The failure time of sample B > sample C > sample D indicates that the thicker the ALD-deposited Al2O3 passivation layer, the better its moisture resistance.
[0051] like Figure 3 As shown, the forward voltage of four samples under 1000 hours of high temperature and humidity (85℃ / 85%RH) varies with aging time. The forward voltage of sample A stabilizes before 96 hours, then shows a significant upward trend, with the voltage at 1000 hours increasing by 19.84% compared to 0 hours. Under high temperature and humidity, the passivation effect of the SiO2 passivation layer deposited by PECVD is not ideal. With increasing aging time, the ohmic contacts between materials in the device degrade, semiconductor defects increase, and corrosion occurs at the gold wires, leading to increased series resistance and a significant increase in forward voltage. The forward voltages of samples B, C, and D show no significant change. This is because the Al2O3 passivation layer deposited by ALD has excellent passivation protection, mitigating the penetration of moisture. Within the limited aging time, the change in forward voltage clearly shows that Al2O3 has better moisture resistance than SiO2, but the difference in forward voltage between different passivation layer thicknesses is not significant.
[0052] like Figure 4 The figure shows the brightness variation curves of four samples under 1000h of high temperature and high humidity conditions (85℃ / 85%RH) as a function of aging time. As can be seen from the figure, the brightness of all four samples decreased under these conditions. Sample A showed the most significant brightness decrease, with a 23% reduction in brightness after 1000h compared to 0h. The brightness decrease was most pronounced between 0 and 200h. In this high temperature and high humidity environment, high temperature accelerates chip performance degradation, while the introduction of moisture accelerates various chemical reactions, leading to reduced light output and brightness. The brightness decreases for samples B, C, and D were 1.47%, 3.05%, and 4.12%, respectively. This indicates that the 100nm Al2O3 passivation layer showed the least brightness decrease, followed by the 70nm Al2O3 passivation layer, and the 40nm Al2O3 passivation layer showed the greatest decrease. Based on the above data, it can be concluded that the moisture resistance of the Al2O3 passivation layer deposited by ALD is better than that of the SiO2 passivation layer deposited by PECVD, and the thicker the Al2O3 passivation layer, the stronger its moisture resistance.
[0053] In summary, this embodiment first introduces the current research status of LED passivation layers, pointing out that Al2O3 is a superior passivation layer material compared to SiO2, and that ALD deposition technology is superior to PECVD. To improve the chip's inherent moisture resistance, it is proposed to change the passivation layer material of the LED chip by using ALD to prepare an Al2O3 passivation layer instead of the SiO2 passivation layer prepared by PECVD. Specifically, PECVD deposits a 100nm SiO2 passivation layer, while ALD deposits 100nm, 70nm, and 40nm Al2O3 passivation layers. The prepared samples were subjected to photoelectric property testing. In bare-die testing, the SiO2 passivation layer sample exhibited better photoelectric properties than the Al2O3 passivation layer sample. After capping with adhesive, the photoelectric properties of the Al2O3 passivation layer improved, with a thickness of 70nm showing the best output light power. Subsequently, the samples underwent reverse electrolysis testing and 85℃ / 85%RH high-temperature and high-humidity aging testing. In reverse electrolysis testing, the ALD-deposited Al2O3 passivation layer sample reached failure time faster than the PECVD-deposited SiO2 passivation layer sample. In high-temperature and high-humidity aging testing, the forward voltage drift of the Al2O3 passivation layer was smaller than that of the SiO2 passivation layer. The brightness decrease of the SiO2 passivation layer reached 23%, while the highest brightness decrease in the Al2O3 passivation layer was observed in the 40nm thick layer, at 4.12%, significantly lower than that of the SiO2 passivation layer. Both reverse electrolysis and high-temperature and high-humidity aging tests demonstrate that the passivation effect of Al2O3 is superior to that of SiO2, and the thicker the deposited Al2O3, the more significant its moisture resistance.
[0054] In the description of this specification, references to terms such as "one embodiment," "some embodiments," "example," "specific example," or "some examples," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.
[0055] The embodiments described above are merely illustrative of several implementations of the present invention, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the present invention. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these all fall within the protection scope of the present invention. Therefore, the protection scope of this patent should be determined by the appended claims.
Claims
1. A method for preparing an Al2O3 passivation layer, characterized in that, The preparation method includes: An LED chip is placed in a reaction chamber, and TMA vapor is controlled to enter the reaction chamber in a pulsed manner, where a chemical adsorption reaction occurs on the wafer surface of the LED chip. An inert gas is first purged into the reaction chamber to allow some TMA vapor and the reaction byproduct methane to exit the reaction chamber. Water vapor is controlled to enter the reaction chamber in a pulsed manner, and continues to carry out surface chemical reaction with the wafer surface adsorbed with TMA precursor; The inert gas is purged into the reaction chamber again to remove excess water vapor and reaction byproduct methane, resulting in a single-layer Al2O3 film. Repeat the above steps multiple times to obtain an Al2O3 passivation layer of the preset thickness; The chemical adsorption reaction on the wafer surface of the LED chip lasts for 50-100 seconds, and the reaction temperature in the reaction chamber is 200-300℃. The continuous reaction time for water vapor to continue the surface chemical reaction with the TMA precursor adsorbed on the wafer surface is 50s-100s. The number of cycles required to form the Al2O3 passivation layer is 120-160.
2. The method for preparing the Al2O3 passivation layer according to claim 1, characterized in that, The inert gas purging the reaction chamber is N2, and the duration of the first and second purging of the inert gas is 30s-50s.
3. The method for preparing the Al2O3 passivation layer according to claim 1, characterized in that, The preset thickness is 600Å-800Å.
4. A moisture resistance test structure for the passivation layer on the surface of an LED chip, characterized in that, The test structure includes: A substrate, an N-type semiconductor layer, a multiple quantum well layer and a P-type semiconductor layer stacked on the substrate, and an electron blocking layer and a transparent conductive layer stacked on the P-type semiconductor layer; An N-type metal electrode and a P-type metal electrode, wherein the N-type metal electrode is disposed on the N-type semiconductor layer and the P-type metal electrode is disposed on the P-type semiconductor layer, wherein one of the N-type metal electrode and the P-type metal electrode is a Ti-containing metal electrode whose outermost layer contains Ti metal and the other is a Ti-free metal electrode whose outermost layer does not contain Ti metal. The passivation layer includes an Al2O3 passivation layer prepared by any one of claims 1-3, the Al2O3 passivation layer covering the wafer surface of the test structure and exposing the Ti-free metal electrode, and a SiO2 passivation layer covering the wafer surface and exposing the Ti-containing metal electrode.
5. A method for improving the moisture resistance of a passivation layer on the surface of an LED chip, characterized in that, The method employs the test structure described in claim 4 for testing, and the method includes: The LED chip is placed on a preset yellow film, and the LED chip is powered on. The positive terminal of the power supply is connected to the P-type metal electrode of the LED chip, and the negative terminal of the power supply is connected to the N-type metal electrode of the LED chip. A preset electrolyte is dropped onto the wafer surface of the LED chip until it covers the wafer surface; Obtain the initial voltage Vf0 at the initial moment; Starting from the initial moment, a preset time is started and the power is turned off. The initial voltage Vf0 at the initial moment is repeatedly acquired to generate the electrical data of the LED chip within the preset time. When the output voltage Vf and the initial voltage Vf0 meet the preset conditions, the LED chip is determined to be faulty.
6. The method for improving the moisture resistance of the passivation layer on the surface of an LED chip according to claim 5, characterized in that, The electrolyte is 0.1g NaCl + 100mL ultrapure water.
7. The method for improving the moisture resistance of the passivation layer on the surface of an LED chip according to claim 5, characterized in that, The method further includes performing a high-temperature and high-humidity aging test on the test structure, including: The test structure was placed in a constant temperature and humidity test chamber at 85℃ / 85%RH and continuously tested with a -5V reverse voltage. A 20mA current was applied to light the device at 24h, 96h, and 168h, and the test time was gradually increased to 1000h to obtain the changes in its positive voltage and brightness.
Citation Information
Patent Citations
Substrate, LED epitaxial wafer having the substrate, chip and light-emitting device
CN102263181A
Light-emitting diode chip manufacturing method and light-emitting diode chip
JP2018029110A