Preparation method of high-efficiency evaporation membrane and comprehensive evaluation method for membrane surface performance

A hydrophilic-hydrophobic sandwich evaporation membrane with well-developed and uniformly distributed pores was prepared by plasma dry processing, which solved the problems of low flux and low desalination efficiency of existing evaporation membranes, and realized a highly efficient freshwater recovery and environmentally friendly modification technology.

CN116808844BActive Publication Date: 2026-11-24SUZHOU UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202310285042.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2026-11-24
Estimated Expiration
2043-03-22

AI Technical Summary

Technical Problem

Existing evaporation membranes have low membrane flux and low desalination efficiency, and wet chemical surface modification methods use large amounts of organic solvents, leading to environmental pollution.

Method used

A plasma dry process was adopted to modify the membrane surface with a hydrophilic-hydrophobic sandwich structure using silicon-based reagents. The hydrophobic or hydrophilic membrane was then modified by a plasma processor to prepare a high-efficiency evaporation membrane with well-developed and uniformly distributed pores.

Benefits of technology

It improves the desalination efficiency and flux of membranes, broadens the range of membrane options, reduces environmental pollution, and achieves efficient freshwater recovery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116808844B_ABST
    Figure CN116808844B_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing a high-efficiency evaporation membrane and a method for comprehensively evaluating the surface properties of the membrane. Belonging to the field of membrane modification and preparation technology, the method utilizes tridecafluorooctyltrimethoxysilane and commercially available SiO2 nanoparticles to prepare a hydrophobic modifying agent. Ammonia water is used to catalyze the hydrolysis and condensation of tetraethyl orthosilicate (TEOS) in an ethanol solution to prepare a hydrophilic modifying agent containing SiO2 nanoparticles. Plasma treatment is then used to sequentially modify the surface of the hydrophilic membrane in a "hydrophobic first, then hydrophilic" order, or to directly modify the surface of the hydrophobic membrane to be hydrophilic. This process prepares a hydrophilic-hydrophobic sandwich MD membrane with well-developed and uniformly distributed pores, further broadening the screening range for membranes used in MD desalination and further improving the MD desalination energy efficiency and production efficiency of existing commercial membranes, meeting the practical needs of the saline desalination market.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of membrane surface modification technology, specifically relating to a method for preparing a high-efficiency evaporation membrane and a method for comprehensively evaluating membrane surface performance. Background Technology

[0002] Freshwater scarcity and uneven distribution are among the major limiting factors hindering sustainable socio-economic development. Obtaining freshwater through desalination of seawater, brackish water, and industrial wastewater is an important way to effectively alleviate freshwater scarcity and environmental pollution. Currently, there are various water desalination technologies, with evaporation, reverse osmosis (RO), and membrane distillation (MD) being commonly used in production. Evaporation involves heating water to boiling and then cooling the steam generated to obtain freshwater; it is simple to install, flexible in construction, and easy to operate, but it has the highest energy consumption. RO desalination achieves transmembrane water desalination through the size repulsion of salt ions in the water by a dense RO membrane driven by feed-side pressure; it has high desalination efficiency, is easy to integrate and scale up, but has high feed-side driving pressure, high energy consumption, and strict limitations on influent salinity, suspended solids (SS), and other impurities. MD, on the other hand, is a new desalination technology that combines the advantages of evaporation and membrane desalination technologies and is suitable for operation under low-temperature conditions. This low-temperature operation characteristic creates the preconditions for MD to utilize low-grade waste heat wasted in actual production processes or to combine it with renewable energy sources such as solar and hydropower as heat or energy sources, or to integrate it with a high-efficiency latent heat recovery system. This can significantly reduce the energy input of MD, or even eliminate energy consumption altogether. Therefore, these flexible comprehensive energy-saving solutions for MD enable it to gain an increasing competitive advantage over other advanced desalination technologies and have become the most competitive advanced desalination technology.

[0003] The excellent desalination performance and wide applicability of microporous distillation (MD) membranes depend on the MD membrane itself. Commonly used hydrophobic polymer microporous MD membranes in industry include polypropylene (PP), polytetrafluoroethylene (PTFE), and polyvinylidene fluoride (PVDF). These hydrophobic polymer membranes have low intrinsic surface energy and are hydrophobic, allowing them to be directly applied to the MD desalination process. Semi-hydrophilic and hydrophilic nylon membranes, polysulfone membranes, and cellulose ester membranes require surface hydrophobic modification before they can be used for MD desalination. Generally, distillation membranes with a single hydrophobic surface suffer from low membrane flux and low desalination efficiency. Common methods for membrane surface modification can be divided into wet and dry methods. Wet chemical surface modification involves coating or impregnation to apply hydrophobic modifiers to the membrane surface. However, this method requires the use of hydrophobic / hydrophilic polymers containing large amounts of organic solvents and generates high concentrations of wastewater, waste gas, and other environmental pollutants. Plasma dry surface modification only requires monomer molecules of these hydrophobic / hydrophilic polymers as precursors, thus avoiding the use of other organic solvents and the environmental problems caused by them in the wet coating process. Therefore, plasma dry treatment is a green and clean material surface modification technology. Summary of the Invention

[0004] In view of the shortcomings of the prior art, the purpose of this invention is to provide a method for preparing a high-efficiency evaporation membrane and a method for comprehensively evaluating the surface properties of the membrane.

[0005] The objective of this invention can be achieved through the following technical solutions:

[0006] A method for preparing a high-efficiency evaporation membrane includes the following steps:

[0007] Select a hydrophilic membrane substrate or a hydrophobic membrane substrate, wash it, and then dry it to obtain the hydrophilic membrane substrate or hydrophobic membrane substrate to be modified.

[0008] The hydrophobic film substrate is directly immersed in a silicon-based hydrophilic modifier for uniform coating, dried, and then placed in a plasma processor for treatment to obtain a hydrophilic modified film.

[0009] Alternatively, the hydrophilic film substrate can be immersed in a prepared silicon-based hydrophobic modification reagent for uniform coating and drying, then treated with plasma, immersed in a prepared silicon-based hydrophilic modification reagent for uniform coating and drying, and finally placed in a plasma processor for treatment to obtain a hydrophilic-hydrophobic sandwich modified film.

[0010] The silicon-based hydrophobic modifier is prepared from tridecafluorooctyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane and SiO2, and the hydrophilic modifier is prepared by hydrolysis-condensation of tetraethyl orthosilicate in ethanol solution catalyzed by ammonia water.

[0011] Furthermore, the method for determining the uniformity of the hydrophilic modified film and the hydrophilic-hydrophobic sandwich modified film is to test the uniformity of the coating by testing its negative pressure curve in a fog or air environment.

[0012] Furthermore, the specific preparation method of the silicon-based hydrophobic modifying agent is as follows:

[0013] A silicon-based hydrophobic modifier was obtained by mixing tridecafluorooctyltrimethoxysilane and 3-glycidoxypropyltrimethoxysilane, adding SiO2, and then adding acetic acid.

[0014] Furthermore, the specific preparation method of the silicon-based hydrophilic modifying reagent is as follows:

[0015] The preparation method of the silicon-based hydrophilic modification reagent is as follows: prepare a TEOS ethanol solution by adding the TEOS ethanol solution to an ammonia / ethanol solution, wherein the concentration of the TEOS ethanol solution is 0.2 mol / L and the volume ratio of ammonia to ethanol in the ammonia / ethanol solution is 1:4.

[0016] Furthermore, the molar ratio of the tridecafluorooctyltrimethoxysilane and 3-glycidoxypropyltrimethoxysilane is 3:1, and the acetic acid concentration is 0.025 mol / L.

[0017] A high-efficiency evaporation membrane, comprising a hydrophilic modified membrane or a hydrophilic-hydrophobic sandwich modified membrane, wherein the hydrophilic modified membrane is coated with a silicon-based hydrophilic modifying agent and treated by a plasma processor, and the hydrophilic-hydrophobic sandwich modified membrane is sequentially coated with a silicon-based hydrophobic modifying agent and a silicon-based hydrophilic modifying agent and treated by a plasma processor.

[0018] Furthermore, the silicon-based hydrophilic modifying agent is prepared by hydrolyzing and condensing tetraethyl orthosilicate in an ethanol solution using ammonia water as a catalyst, and the silicon-based hydrophobic modifying agent is prepared by tridecafluorooctyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane and SiO2.

[0019] A silicon-based hydrophobic modifier is prepared from tridecafluorooctyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane and SiO2.

[0020] A silicon-based hydrophilic modifying agent is prepared by hydrolysis-condensation of tetraethyl orthosilicate in an ethanol solution catalyzed by ammonia water.

[0021] The beneficial effects of this invention are:

[0022] This invention provides a method for preparing a novel high-throughput hydrophobic-hydrophilic sandwich MD membrane based on plasma dry processing. A hydrophobic modifying agent is prepared using tridecafluorooctyltrimethoxysilane and commercially available SiO2 nanoparticles. Ammonia water is used to catalyze the hydrolysis and condensation of tetraethyl orthosilicate (TEOS) in an ethanol solution to prepare a hydrophilic modifying agent containing SiO2 nanoparticles. Plasma treatment is then used to sequentially modify the surface of the hydrophilic membrane in a "hydrophobic first, then hydrophilic" order, or to directly modify the surface of the hydrophobic membrane to be hydrophilic. This process prepares a hydrophilic-hydrophobic sandwich MD membrane with well-developed and uniformly distributed pores, further broadening the screening range for membranes used in MD desalination and further improving the MD desalination energy efficiency and production efficiency of existing commercial membranes, meeting the practical needs of the saline desalination market. Furthermore, the plasma dry surface modification process only requires these monomer molecules as precursors, thus avoiding the use of other organic solvents and the environmental problems they cause, making it a green and clean material surface modification technology. Attached Figure Description

[0023] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, for those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0024] Figure 1 This is a schematic diagram of the hydrophobic MD membrane, Janus MD membrane, and hydrophilic-hydrophobic sandwich MD membrane of the present invention;

[0025] Figure 2 The effects of the filter paper, the number of times the hydrophobic reagent was applied, and the DBD plasma treatment on the air osmotic pressure of this invention are as follows: a) untreated filter paper, b) 1-time dipping, c) 2-time dipping, d) 3-time dipping, e) 1-time dipping + plasma treatment (24V, 5min). Detailed Implementation

[0026] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0027] To address the issues of low membrane flux and low desalination efficiency associated with distillation membranes having only one hydrophobic surface, we discovered the potential of using a Janus membrane (such as...) with one hydrophilic and one hydrophobic surface. Figure 1As shown, the desalination efficiency of MD membranes can be further improved. Given the technical advantage of the high desalination efficiency of Janus MD membranes, and considering the low flux and efficiency of distillation membranes with only a single hydrophobic surface (including commercial hydrophobic membranes), the inability of hydrophilic membranes to be directly used for MD desalination, and the practical problems of large amounts of organic solvents and the generation of "three wastes" pollutants in wet chemical surface modification of membranes, it was found in the process of plasma functional modification of different substrate materials that: by using an air dielectric barrier discharge (DBD) plasma processor, the hydrophilicity of traditional hydrophobic membranes can be directly controlled by air discharge plasma treatment; and by using plasma to induce in-situ polymerization of low surface energy monomer molecules such as silanes and fluorosilanes on the surface of hydrophilic substrates, the hydrophobic modification of existing hydrophilic commercial microporous membranes can also be achieved, enabling them to be used for MD desalination and freshwater recovery, greatly expanding the selection range of membranes for MD. Meanwhile, using commercial SiO2 nanoparticles to prepare surface-roughened hydrophobic films can further improve the flux and desalination efficiency of single hydrophobic surface distillation films. However, due to the self-aggregation of commercial nano-SiO2 particles during the solution preparation or plasma treatment of raw materials, it is difficult to form a uniform rough coating on the surface of the modified material and to control the ideal pores required for the transmembrane permeation of MD gas-phase water molecules. Numerous experimental studies have found that using silicon-based reagents under the induced drive of air dielectric barrier discharge (DBD) plasma treatment, SiO2 particles can be polymerized in the gas phase to form larger particles, thereby modifying the surface of the membrane substrate (hydrophobic or hydrophilic membrane) with a uniform roughened layer of hydrophobic or hydrophilic nano-SiO2 particles.

[0028] A method for preparing a high-efficiency evaporation membrane is as follows:

[0029] According to the membrane diameter required for the MD desalination experimental apparatus First, select the hydrophobic or hydrophilic membrane to be treated and cut it to the required size for the MD desalination membrane. Then, wash these membrane substrates with deionized water and dry them in an oven at 60°C to obtain the membrane substrate to be modified. For hydrophobic commercial membranes (PP, PTFE, PVDF, etc.), prepare a silicon-based hydrophilic modification reagent containing SiO2 nanoparticles; or for hydrophilic commercial membranes (nylon, polysulfone membranes, etc.), prepare silicon-based hydrophobic and hydrophilic modification reagents containing SiO2 nanoparticles. Subsequently, for hydrophobic commercial films, they can be directly immersed in a prepared silicon-based hydrophilic modification reagent for pre-coating, dried in an oven at 110°C, and then placed in an air dielectric barrier discharge (DBD) plasma processor for in-situ polymerization and grafting. Alternatively, for hydrophilic commercial films (nylon, polysulfone films, etc.), they are first immersed in a prepared silicon-based hydrophobic modification reagent for pre-coating, dried in an oven at 110°C, hydrophobically modified by plasma treatment, then immersed in a prepared silicon-based hydrophilic modification reagent for dip coating, dried in an oven at 110°C, and then processed in an air dielectric barrier discharge (DBD) plasma processor. In this way, a hydrophilic-hydrophobic sandwich MD film with well-developed and uniformly distributed pores can be obtained. Furthermore, multiple dip coatings can achieve uniform coating modification and the required coating amount.

[0030] In this process, a hydrophobic modifying agent was prepared using tridecafluorooctyltrimethoxysilane and commercially available SiO2 nanoparticles. A hydrophilic modifying agent was prepared by hydrolyzing and condensing tetraethyl orthosilicate (TEOS) in an ethanol solution using ammonia water catalysis. The surface of the hydrophilic membrane was then modified stepwise in a "hydrophobic first, then hydrophilic" order using plasma treatment, or the hydrophobic membrane was directly modified to be hydrophilic, thus preparing a hydrophilic-hydrophobic sandwich MD membrane with highly developed and uniformly distributed pores.

[0031] Methods for evaluating the effects of membrane modification and the desalination performance of modified membranes (MD):

[0032] For pre-coated or modified MD films, the uniformity of the coating can be verified by testing its negative pressure curve in a fog or air environment. The specific procedure is as follows: First, connect the outlet of a commercial filter containing the MD film to be tested to a negative pressure device equipped with a pressure sensor, with the inlet open; then place it in a fog or air environment and apply negative pressure. Compare the changes in the negative pressure curves of the MD film before and after pre-coating or modification. This allows for a rapid and accurate verification of whether the uniformity of the film surface coating meets the standards, ensuring that a uniformly modified film is obtained after plasma treatment, and improving the one-time yield of the prepared film and the modification efficiency of qualified products. Alternatively, a fog (air) negative pressure test method can be used to test the uniformity and stability of the coating on modified MD films. The fog environment can be achieved in a closed space using an ultrasonic atomization device.

[0033] When evaluating the desalination performance of modified MD membranes, commonly used MD devices, such as direct contact MD (DCMD) or vacuum MD (VMD), can be used for testing to evaluate the desalination performance of the prepared membrane. The specific operation is as follows: The modified MD membrane is installed in the membrane module of the MD device for membrane distillation experiments, and the permeate flow rate and conductivity are measured within a certain operating time. This yields the desalination performance of the modified MD membrane under the set MD desalination operating conditions, including: desalination rate (%) and membrane flux (kg·m³). -2 ·h -1 This can guide the screening of membranes for MD desalination, and guide the actual production of MD desalination and freshwater recovery for different types of saline water.

[0034] Take, for example, a hydrophilic-hydrophobic sandwich MD membrane with well-developed and uniformly distributed pores, prepared by atmospheric pressure air dielectric barrier discharge (DBD) plasma treatment using hydrophilic membrane material as substrate.

[0035] First, based on the membrane diameter required for the MD desalination experimental setup... Select the hydrophilic membrane to be treated and cut the membrane substrate to the required size for the MD desalination membrane; then wash these membrane substrates with deionized water and dry them in an oven at 60°C to obtain the membrane substrate to be modified. At the same time, prepare a certain volume of silicon-based hydrophobic modification reagent containing SiO2 nanoparticles and silicon-based hydrophilic modification reagent containing SiO2 nanoparticles respectively, and put them into the hydrophobic pretreatment impregnation tank and the hydrophilic treatment impregnation tank respectively.

[0036] Then, the substrate to be modified is first immersed in a hydrophobic pretreatment dip coating bath for dip coating, and then dried in an oven at 110℃. This dip coating is repeated multiple times. The osmotic pressure curve of the membrane sample after each dip coating is tested with a mist osmotic pressure tester until the mist osmotic pressure curve of the membrane after dip coating is stable. The pre-dip coating is then stopped to obtain a uniform pre-coated membrane with the required amount of dip coating. Finally, the uniformly dip-coated membrane is placed in a DBD plasma processor for surface roughening and hydrophobic modification to obtain a uniformly roughened hydrophobic modified membrane. The DBD plasma treatment conditions are: the optimized treatment voltage is 24V and the treatment time is 5min. The hydrophobic modified film with roughened surface was then immersed in a hydrophilic coating bath for dip coating, and then dried in an oven at 110°C. This dip coating process was repeated multiple times, and the uniformity of the pre-coating was determined using the osmotic pressure curve as described above. The uniformly coated film was then placed in a DBD plasma processor for surface roughening and hydrophilic modification. The DBD plasma hydrophilic modification conditions were: optimized processing voltage of 30V and processing time of 5 minutes. After the above hydrophobic and hydrophilic modifications, an MD film with a well-developed and uniformly distributed hydrophilic-hydrophobic interlayer surface was obtained. During the film surface modification process, a mist osmotic pressure tester was used to test the modified MD film and evaluate the coating uniformity, stability, and other modification effects.

[0037] Finally, the modified membrane material was tested for desalination using a high-efficiency vacuum membrane distillation (VMD) desalination testing device. The specific operation was as follows: the modified MD membrane was installed in the membrane module of the VMD device for membrane distillation experiments, and the permeate flow rate and conductivity were measured within a certain operating time. This yielded the desalination performance of the modified MD membrane under the set MD desalination operating conditions, including: desalination rate (%) and membrane flux (kg·m³). -2 ·h -1 This can guide the screening or modification of membranes for MD desalination, as well as guide the actual production of MD desalination and freshwater recovery of saline water with different properties using the required membranes.

[0038] Among them, the MD film with well-developed and uniformly distributed hydrophilic-hydrophobic interlayer surface prepared by atmospheric pressure air dielectric barrier discharge (DBD) plasma treatment using hydrophilic film material as substrate is taken as an example. The preparation method of the hydrophobic modification reagent (1) used for hydrophobic surface modification of hydrophilic film material is as follows: first prepare 0.1 mol / L silane in ethanol / water solution (V 乙醇 V 水=1: The silanes include: tridecafluorooctyltrimethoxysilane and 3-glycidoxypropyltrimethoxysilane, with a molar ratio of 3:1; then add SiO2 particles with a particle size of 50±5nm and a concentration of 0.025mol / L; then add 0.1ml acetic acid, and stir at 1500rpm for 12h at room temperature using a CNC magnetic stirrer, and let it mature for later use. The preparation method of the hydrophilic modification reagent (2) is as follows: prepare a certain volume of 0.2mol / L TEOS ethanol solution, and then add the prepared TEOS ethanol solution dropwise to an equal volume of ammonia / ethanol solution at a certain feed rate, wherein the feed rate is 10ml / h, the volume ratio of ammonia to ethanol is 1:4, and after mixing, stir at 1500rpm for 12h at room temperature, and let it mature for later use.

[0039] Surface modification and desalination performance testing:

[0040] 1. Comparison of the effects of surface roughening hydrophobic coating and plasma treatment on the surface modification and desalination performance of filter paper hydrophilic membrane

[0041] For a comparison of hydrophobic modification of the hydrophilic surface of filter paper substrate and its desalination performance, please refer to [reference needed]. Figure 2 and Table 1. From Figure 2 As can be seen, the air negative pressure curve of the filter paper (without mist) fluctuates in the range of 10.13-10.23 kPa; the air osmotic pressure curve of the filter paper after being impregnated and dried in 0.1M fluorosilane hydrophobic modifier fluctuates in the range of 10.03-10.25 kPa. Compared with the filter paper, the maximum resistance increases after one impregnation, but the fluctuation range of the resistance curve further increases, indicating that the surface of the filter paper membrane is not uniformly coated and has relatively small defects and voids. When the fluctuation of the air osmotic pressure curve of the filter paper after two impregnations is eliminated, the membrane resistance value is maintained at 10.28 kPa; as the number of impregnations increases to three, the air osmotic pressure curve does not fluctuate, but the membrane resistance value increases to about 10.37 kPa, indicating that the impregnated coating is uniform and the thickness increases. Plasma treatment of the once-coated filter paper eliminated fluctuations in the air osmotic pressure curve, indicating that the fluorosilane monomer molecules in the coating underwent in-situ polymerization under plasma induction, forming a polymer coating of fluorosilane on the filter paper surface. This polymer coating prevented the migration of the fluorosilane monomer modification solution coating on the membrane surface. Table 1 shows that the uncoated filter paper exhibited the highest permeation flux, reaching 3657.9 L / m³. 2 The permeation flux was ·h, but the desalination rate was 0, indicating no desalination performance. Filter paper coated only with fluorosilane but not subjected to plasma treatment showed a slight decrease in permeation flux, with a value of 3302.4 L / m. 2 The permeability of the hydrophobic filter paper, after being coated once and subjected to plasma treatment, decreased to 27.6 L / m³, but the desalination rate remained at 0, indicating no desalination performance.2 The desalination rate increased to 67.3% with increasing temperature and humidity, demonstrating good desalination performance. The hydrophobic filter paper, after being coated twice and then treated with plasma, further reduced its permeation flux to 8.9 L / m³. 2 •h, the desalination rate is increased to 100.0%, demonstrating excellent desalination performance.

[0042] Table 1 Comparison of the desalination effects of hydrophobic reagent impregnation and DBD plasma treatment on filter paper (MD evaluation device operating conditions: feed 0.8% NaCl, temperature 60℃, temperature difference between the two membranes 50℃)

[0043]

[0044] 2. Comparison of the effects of surface roughening hydrophobic modification and surface roughening hydrophobic-hydrophilic modification on the desalination performance of commercial nylon membranes

[0045] Table 2 compares the effects of surface roughening hydrophobic modification and surface roughening hydrophobic-hydrophilic modification on the desalination performance of nylon membranes. As shown in Table 2, under the operating conditions of the MD experiment, the permeation flux of this commercial nylon membrane is 222.3 L / m³. 2 The surface roughened hydrophobic modified nylon membrane, prepared by pre-coating with a SiO2-containing roughened fluorosilane hydrophobic reagent and plasma treatment, exhibits a permeation flux of 15.0 L / m³, but with a desalination rate of 0, indicating no desalination performance. 2 The desalination rate reached 99.3%, demonstrating excellent desalination performance. A hydrophobic nylon membrane with a roughened surface and hydrophobic modification using fluorosilane was further modified with a roughening hydrophilic reagent via plasma treatment, resulting in a permeation flux of 27.3 L / m². 2 The desalination rate was further increased to 100.0%. While ensuring further improvement in desalination performance, the permeation flux of the nylon membrane with a roughened hydrophobic-hydrophilic surface increased by 82.0%, which greatly improved the permeate flux of the modified membrane and its energy efficiency of MD desalination.

[0046] Table 2 Comparison of the effects of surface roughening hydrophobic modification and surface roughening hydrophobic-hydrophilic modification on the desalination performance of nylon membranes

[0047] (MD evaluation device operating conditions: feed is 0.8% NaCl, temperature is 60℃, temperature difference between the two membranes is 50℃)

[0048]

[0049] 3. Comparison of the effects of surface roughening hydrophobic modification and surface roughening hydrophobic-hydrophilic modification on the desalination performance of commercial PP hydrophobic membranes

[0050] Table 3 compares the effects of surface roughening hydrophobic modification and surface roughening hydrophobic-hydrophilic modification on the desalination performance of commercial PP hydrophobic membranes. As shown in Table 3, under the operating conditions of the MD experiment, the commercial PP hydrophobic membrane exhibits good desalination performance, with a permeation flux of 8.3 L / m³. 2 •h, the desalination rate reached 99.0%. Plasma treatment was used to roughen and hydrophilically modify the commercial PP hydrophobic membrane, resulting in a surface-roughened hydrophobic-hydrophilic modified PP hydrophobic membrane with a permeation flux increasing to 13.9 L / m. 2 The desalination rate was further increased to 100.0% by h. While ensuring further improvement in desalination performance, the water flux of the nylon membrane with a roughened hydrophobic-hydrophilic surface increased by approximately 67.5%, effectively improving the desalination energy efficiency of commercial PP hydrophobic membranes.

[0051] Table 3 Comparison of the effects of surface roughening hydrophobic modification and surface roughening hydrophobic-hydrophilic modification on the desalination performance of PP membranes

[0052] (MD evaluation device operating conditions: feed is 0.8% NaCl, temperature is 60℃, temperature difference between the two membranes is 50℃)

[0053]

[0054] In the description of this specification, references to terms such as "an embodiment," "example," "specific example," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the invention. In this specification, illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.

[0055] The foregoing has shown and described the basic principles, main features, and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The embodiments and descriptions in the specification are merely illustrative of the principles of the invention. Various changes and modifications can be made to the invention without departing from its spirit and scope, and all such changes and modifications fall within the scope of the claimed invention.

Claims

1. A method for preparing a high-efficiency evaporation membrane, characterized in that, Includes the following steps: After selecting and washing the hydrophilic membrane substrate, it is dried to obtain the hydrophilic membrane substrate to be modified. The hydrophilic film substrate to be modified is immersed in the prepared silicon-based hydrophobic modification reagent for dip coating and then dried. The negative pressure curve of the film sample in the fog or air environment is tested after each dip coating. The pre-dip coating is stopped when the negative pressure curve of the film after dip coating is stable, and a uniform pre-coated film with the required dip coating amount is obtained. Then, the uniformly dip-coated film is placed in the DBD plasma processor for surface roughening and hydrophobic modification to obtain a uniformly roughened hydrophobic modified film. The surface-roughened hydrophobic modified film was immersed in a prepared silicon-based hydrophilic modification reagent for dip coating and then dried. The negative pressure curve of the film sample in a fog or air environment was tested after each dip coating until the negative pressure curve of the film stabilized. The pre-dip coating was then stopped. The surface-roughened and uniformly coated film was then placed in a DBD plasma processor for surface roughening and hydrophilic modification to obtain a hydrophilic-hydrophobic sandwich modified film. The silicon-based hydrophobic modifying agent comprises tridecafluorooctyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, and... It is prepared by hydrolysis and condensation of tetraethyl orthosilicate in ethanol solution using ammonia water as a catalyst.

2. The method for preparing a high-efficiency evaporation membrane according to claim 1, characterized in that, The specific preparation method of the silicon-based hydrophobic modification reagent is as follows: Mix tridecafluorooctyltrimethoxysilane and 3-glycidoxypropyltrimethoxysilane and add After adding acetic acid and mixing, a silicon-based hydrophobic modified reagent is obtained.

3. The method for preparing a high-efficiency evaporation membrane according to claim 1, characterized in that, The specific preparation method of the silicon-based hydrophilic modification reagent is as follows: To prepare a TEOS ethanol solution, add the TEOS ethanol solution to an ammonia / ethanol solution. The concentration of the TEOS ethanol solution is 0.2 mol / L, and the volume ratio of ammonia to ethanol in the ammonia / ethanol solution is 1:

4.

4. The method for preparing a high-efficiency evaporation membrane according to claim 2, characterized in that, The molar ratio of the tridecafluorooctyltrimethoxysilane and 3-glycidoxypropyltrimethoxysilane is 3:1, and the acetic acid concentration is 0.025 mol / L.

5. A high-efficiency evaporation membrane prepared by any one of the preparation methods according to claims 1-4, characterized in that, The evaporation membrane comprises a hydrophilic-hydrophobic sandwich modified membrane, on which a silicon-based hydrophobic modifying agent and a silicon-based hydrophilic modifying agent are sequentially coated, and then processed by a plasma processor.

6. The high-efficiency evaporation membrane according to claim 5, characterized in that, The silicon-based hydrophilic modifying agent is prepared by hydrolysis-condensation of tetraethyl orthosilicate in ethanol solution catalyzed by ammonia water. The silicon-based hydrophobic modifying agent is composed of tridecafluorooctyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, and... It is prepared.

Citation Information

Patent Citations

  • Polymer microporous membrane and preparation method thereof, and water treatment equipment

    CN111450707A

  • Hydrophobic membrane for membrane distillation with protein pollution resisting function as well as preparation method and application of hydrophobic membrane

    CN115518529A

  • Preparation method and preparation device of efficient evaporation film

    CN115770489A