A forging method for improving carbide banding in GH4141 alloy

By improving the carbide strip distribution of GH4141 alloy through a multi-step forging process, the problem of uneven carbide distribution was solved, resulting in a more uniform microstructure and improved performance.

CN116809829BActive Publication Date: 2026-11-24西部超导材料科技股份有限公司
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310538500.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-15
Publication Date
2026-11-24
Estimated Expiration
2043-05-15

AI Technical Summary

Technical Problem

The uneven distribution of carbide strips during the forging process of GH4141 alloy leads to uneven microstructure and reduced performance.

Method used

A multi-step forging process is adopted, including axial upsetting, axial roughing and radial elongation in different temperature ranges, combined with specific deformation and cooling treatment to control the distribution of carbides.

Benefits of technology

It effectively improves the dispersion distribution of carbides, enhances the uniformity of the alloy's structure and properties, and increases forging efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116809829B_ABST
    Figure CN116809829B_ABST
Patent Text Reader

Abstract

This invention relates to the field of high-temperature alloy hot working technology, and discloses a forging method for improving the carbide strip distribution of GH4141 alloy, comprising the following three steps: Step 1: Forging a GH4141 alloy ingot within a first preset temperature range, involving at least two axial upsetting processes with a deformation of 10% to 30%, to obtain an octagonal cross-section intermediate billet; Step 2: Axially upsetting the intermediate billet within a second preset temperature range, with a height-to-diameter ratio of 0.4 to 0.8, rounding it, and then radially elongating the round cross-section billet to obtain a first intermediate billet; Step 3: Radially elongating the first intermediate billet within a third preset temperature range, with a deformation of 20% to 40%, followed by one rounding and beveling, and air cooling to obtain the finished GH4141 alloy bar. The GH4141 alloy bar obtained by the forging method of this application exhibits a dispersed carbide distribution and significantly improved strip distribution.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of high-temperature alloy hot working technology, and in particular to a forging method for improving the carbide strip distribution of GH4141 alloy. Background Technology

[0002] GH4141 is a highly alloyed Ni-Cr-Co based precipitation-strengthened wrought superalloy. It exhibits high tensile, creep, and endurance strengths, yield strength, fatigue resistance, and good oxidation resistance within the temperature range of 650℃ to 900℃. It is widely used in the aerospace field, primarily for manufacturing components for aero-engines operating at temperatures below 870℃. To enhance grain boundary strengthening, a large amount of carbon is added to the alloy, forming numerous carbides with elements such as titanium and chromium to improve alloy properties. However, during the GH4141 alloy ingot forming process, due to metal flow, the carbides often run parallel to the processing flow lines, densely distributing in a banded pattern along the axial direction, resulting in uneven microstructure and reduced performance. Therefore, it is necessary to control the carbide distribution during the GH4141 alloy forging process, reducing the banded distribution and promoting a more dispersed distribution. Summary of the Invention

[0003] To address at least one of the problems existing in the above-mentioned background art, the present invention provides a forging method for improving the carbide strip distribution of GH4141 alloy.

[0004] This invention provides a forging method for improving the carbide strip distribution in GH4141 alloy, comprising the following three steps:

[0005] Step 1: Forging the GH4141 alloy ingot within the first preset temperature range, axial upsetting at least twice, with a deformation of 10% to 30%, to obtain an intermediate billet with an octagonal cross section.

[0006] Step 2: The intermediate billet is axially upset within the second preset temperature range, with a height-to-diameter ratio of 0.4 to 0.8, and then rounded. The round cross-section billet is then radially elongated to obtain the first intermediate billet.

[0007] Step 3: Within the third preset temperature range, the first intermediate billet is radially drawn 2 to 3 times, with a deformation of 20% to 40%, and then beveled and rounded once. After air cooling, the GH4141 alloy finished bar is obtained.

[0008] Furthermore, in the forging method described above for improving the carbide strip distribution of GH4141 alloy, the GH4141 alloy in step one contains 0.08% to 0.12% carbon, 10.0% to 12.0% cobalt, ≤5.0% iron, 18.0% to 20.0% chromium, 9.0% to 10.5% molybdenum, 1.4% to 1.6% aluminum, 3.0% to 3.3% titanium, ≤0.07% zirconium, 0.003% to 0.01% boron, ≤0.5% manganese, ≤0.5% silicon, ≤0.015% sulfur, ≤0.015% phosphorus, ≤0.5% copper, and the remainder is nickel.

[0009] Furthermore, in the forging method described above for improving the carbide strip distribution of GH4141 alloy, the GH4141 alloy ingot in step one is produced using a two-stage melting process or a three-stage melting process.

[0010] Furthermore, in the forging method described above for improving the carbide strip distribution of GH4141 alloy, the two-stage melting process is vacuum induction melting plus vacuum arc remelting; the three-stage melting process is vacuum induction melting plus electroslag remelting plus vacuum arc remelting.

[0011] Furthermore, in the forging method described above for improving the distribution of carbide stripes in GH4141 alloy, asbestos is coated on the surface of the ingot during each forging process in step one.

[0012] Furthermore, in the forging method described above for improving the distribution of carbide strips in GH4141 alloy, the Φ of the finished GH4141 alloy bar is 150mm to 300mm.

[0013] Furthermore, in the forging method described above for improving the carbide strip distribution of GH4141 alloy, the first preset temperature range is 1140°C to 1170°C.

[0014] Furthermore, in the forging method described above for improving the carbide strip distribution of GH4141 alloy, the second preset temperature range is 1120°C to 1140°C.

[0015] Furthermore, in the forging method described above for improving the carbide strip distribution of GH4141 alloy, the third preset temperature range is 1080℃ to 1120℃.

[0016] Furthermore, in the forging method described above for improving the carbide strip distribution of GH4141 alloy, the multiple forging passes are two to three times.

[0017] The beneficial effects of this invention are as follows: The forging method for improving the carbide strip distribution of GH4141 alloy provided by the embodiments of this invention includes the following three steps: Step 1: Forging a GH4141 alloy ingot in a first preset temperature range, performing at least two axial upsetting and drawing processes with a deformation of 10% to 30%, to obtain an octagonal cross-section intermediate billet; Step 2: Axially upsetting the intermediate billet in a second preset temperature range with a height-to-diameter ratio of 0.4 to 0.8, rounding it, and then radially elongating the round cross-section billet to obtain a first intermediate billet; Step 3: Radially elongating the first intermediate billet in a third preset temperature range with multiple processes, a deformation of 20% to 40%, chamfering and rounding in one process, and air cooling to obtain the finished GH4141 alloy bar. To achieve a more dispersed carbide distribution, the traditional method involves adding upsetting and drawing cycles to the conventional forging process. In contrast, this application does not require additional upsetting and drawing cycles, thus improving forging efficiency. Furthermore, the GH4141 alloy bars forged using this application exhibit a more dispersed carbide distribution and significantly improved banding. Attached Figure Description

[0018] To more clearly illustrate the technical solutions in the embodiments of the present invention or the conventional technology, the drawings used in the description of the embodiments or the conventional technology will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0019] Figure 1 A schematic diagram of a forging method for improving the carbide strip distribution of GH4141 alloy, provided for an embodiment of the present invention;

[0020] Figure 2 The carbide distribution in traditional forging methods;

[0021] Figure 3 This invention provides a forging method for improving the carbide strip distribution in GH4141 alloy, as described in an embodiment of the invention.

[0022] Figure 4 A cloud map characterizing the degree of carbide dispersion in traditional forging methods;

[0023] Figure 5 This is a cloud map characterizing the degree of carbide dispersion in a forging method for improving the carbide strip distribution of GH4141 alloy, provided in an embodiment of the present invention. Detailed Implementation

[0024] To make the above-mentioned objects, features, and advantages of the present invention more apparent and understandable, specific embodiments of the present invention will be described in detail below with reference to the accompanying drawings. Many specific details are set forth in the following description to provide a thorough understanding of the present invention. However, the present invention can be practiced in many other ways different from those described herein, and those skilled in the art can make similar modifications without departing from the spirit of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.

[0025] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein in the description of the invention is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.

[0026] Figure 1 This is a schematic diagram of a forging method for improving the carbide strip distribution of GH4141 alloy, provided as an embodiment of the present invention.

[0027] This invention provides a forging method for improving the carbide strip distribution in GH4141 alloy, combined with... Figure 1 It includes three steps, S101 to S103:

[0028] S101: The GH4141 alloy ingot is forged in the first preset temperature range, and then axially upsetting is performed in at least two heats with a deformation of 10% to 30% to obtain an intermediate billet with an octagonal cross section.

[0029] Specifically, in this embodiment of the application, before casting the GH4141 alloy ingot, the GH4141 alloy is batched. The batching must meet the following requirements: carbon content of 0.08% to 0.12%, cobalt content of 10.0% to 12.0%, iron content of ≤5.0%, chromium content of 18.0% to 20.0%, molybdenum content of 9.0% to 10.5%, aluminum content of 1.4% to 1.6%, titanium content of 3.0% to 3.3%, zirconium content of ≤0.07%, boron content of 0.003% to 0.01%, manganese content of ≤0.5%, silicon content of ≤0.5%, sulfur content of ≤0.015%, phosphorus content of ≤0.015%, copper content of ≤0.5%, and the remainder being nickel.

[0030] Specifically, in this embodiment of the application, the first preset temperature range is 1140°C to 1170°C.

[0031] It should be understood that the GH4141 alloy ingot can be forged at any temperature between 1140°C and 1170°C, but this does not limit the scope of protection of this application.

[0032] S102: The intermediate billet is axially upset within the second preset temperature range, with a height-to-diameter ratio of 0.4 to 0.8, and then rounded. The round cross-section billet is then radially elongated to obtain the first intermediate billet.

[0033] Specifically, in this embodiment of the application, the second preset temperature range is 1120°C to 1140°C.

[0034] It should be understood that intermediate billets can be axially upset at any temperature between 1120°C and 1140°C, but this does not limit the scope of protection of this application.

[0035] S103: The first intermediate billet is radially drawn in multiple passes within the third preset temperature range, with a deformation of 20% to 40%. After one pass, the billet is beveled and rounded, and then air-cooled to obtain GH4141 alloy finished bar.

[0036] Specifically, in this embodiment, the third preset temperature range is 1080°C to 1120°C. Multiple firing cycles are two to three times.

[0037] It should be understood that the first intermediate billet can be radially drawn multiple times at any temperature between 1080°C and 1120°C, but this does not limit the scope of protection of this application.

[0038] Figure 2 The distribution of carbides is as shown in traditional forging methods.

[0039] Figure 3 This invention provides a forging method for improving the carbide strip distribution of GH4141 alloy, as described in an embodiment of the invention.

[0040] Combination Figure 2 and Figure 3 The GH4141 alloy bars obtained by the forging method described in S101 to S103 of this application for improving the carbide strip distribution have a more dispersed carbide distribution and a significantly improved strip distribution.

[0041] Figure 4 A cloud map characterizing the degree of carbide dispersion in traditional forging methods.

[0042] Figure 5 This is a cloud map characterizing the degree of carbide dispersion in a forging method for improving the carbide strip distribution of GH4141 alloy, provided in an embodiment of the present invention.

[0043] Combination Figure 4 and Figure 5Similarly, it can be seen that the GH4141 alloy bar obtained by the forging method for improving the carbide strip distribution of GH4141 alloy described in S101 to S103 of this application has a dispersed carbide distribution and a significantly improved strip distribution.

[0044] Furthermore, in the forging method described above for improving the carbide strip distribution of GH4141 alloy, the GH4141 alloy ingot in step one is produced using a two-stage melting process or a three-stage melting process.

[0045] Specifically, in the embodiments of this application, the two-stage melting process is vacuum induction melting plus vacuum consumable melting; the three-stage melting process is vacuum induction melting plus electroslag remelting plus vacuum consumable melting.

[0046] Furthermore, in the forging method described above for improving the distribution of carbide stripes in GH4141 alloy, asbestos is coated on the surface of the ingot during each forging process in step one.

[0047] Furthermore, in the forging method described above for improving the distribution of carbide strips in GH4141 alloy, the finished GH4141 alloy bar has a diameter of 150mm to 300mm.

[0048] Specifically, the diameter of the GH4141 alloy finished bar obtained in this application embodiment is 150mmΦ300mm, which is convenient for application.

[0049] The following describes a forging method for improving the carbide strip distribution of GH4141 alloy, using three embodiments:

[0050] Example 1:

[0051] A forging method for improving the carbide stripe distribution in GH4141 alloy includes the following three steps:

[0052] Step 1: The GH4141 alloy ingot is forged at 1160℃, and then axially upsetting is performed in two heats with a deformation of 20% to obtain an intermediate billet with an octagonal cross section.

[0053] Step 2: Upset the billet axially at 1140℃ with a height-to-diameter ratio of 0.6, roll it into a round shape, and then draw the round cross-section billet radially.

[0054] Step 3: The billet is radially drawn three times at 1100℃ with a deformation of 40%, and then beveled and rounded once. Finally, it is air-cooled in the factory to obtain GH4141 alloy finished bar.

[0055] Example 2

[0056] A forging method for improving the carbide strip distribution of GH4141 alloy includes the following steps:

[0057] Step 1: The GH4141 alloy ingot is forged at 1150℃, and then axially upsetting and drawing is performed in two heats with a deformation of 20% to obtain an intermediate billet with an octagonal cross section.

[0058] Step 2: Upset the billet axially at 1130℃ with a height-to-diameter ratio of 0.5, roll it into a round shape, and then elongate the round cross-section billet radially.

[0059] Step 3: The billet is radially drawn three times at 1100℃ with a deformation of 40%, then beveled and rounded once, and finally air-cooled in the factory to obtain GH4141 alloy finished bar.

[0060] Example 3

[0061] A forging method for improving the carbide strip distribution of GH4141 alloy includes the following steps:

[0062] Step 1: The GH4141 alloy ingot is forged at 1150℃, and then axially upsetting and drawing is performed in two heats with a deformation of 20% to obtain an intermediate billet with an octagonal cross section.

[0063] Step 2: Upset the billet axially at 1120℃ with a height-to-diameter ratio of 0.4, roll it into a round shape, and then draw the round cross-section billet radially.

[0064] Step 3: The billet is radially drawn three times at 1100℃ with a deformation of 30%, then beveled and rounded once, and finally air-cooled in the factory to obtain GH4141 alloy finished bar.

[0065] Tests showed that, compared with existing technologies, the GH4141 alloy rods obtained through the above three examples (Examples 1 to 3) exhibited significantly improved carbide distribution and banding.

[0066] Those skilled in the art will understand that although some embodiments described herein include certain features included in other embodiments but not others, combinations of features from different embodiments are meant to be within the scope of the invention and form different embodiments.

[0067] Those skilled in the art will understand that the descriptions of the various embodiments have different focuses, and for parts not described in detail in a certain embodiment, reference can be made to the relevant descriptions of other embodiments.

[0068] The above are merely specific embodiments of the present invention, but the scope of protection of the present invention is not limited thereto. Any person skilled in the art can easily conceive of various equivalent modifications or substitutions within the technical scope disclosed in the present invention, and these modifications or substitutions should all be covered within the scope of protection of the present invention. Therefore, the scope of protection of the present invention should be determined by the scope of the claims.

Claims

1. A forging method for improving the carbide strip distribution of GH4141 alloy, characterized in that, It includes the following three steps: Step 1: Forging the GH4141 alloy ingot within the first preset temperature range of 1140℃ to 1170℃, axial upsetting and drawing at least two times, with a deformation of 10% to 30%, to obtain an intermediate billet with an octagonal cross section. Step 2: The intermediate billet is axially upset within the second preset temperature range of 1120℃ to 1140℃, with a height-to-diameter ratio of 0.4 to 0.8, and then rounded. The round cross-section billet is then radially elongated to obtain the first intermediate billet. Step 3: The first intermediate billet is radially drawn in multiple passes within the third preset temperature range of 1080℃ to 1120℃, with a deformation of 20% to 40%. After one pass, the billet is beveled and rounded, and then air-cooled to obtain GH4141 alloy finished bars with a diameter of 150mm to 300mm. In step one, the GH4141 alloy contains 0.08% to 0.12% carbon, 10.0% to 12.0% cobalt, ≤5.0% iron, 18.0% to 20.0% chromium, 9.0% to 10.5% molybdenum, 1.4% to 1.6% aluminum, 3.0% to 3.3% titanium, ≤0.07% zirconium, 0.003% to 0.01% boron, ≤0.5% manganese, ≤0.5% silicon, ≤0.015% sulfur, ≤0.015% phosphorus, ≤0.5% copper, and the remainder is nickel.

2. The forging method for improving the carbide strip distribution of GH4141 alloy according to claim 1, characterized in that, The GH4141 alloy ingot in step one is produced using a two-stage or three-stage smelting process.

3. The forging method for improving the carbide strip distribution of GH4141 alloy according to claim 2, characterized in that, The two-stage melting process is vacuum induction melting plus vacuum consumable melting; the three-stage melting process is vacuum induction melting plus electroslag remelting plus vacuum consumable melting.

4. The forging method for improving the carbide strip distribution of GH4141 alloy according to claim 1, characterized in that, In step one, asbestos is coated onto the surface of the ingot during each forging process.

5. The forging method for improving the carbide strip distribution of GH4141 alloy according to claim 1, characterized in that, The multiple firings refer to two to three firings.

Citation Information

Patent Citations

  • GH 3039 high temperature alloy bar and preparation method thereof

    CN111020298A

  • Preparation method of difficult-to-deform high-temperature alloy GH4141 alloy ingot

    CN115233013A